Heavy-duty anti-corrosion powder coating based on waste polyester fibers and preparation method thereof
By modifying and compounding waste polyester fibers, a heavy-duty anti-corrosion powder coating with excellent anti-corrosion performance and long-term durability was prepared, which solved the problem of durability and stability of powder coatings in harsh environments, and realized resource recycling and performance improvement.
Patent Information
- Application Number
- CN202411103653.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-13
AI Technical Summary
Existing powder coatings lack durability and stability under harsh chemical and environmental conditions, and their raw materials are derived from petrochemical products, resulting in high costs and significant environmental impact. The high-value application of waste polyester fibers in coatings has not been fully developed.
Waste polyester fibers were ultrasonically cleaned, crushed, alcoholized, and modified to introduce isocyanate compounds and trimethoxysilane functional groups, thus preparing modified polyester fiber powder. This powder was then compounded with E51 epoxy resin, E20 epoxy resin, and composite fillers to prepare heavy-duty anti-corrosion powder coatings.
This technology enables the high-value transformation of waste polyester fibers, producing heavy-duty anti-corrosion powder coatings with excellent anti-corrosion properties, mechanical properties, long-term durability, and stability, meeting the application needs of harsh environments such as chemical and marine industries.
Smart Images

Figure BDA0004990084880000061 
Figure BDA0004990084880000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of anti-corrosion coatings, and in particular to a heavy-duty anti-corrosion powder coating based on waste polyester fibers and a preparation method thereof. Background Art
[0002] As an important protective material in the industrial field, anti-corrosion coatings are widely used in many industries such as chemical, marine, and infrastructure to protect metal structures from corrosion. Traditional anti-corrosion coatings mostly use solvent-based coatings, but with the increase in environmental awareness and strict regulations, solvent-based coatings are gradually restricted due to volatile organic compound (VOC) emissions. Therefore, the development of environmentally friendly and high-performance anti-corrosion coatings has become a research hotspot.
[0003] As an environmentally friendly coating, powder coating is favored for its advantages such as solvent-free, low VOC emission and high utilization rate. However, the existing powder coating still has limitations in anti-corrosion performance, especially under harsh chemical and environmental conditions, such as chemical facilities and offshore platforms, its durability and stability need to be improved. In addition, the raw materials of powder coating are usually derived from petrochemical products, which are costly and have an impact on the environment that cannot be ignored.
[0004] As a renewable resource, the recycling of waste polyester fibers has made certain progress in the fields of textiles, packaging, etc. However, in the field of coatings, especially in the preparation of heavy-duty anti-corrosion powder coatings, the high-value application of waste polyester fibers has not been fully developed. In the prior art, the recycling of waste polyester fibers mostly adopts physical methods, such as mechanical crushing, melt regeneration, etc. These methods are difficult to achieve high-performance application of waste polyester fibers in coatings. Therefore, exploring the application of waste polyester fibers in heavy-duty anti-corrosion powder coatings can not only realize the recycling of resources, but also improve the environmental protection performance and application scope of coatings, which has important practical significance and market prospects. Summary of the invention
[0005] In view of the above shortcomings of the prior art, the present invention provides a method for preparing a heavy-duty anti-corrosion powder coating based on waste polyester fibers, so as to solve the technical problems in the prior art that waste polyester fibers are difficult to effectively recycle, the heavy-duty anti-corrosion powder coating has insufficient performance, and it is difficult to meet the long-term durability and stability requirements in harsh environments such as chemical industry, ocean, and infrastructure. Through the preparation method of the present invention, not only the high-value conversion of waste polyester fibers is achieved, but also the prepared heavy-duty anti-corrosion powder coating has both excellent anti-corrosion performance and environmental adaptability, while ensuring the long-term durability and stability of the coating, meeting the application requirements under harsh chemical and environmental conditions.
