Aramid paper composite material adhesive

By using a composite adhesive formed by crosslinking a composite polyacrylic resin modified by bisphenol A epoxy resin and silicone intermediate in the C-grade insulating paper composite material, the composite adhesive is solved by crosslinking the composite material by high temperature and oil resistance. The problem of insufficient results enables the high-performance bonding and resistance requirements to be met.

CN118879259APending Publication Date: 2024-11-01TAIHE NEW MATERIALS (NINGXIA) TECHNOLOGY R&D CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410831944.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the prior art, composite adhesives are used in C-grade insulating paper composite materials with insufficient high temperature resistance, oil resistance, humidity and heat resistance, and cannot meet high performance requirements.

Method used

A high molecular weight hydroxy polyacrylic resin is used to adopt an aramid paper composite material adhesive, including component A and component B. Component A is modified from bisphenol A epoxy resin and silicone intermediate. Component B is high NCO The liquid isocyanate content is formed by cross-linking curing to form a composite adhesive with excellent bonding strength and high temperature resistance.

Benefits of technology

This adhesive achieves excellent initial adhesion and final adhesion strength in C-grade aramid paper insulated paper composite materials, and has high temperature resistance, oil resistance, corrosion resistance, acid and alkali resistance, etc., to meet the high performance needs of composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to the field of adhesive materials, and particularly relates to an aramid paper composite material adhesive. Comprising a component A and a component B, and the weight ratio of the component A to the component B is (5-7): 1; the component A is prepared by the following steps: dissolving bisphenol A epoxy resin in a solvent, and heating to 80-130 DEG C to obtain a bisphenol A epoxy resin solution; mixing hydroxyl acrylate, an auxiliary agent and the organic silicon intermediate to obtain an organic silicon intermediate mixture; dropwise adding the organic silicon intermediate mixture into the bisphenol A epoxy resin solution, carrying out a reaction, and after the reaction is finished, carrying out heat preservation for a preset period of time, and cooling to obtain a component A; the weight ratio of the bisphenol A epoxy resin to the organosilicon intermediate is (5-10): (3-8); and the component B is modified isocyanate. The obtained composite adhesive is used for composite bonding of a C-grade aramid paper insulation paper composite material, and can meet the requirements of the C-grade aramid paper insulation paper composite material on bonding, high temperature resistance, hydrolysis resistance and alkali resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of adhesive materials, and in particular relates to an aramid paper composite material adhesive. Background Art

[0002] Nomex (aramid) insulation paper has good mechanical strength, electrical properties, thermal stability and chemical compatibility, and is widely used in F-class and C-class motors. With the development of science and technology, fields such as aerospace and high-speed trains have put forward higher requirements on motor capacity, and electrical equipment tends to be miniaturized and large-capacity, which also puts forward higher requirements on the high temperature resistance, strength and insulation properties of insulation materials.

[0003] The insulation materials of traditional motors mainly include pure insulation paper, pure insulation film, and flexible insulation materials composed of multiple layers of insulation paper and insulation film. The heat resistance grades of these insulation materials are divided into Class A (the maximum allowable temperature is at least 105°C, such as traditional kraft paper), Class E (the maximum allowable temperature is at least 120°C, such as the heat-modified cellulose insulation paper TUKPaper developed by Westinghouse Electric Company in the late 1950s), Class B (the maximum allowable temperature is at least 130°C, such as the new high-temperature resistant insulation paper T910 developed by DuPont through a mixed copying process), Class F (the maximum allowable temperature is at least 155°C), Class H (the maximum allowable temperature is at least 180°C, such as flexible insulation paper composite materials NHN, NMN, etc.), Class C (the maximum allowable temperature is at least 220°C, such as DuPont's 410 insulation paper), and Class C insulation paper composite materials have higher resistance to high temperature, oil, and moisture and heat aging.

[0004] The Chinese invention patent with patent number CN206558295U discloses a laminated busbar adhesive film structure with stable insulation performance resistant to high temperature and high humidity, including a double-sided stretched polyester layer, a polyester adhesive layer, a polyester hot melt adhesive layer and a matte film, which puts forward higher performance requirements for high temperature resistance, oil resistance, and resistance to heat and humidity aging for the composite adhesive used for Class C insulation paper composite materials. The Chinese invention patent with patent number CN114085639A discloses an adhesive for Class C insulation paper composite materials and a preparation method thereof, wherein the curing agent introduces polysilazane resin modified isocyanate, but when the adhesive is used for the above-mentioned laminated busbar adhesive film with stable insulation performance resistant to high temperature and high humidity, its high temperature resistance, oil resistance and resistance to heat and humidity aging are still insufficient and cannot meet the requirements. Summary of the invention

[0005] In view of this, the present invention provides an aramid paper composite material adhesive to solve the technical problem that the composite adhesive in the prior art is insufficient in high temperature resistance, oil resistance, and moisture and heat resistance when used for Class C insulating paper composite materials.

[0006] To achieve the above objectives, this application adopts the following scheme:

[0007] An aramid paper composite adhesive comprises a component A and a component B, wherein the weight ratio of the component A to the component B is (5 to 7):1;

[0008] Wherein, the component A is prepared by the following steps:

[0009] S10. dissolving bisphenol A epoxy resin in a solvent and heating the mixture to 80° C. to 130° C. to obtain a bisphenol A epoxy resin solution;

[0010] S20. Mix the hydroxy acrylate, the additive and the silicone intermediate to obtain a silicone intermediate mixture;

[0011] S30. Add the organic silicon intermediate mixture dropwise to the bisphenol A epoxy resin solution to react. After the reaction is completed, keep the mixture warm for a predetermined time and cool it down to obtain a composite modified hydroxy acrylic resin, i.e., component A; wherein the weight ratio of the bisphenol A epoxy resin to the organic silicon intermediate is (5 to 10):(3 to 8);

[0012] The B component is prepared by the following steps:

[0013] K10. Carbodiimide-modified MDI and polymeric MDI are mixed to obtain an MDI mixture;

[0014] K20. The MDI mixture is heated to a first temperature and stirred for reaction. After the reaction is completed, the temperature is lowered and the material is discharged to obtain a modified isocyanate, namely, the B component.

[0015] Preferably, the auxiliary agent is: methacrylate monomer, methacrylic acid, styrene and initiator, and the weight ratio of the methacrylate monomer, methacrylic acid, styrene and initiator is: (10 to 35): (3 to 8): (10 to 35): (0.5 to 3).

[0016] Preferably, the rotational viscosity of component A at 25°C is 500mPa.s to 2000mPa.s, and the solid content is 50% to 70%; the relative molecular mass of component A is 10000 to 50000, the acid value is less than 5mgKOH / g, the hydroxyl value is 5mgKOH / g to 25mgKOH / g, and the glass transition temperature is -10°C to 5°C.

[0017] Preferably, the organosilicon intermediate is one or more organosilicon intermediates containing epoxy or unsaturated double bonds.

[0018] Preferably, the solvent is at least one of xylene, ethyl acetate, butyl acetate, propylene glycol butyl ether, propylene glycol methyl ether, ethylene glycol methyl ether and ethylene glycol butyl ether.

[0019] Preferably, the methacrylate monomer is at least one of methyl methacrylate, butyl methacrylate, ethyl methacrylate and isobornyl methacrylate.

[0020] Preferably, the hydroxyacrylate is at least one of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate and hydroxypropyl methacrylate.

[0021] Preferably, the initiator is at least one of azobisisobutyronitrile, azobisisovaleronitrile, tert-butyl hydroperoxide, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide.

[0022] Preferably, in step K10, the weight ratio of the carbodiimide-modified MDI to the polymeric MDI is (1:9) to (9:1).

[0023] Preferably, the B component has a rotational viscosity of 50 to 500 mPa.s at 25° C., a solid content of 90% to 100%, and an NCO content of 25% to 35%.