[0006] In order to achieve the above purpose, the technical solution adopted by the present invention is:
[0007] A method for preparing a heavy-duty anti-corrosion powder coating based on waste polyester fibers, the method comprising the following steps:
[0008] S1: sorting the waste polyester fibers with a PET content greater than 70% by color, performing ultrasonic cleaning, drying, crushing, and then adding them to a pretreatment solution for partial alcoholysis reaction to obtain short-cut polyester fiber alcoholysis products;
[0009] S2: Grind the alcoholysis product of the short-cut polyester fiber obtained in step S1 into powder, and then add it to a modifier containing an isocyanate compound to carry out a multifunctional grafting modification reaction of disulfide bonds and trimethoxysilane functional groups to obtain modified polyester fiber powder; In step S2 of the present application, by powdering the alcoholysis product of the short-cut polyester fiber, the specific surface area of the material is significantly increased, thereby enhancing its dispersibility in the coating formulation and providing a more active surface for subsequent chemical modification. The powdered polyester fiber reacts with a modifier containing an isocyanate compound to achieve the introduction of disulfide bonds and trimethoxysilane functional groups. These modifications not only enhance the compatibility of the fiber with the resin matrix, but also significantly improve the mechanical properties and chemical stability of the coating. The introduction of disulfide bonds provides the coating with self-healing ability, while the trimethoxysilane functional group further improves the chemical resistance and temperature resistance of the coating through a cross-linking reaction with the epoxy resin. In addition, the modified coating exhibits better thermal stability, wear resistance and scratch resistance, while the enhanced adhesion ensures the application stability of the coating on different substrates. Overall, the technical effect of step S2 brings excellent comprehensive performance to the prepared heavy-duty anti-corrosion powder coating, meeting the long-term durable anti-corrosion requirements under harsh chemical and environmental conditions.
[0010] S3: The modified polyester fiber powder obtained in step S2 is mixed with E51 epoxy resin, E20 epoxy resin, composite filler, curing agent and auxiliary agent, and the heavy-duty anti-corrosion powder coating is obtained through melt extrusion, tableting, air cooling, grinding and screening.
[0011] As a preferred technical solution, the pretreatment solution is a mixed solution of zinc acetate and an alcohol compound.
[0012] As a preferred technical solution, in step S1, the reaction conditions of the alcoholysis reaction are: the reaction time is 0.5 to 1 h, and the reaction temperature is controlled at 60 to 80°C.
[0013] As a preferred technical solution, in step S2, the alcoholysis product of the short-cut polyester fiber is ground into powder to obtain a fineness of 30 to 70 meshes.
[0014] As a preferred technical solution, the modifier is a mixture of a reaction product of dithiodiol and diisocyanate and 3-isocyanatepropyltrimethoxysilane.
[0015] As a preferred technical solution, the dithiodiol is at least one of ethylene-2,2'-di(dithio)di(ethanol), 2,2'-(1,3-propanediyldisulfanediyl)diethanol, 2,2'-dithiodi-ethanol, and 4,4'-dithiodibutane-1-ol.
[0016] As a preferred technical solution, the diisocyanate is at least one of hexamethylene diisocyanate, isophorone diisocyanate, 2,4-toluene diisocyanate, and 2,6-toluene diisocyanate.
[0017] As a preferred technical solution, the composite filler is a mixture of mica powder, quartz powder and talcum powder, wherein the amount of mica powder is 20-30% of the total filler mass, the amount of quartz powder is 40-50% of the total filler mass, and the amount of talcum powder is 20-30% of the total filler mass.
[0018] As a preferred technical solution, the curing agent is at least one of ethylenediamine, diethylenetriamine and triethylenetetramine.
[0019] As a preferred technical solution, the auxiliary agent is at least one of a leveling agent, a dispersant, an anti-settling agent, and an anti-ultraviolet agent.
[0020] Another aspect of the present invention is to provide a heavy-duty anti-corrosion powder coating based on waste polyester fibers, wherein the heavy-duty anti-corrosion powder coating is prepared by the above-mentioned method for preparing the heavy-duty anti-corrosion powder coating based on waste polyester fibers.
[0021] Beneficial effects of the present invention:
[0022] The heavy-duty anti-corrosion powder coating preparation method of the present invention effectively converts waste polyester fibers into high-value anti-corrosion coatings, achieving the dual goals of resource recycling and environmental protection. Through this innovative process, the coating not only exhibits excellent anti-corrosion performance, but also has other significant advantages.
[0023] The present invention is a method for preparing a heavy-duty anti-corrosion powder coating based on waste polyester fibers, which turns waste into treasure. By recycling waste polyester fibers, no additional pigments need to be added, and the powder coating has excellent anti-corrosion properties. Specifically, by innovatively introducing a modifier containing an isocyanate compound and performing multifunctional grafting modification of disulfide bonds and trimethoxysilane functional groups, the powder coating has excellent mechanical properties and resistance to chemical media corrosion. Further compounding with E51 epoxy resin, E20 epoxy resin, composite fillers, etc., not only enhances the cohesion and adhesion of the coating, but also significantly improves the temperature resistance, weather resistance and long-term stability of the coating.
[0024] In general, the heavy-duty anti-corrosion powder coating based on waste polyester fibers prepared by the present invention has strong overall comprehensive performance. It not only has excellent anti-corrosion performance and environmental adaptability, but also ensures the long-term durability and stability of the coating, and can meet the long-term durability and stability requirements in harsh environments such as chemical, marine, and infrastructure. DETAILED DESCRIPTION
[0025] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.
[0026] Example 1
[0027] The method for preparing a heavy-duty anticorrosive powder coating based on waste polyester fibers in this embodiment comprises the following steps:
[0028] S1: After sorting the waste polyester fibers with a PET content greater than 70% by color, ultrasonic cleaning is performed, and crushing is performed after drying, and then added to a pretreatment solution for partial alcoholysis reaction to obtain short-cut polyester fiber alcoholysis products. The waste polyester fibers account for 15% of the total mass of the pretreatment solution, and the pretreatment solution is a mixed solution of zinc acetate and ethylene glycol in a mass ratio of 1:20. The reaction conditions of the alcoholysis reaction are: the reaction time is 0.5h, and the reaction temperature is controlled at 60°C.
[0029] S2: Grind 30g of the alcoholysis product of the short-cut polyester fiber obtained in step S1 into powder, obtain a fineness of 40 mesh, disperse it in 100mL of toluene solvent, and then add 5g of a modifier containing an isocyanate compound under the protection of an inert atmosphere of nitrogen to carry out a multifunctional grafting modification reaction of disulfide bonds and trimethoxysilane functional groups, and react in a constant temperature water bath at 50°C for 2h to obtain a modified polyester fiber powder. The modifier is a mixture of a reaction product of 2,2'-dithiodi-ethanol and isophorone diisocyanate and 3-isocyanate propyltrimethoxysilane. The reaction product is obtained by reacting an excess of isophorone diisocyanate. Specifically, the molar ratio of the reaction of 2,2'-dithiodi-ethanol and isophorone diisocyanate is 1:2, and the terminal group of the obtained reaction product is an isocyanate group. Further, the molar ratio of the reaction product to 3-isocyanate propyltrimethoxysilane is 3:2.
[0030] S3: By weight, 20 parts of the modified polyester fiber powder obtained in step S2 are compounded and mixed with 25 parts of E51 epoxy resin, 15 parts of E20 epoxy resin, 10 parts of composite filler, 4 parts of ethylenediamine and 1 part of auxiliary agent, and the heavy anti-corrosion powder coating is obtained after melt extrusion, tableting, air cooling, grinding and screening. The composite filler is a mixture of mica powder, quartz powder and talcum powder, wherein the amount of mica powder is 20% of the total filler mass, the amount of quartz powder is 50% of the total filler mass, and the amount of talcum powder is 30% of the total filler mass. The curing agent is ethylenediamine. The auxiliary agent is composed of leveling agent BYK-333, dispersant Hydropalat 3204, anti-settling agent organic bentonite and anti-ultraviolet agent Tinuvin 328 in a mass ratio of 5:15:3:3.