[0024] The technical solution adopted in this application can achieve the following beneficial effects:

[0025] The present application provides an aramid paper composite adhesive, comprising component A and component B, wherein the main components of component A are bisphenol A epoxy resin and high molecular weight hydroxy polyacrylic resin modified by organosilicon intermediates, the rotational viscosity of component A at 25°C is 500mpa.s to 2000mpa.s, and the solid content is 50% to 70%; after reacting with component B, it has excellent initial adhesion and final bonding strength between Nomex paper / PET film and Nomex paper / PA film. By adding bisphenol A epoxy resin and organosilicon intermediates, component A can enhance the adhesion to PET sheets and PA films, and at the same time improve the heat resistance of the adhesive layer at high temperatures. Component B uses liquid isocyanate with high NCO content. Component B has a rotational viscosity of 50mpa.s to 500mpa.s at 25°C, a solid content of 90% to 100%, and an NCO content of 25% to 35%. After cross-linking and curing with component A, it has excellent bonding strength to Nomex paper material, and also has excellent high temperature resistance, oil resistance, corrosion resistance, acid and alkali resistance, etc. The composite adhesive composed of component A and component B is used for composite bonding of C-grade aramid paper insulation paper composite materials, and can meet the requirements for bonding, high temperature resistance, hydrolysis resistance, alkali resistance, and chemical resistance. DETAILED DESCRIPTION

[0026] In order to facilitate the understanding of the present application, the present application will be described more comprehensively below in conjunction with the embodiments. And the preferred implementation of the present application is given. However, the present application can be implemented in many different forms and is not limited to the implementation described herein. On the contrary, the purpose of providing these implementations is to make the disclosure of the present application more thoroughly and comprehensively understood.

[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0028] An aramid paper composite adhesive, in this embodiment, comprises a component A and a component B, wherein the weight ratio of the component A to the component B is (5 to 7):1;

[0029] Wherein, the component A is prepared by the following steps:

[0030] S10. dissolving bisphenol A epoxy resin in a solvent and heating the mixture to 80° C. to 130° C. to obtain a bisphenol A epoxy resin solution;

[0031] S20. Mix hydroxy acrylate, auxiliary agent and organosilicon intermediate to obtain an organosilicon intermediate mixture; the weight ratio of the hydroxy acrylate, auxiliary agent and organosilicon intermediate is: (2 to 10): (23.5 to 81): (3 to 8).

[0032] S30. Add the organosilicon intermediate mixture dropwise into the bisphenol A epoxy resin solution to carry out a reaction. After the reaction is completed, keep the mixture warm for a predetermined time and cool it down to obtain a composite modified hydroxy acrylic resin, i.e., component A. The weight ratio of the bisphenol A epoxy resin to the organosilicon intermediate is (5 to 10):(3 to 8). Preferably, the organosilicon intermediate mixture is added dropwise into the bisphenol A epoxy resin solution for 3 to 8 hours.

[0033] The B component is prepared by the following steps:

[0034] K10. Carbodiimide-modified MDI and polymeric MDI are mixed to obtain an MDI mixture;

[0035] K20. The MDI mixture is heated to a first temperature, stirred for reaction, and after the reaction is completed, the temperature is lowered and the material is discharged to obtain a modified isocyanate, namely, the B component. The first temperature is 70° C. to 90° C., preferably 80° C.; the stirring time during the stirring reaction is 1 h to 2 h.

[0036] Among them, the component A is the main agent, and the component B is the curing agent.

[0037] The main agent adopts bisphenol A epoxy resin and epoxy silicone intermediates, acrylate monomers and styrene as the main raw materials of hydroxy polyacrylic resin, which has excellent bonding strength to Nomex insulation paper, PET sheet and PA film; by adding bisphenol A epoxy resin and silicone intermediates, the adhesion to PET sheet and PA film can be enhanced, and the heat resistance of the adhesive layer at high temperature can be improved. Preferably, in the present invention, the rotational viscosity of component A at 25°C is 500mpa.s to 2000mpa.s, and the solid content is 50% to 70%; the relative molecular mass of component A is 10000 to 50000, the acid value is less than 5mgKOH / g, the hydroxyl value is 5mgKOH / g to 25mgKOH / g, and the glass transition temperature is -10°C to 5°C.