[0031] Example 2
[0032] The method for preparing a heavy-duty anticorrosive powder coating based on waste polyester fibers in this embodiment comprises the following steps:
[0033] S1: After sorting the waste polyester fibers with a PET content greater than 70% by color, ultrasonic cleaning is performed, and crushing is performed after drying, and then added to a pretreatment solution for partial alcoholysis reaction to obtain short-cut polyester fiber alcoholysis products. The waste polyester fibers account for 15% of the total mass of the pretreatment solution, and the pretreatment solution is a mixed solution of zinc acetate and ethylene glycol in a mass ratio of 1:20. The reaction conditions of the alcoholysis reaction are: the reaction time is 1h, and the reaction temperature is controlled at 70°C.
[0034] S2: Grind 30g of the alcoholysis product of the short-cut polyester fiber obtained in step S1 into powder, obtain a fineness of 50 mesh, disperse it in 100mL of toluene solvent, and then add 5g of a modifier containing an isocyanate compound under the protection of an inert atmosphere of nitrogen to carry out a multifunctional grafting modification reaction of disulfide bonds and trimethoxysilane functional groups, and react in a constant temperature water bath at 50°C for 2h to obtain a modified polyester fiber powder. The modifier is a mixture of a reaction product of ethylene-2,2'-di(disulfide)di(ethanol) and hexamethylene diisocyanate and 3-isocyanatepropyltrimethoxysilane. The reaction product is obtained by reacting an excess of hexamethylene diisocyanate. Specifically, the molar ratio of the reaction of ethylene-2,2'-di(disulfide)di(ethanol) and hexamethylene diisocyanate is 1:1, and the terminal group of the obtained reaction product is an isocyanate group. Furthermore, the molar ratio of the reaction product to 3-isocyanatepropyltrimethoxysilane is 3:2.
[0035] S3: By weight, 25 parts of the modified polyester fiber powder obtained in step S2 are compounded and mixed with 20 parts of E51 epoxy resin, 20 parts of E20 epoxy resin, 12 parts of composite filler, 5 parts of diethylenetriamine and 1.5 parts of auxiliary agent, and the heavy anti-corrosion powder coating is obtained after melt extrusion, tableting, air cooling, grinding and screening. The composite filler is a mixture of mica powder, quartz powder and talcum powder, wherein the amount of mica powder is 30% of the total filler mass, the amount of quartz powder is 45% of the total filler mass, and the amount of talcum powder is 25% of the total filler mass. The curing agent is ethylenediamine. The auxiliary agent is composed of leveling agent BYK-333, dispersant Hydropalat 3204, anti-settling agent organic bentonite and anti-ultraviolet agent Tinuvin 328 in a mass ratio of 6:12:3:2.
[0036] Example 3
[0037] The method for preparing a heavy-duty anticorrosive powder coating based on waste polyester fibers in this embodiment comprises the following steps:
[0038] S1: After sorting the waste polyester fibers with a PET content greater than 70% by color, ultrasonic cleaning is performed, and crushing is performed after drying, and then added to a pretreatment solution for partial alcoholysis reaction to obtain short-cut polyester fiber alcoholysis products. The waste polyester fibers account for 15% of the total mass of the pretreatment solution, and the pretreatment solution is a mixed solution of zinc acetate and ethylene glycol in a mass ratio of 1:20. The reaction conditions of the alcoholysis reaction are: the reaction time is 1h, and the reaction temperature is controlled at 60°C.
[0039] S2: Grind 30g of the alcoholysis product of the short-cut polyester fiber obtained in step S1 into powder, obtain a fineness of 60 mesh, disperse it in 100mL of toluene solvent, and then add 5g of a modifier containing an isocyanate compound under the protection of an inert atmosphere of nitrogen to carry out a multifunctional grafting modification reaction of disulfide bonds and trimethoxysilane functional groups, and react in a constant temperature water bath at 50°C for 2h to obtain a modified polyester fiber powder. The modifier is a mixture of a reaction product of 2,2'-(1,3-propanediyldisulfanediyl)diethanol and 2,4-toluene diisocyanate and 3-isocyanatepropyltrimethoxysilane. The reaction product is obtained by reacting an excess of 2,4-toluene diisocyanate. Specifically, the molar ratio of the reaction of the 2,2'-(1,3-propanediyldisulfanediyl)diethanol and 2,4-toluene diisocyanate is 1:2, and the terminal group of the obtained reaction product is an isocyanate group. Furthermore, the molar ratio of the reaction product to 3-isocyanatepropyltrimethoxysilane is 2:3.
[0040] S3: By weight, 30 parts of the modified polyester fiber powder obtained in step S2 are compounded and mixed with 15 parts of E51 epoxy resin, 25 parts of E20 epoxy resin, 15 parts of composite filler, 6 parts of triethylenetetramine and 2 parts of auxiliary agents, and the heavy anti-corrosion powder coating is obtained after melt extrusion, tableting, air cooling, grinding and screening. The composite filler is a mixture of mica powder, quartz powder and talcum powder, wherein the amount of mica powder is 25% of the total filler mass, the amount of quartz powder is 50% of the total filler mass, and the amount of talcum powder is 25% of the total filler mass. The curing agent is ethylenediamine. The auxiliary agent is composed of leveling agent BYK-333, dispersant Hydropalat 3204, anti-settling agent organic bentonite and anti-ultraviolet agent Tinuvin 328 in a mass ratio of 7:13:4:3.
[0041] Comparative Example 1
[0042] The preparation method of the heavy-duty anti-corrosion powder coating based on waste polyester fiber in this comparative example has the same raw material composition and preparation steps as those in Example 1, except that in the preparation method of this comparative example, the modifier is only the reaction product of 2,2'-dithiodiethanol and isophorone diisocyanate.
[0043] Comparative Example 2
[0044] The present comparative example is a method for preparing a heavy-duty anti-corrosion powder coating based on waste polyester fibers, and its raw material composition and preparation steps are substantially the same as those of Example 1, except that, in the preparation method of the present comparative example, the modifier is only 3-isocyanatepropyltrimethoxysilane.
[0045] The heavy-duty anti-corrosion powder coatings prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were subjected to performance tests, and the performance results are shown in Table 1: Specifically, the powder coating samples were sprayed on the test steel by an electrostatic spraying process.
[0046] Among them, the cathodic stripping resistance is carried out with reference to SY / T 0413-2002. The test is carried out at a high temperature of 65°C for 48 hours. During the test, the metal substrate of the coating will be connected to a cathodic protection system to simulate the cathodic protection environment in actual use. By applying current, the metal substrate becomes the cathode, and the coating is exposed to the electrochemical reaction caused by the cathodic protection. The degree of coating stripping is used to evaluate the adhesion and anti-corrosion performance of the coating under cathodic protection conditions.
[0047] Impact strength: Tested in accordance with the national standard GB / T 1732, the samples were tested under an impact energy of 5 joules.
[0048] Hardness: Tested in accordance with national standard GB / T 6739.
[0049] Salt spray resistance: Tested in a salt spray chamber with reference to national standard GB / T 1771, with the test temperature set at 35°C, 5% salt solution, and the test duration set at 1000 hours, and evaluated based on the degree of corrosion.
[0050] Ageing resistance: Refer to ISO 11507 and use xenon lamp exposure test, set the test light intensity to 0.75W / m 2 The test temperature is 50℃, the test time is 1000h, and the corrosion degree is evaluated.
[0051] Resistance to moisture and heat: Tested in accordance with the national standard GB / T 1740, with the test conditions set at 50°C, 95% relative humidity, for 1000 hours, and evaluated based on the degree of corrosion. Table 1
[0052] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention, and these changes and improvements fall within the scope of the present invention claimed.
Claims
1. A method for preparing a heavy-duty anticorrosive powder coating based on waste polyester fibers, characterized in that: The preparation method comprises the following steps: S1: sorting the waste polyester fibers with a PET content greater than 70% by color, performing ultrasonic cleaning, drying, crushing, and then adding them to a pretreatment solution for partial alcoholysis reaction to obtain short-cut polyester fiber alcoholysis products; S2: grinding the alcoholysis product of the short-cut polyester fiber obtained in step S1 into powder, and then adding it to a modifier containing an isocyanate compound to carry out a multifunctional grafting modification reaction of disulfide bonds and trimethoxysilane functional groups to obtain modified polyester fiber powder; S3: The modified polyester fiber powder obtained in step S2 is mixed with E51 epoxy resin, E20 epoxy resin, composite filler, curing agent and auxiliary agent, and the heavy-duty anti-corrosion powder coating is obtained through melt extrusion, tableting, air cooling, grinding and screening.
2. The method for preparing a heavy-duty anticorrosive powder coating based on waste polyester fibers as claimed in claim 1, characterized in that: The pretreatment solution is a mixed solution of zinc acetate and an alcohol compound.
3. The method for preparing a heavy-duty anticorrosive powder coating based on waste polyester fibers as claimed in claim 1, characterized in that: In step S1, the reaction conditions of the alcoholysis reaction are: the reaction time is 0.5 to 1 h, and the reaction temperature is controlled at 60 to 80°C.
4. The method for preparing a heavy-duty anticorrosive powder coating based on waste polyester fibers as claimed in claim 1, characterized in that: In step S2, the alcoholysis product of the short-cut polyester fiber is ground into powder to obtain a fineness of 30 to 70 meshes.
5. The method for preparing a heavy-duty anticorrosive powder coating based on waste polyester fibers as claimed in claim 1, characterized in that: The modifier is a mixture of a reaction product of dithiodiol and diisocyanate and 3-isocyanate propyltrimethoxysilane.
6. The method for preparing a heavy-duty anticorrosive powder coating based on waste polyester fibers as claimed in claim 5, characterized in that: The dithiodiol is at least one of ethylene-2,2'-di(dithio)di(ethanol), 2,2'-(1,3-propanediyldisulfanediyl)diethanol, 2,2'-dithiodi-ethanol, and 4,4'-dithiodibutane-1-ol.
7. The method for preparing a heavy-duty anticorrosive powder coating based on waste polyester fibers as claimed in claim 5, characterized in that: The diisocyanate is at least one of hexamethylene diisocyanate, isophorone diisocyanate, 2,4-toluene diisocyanate and 2,6-toluene diisocyanate.
8. The method for preparing a heavy-duty anticorrosive powder coating based on waste polyester fibers as claimed in claim 1, characterized in that: The composite filler is a mixture of mica powder, quartz powder and talcum powder, wherein the amount of mica powder is 20-30% of the total filler mass, the amount of quartz powder is 40-50% of the total filler mass, and the amount of talcum powder is 20-30% of the total filler mass.
9. The method for preparing a heavy-duty anticorrosive powder coating based on waste polyester fibers according to claim 1, characterized in that: The curing agent is at least one of ethylenediamine, diethylenetriamine and triethylenetetramine.
10. A heavy-duty anti-corrosion powder coating based on waste polyester fibers, characterized in that: The heavy-duty anti-corrosion powder coating is prepared by the method for preparing a heavy-duty anti-corrosion powder coating based on waste polyester fibers as described in any one of claims 1 to 9.
Citation Information
Patent Citations
Process for producing polyurethane foamed material with waste polyester
CN105482056A
Graphene modified fluorosilicone anti-corrosive and wear-resistant coating and preparation method thereof
CN113045961A
Wear-resistant floor paint and preparation method thereof
CN113956767A
Application of waste polyester fibers in preparation of powder coating and powder coating
CN114196249A
Low-temperature fast-curing damp-heat-resistant epoxy adhesive as well as preparation method and application thereof
CN114989757A