[0038] The curing agent uses liquid isocyanate with high NCO content, which has excellent bonding strength to Nomex paper material after cross-linking and curing with the main agent, and also has excellent high temperature resistance, oil resistance, corrosion resistance, acid and alkali resistance, etc. The composite adhesive composed of the main agent and the curing agent is used for composite bonding of aramid paper insulation paper composite materials, which can meet the requirements for bonding, high temperature resistance, hydrolysis resistance, alkali resistance, chemical resistance, etc.

[0039] In the present invention, the curing agent is a mixture of carbodiimide modified MDI and polymerized MDI, both of which are liquid isocyanates. After mixing and heating, the NCO content reaches 25% to 35%. The high NCO content in the curing agent can increase the density of the urethane bond, thereby improving the adhesion and heat resistance of the adhesive. Preferably, the rotational viscosity of the B component at 25° C. is 50 mPa.s to 500 mPa.s, and the solid content is 90% to 100%.

[0040] Specifically, the auxiliary agent is: methacrylate monomer, methacrylic acid, styrene and initiator, and the weight ratio of the methacrylate monomer, methacrylic acid, styrene and initiator is: (10 to 35): (3 to 8): (10 to 35): (0.5 to 3).

[0041] Specifically, the epoxy value of the bisphenol A epoxy resin is 0.2 to 0.52.

[0042] Preferably, the organosilicon intermediate is one or more organosilicon intermediates containing epoxy or unsaturated double bonds, for example, the organosilicon intermediate is selected from 3-(methacryloyloxy)propyltrimethoxysilane, vinyltrimethoxysilane, vinyltriisopropoxysilane, 3-glycidyloxypropyltrimethoxysilane and epoxytrimethoxysilane.

[0043] In some specific embodiments, the solvent is at least one of xylene, ethyl acetate, butyl acetate, propylene glycol butyl ether, propylene glycol methyl ether, ethylene glycol methyl ether, and ethylene glycol butyl ether. The solvent is preferably at least one of ethyl acetate, butyl acetate, and xylene.

[0044] In some specific embodiments, the methacrylate monomer is at least one of methyl methacrylate, butyl methacrylate, ethyl methacrylate, and isobornyl methacrylate. The methacrylate monomer is a major component of the high molecular weight modified acrylic polymer.

[0045] The hydroxy acrylate is at least one of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate and hydroxypropyl methacrylate.

[0046] In some specific embodiments, the initiator is one or more of azobisisobutyronitrile, azobisisovaleronitrile, tert-butyl hydroperoxide, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide. Azobisisobutyronitrile is preferred. The initiator initiates free radical polymerization of unsaturated monomers to control the molecular weight of the polymer.

[0047] In some preferred embodiments, in step K10, the weight ratio of the carbodiimide-modified MDI to the polymeric MDI is (1:9) to (9:1), preferably 1:1.

[0048] The following specific experimental examples are used to further illustrate the technical solutions and technical effects of the present invention. It should be noted that the following experimental examples are only for further explaining the present invention and do not limit the technical solutions of the present invention.

[0049] Experimental Example 1: Component A is not modified

[0050] 1.1 Experimental procedures

[0051] 1.1.1 Preparation of component A

[0052] Add solvent a, solvent b, and solvent c into a reaction kettle, raise the temperature to 100°C, and dropwise add a mixed solution consisting of methyl methacrylate, butyl methacrylate, styrene, isobornyl methacrylate, tert-butyl hydroperoxide, methacrylic acid, and hydroxypropyl acrylate. The dropping time is 5 hours. After the dropping is completed, keep warm for 4 hours, and then cool to room temperature to obtain component A. The feeding amounts of the above components are shown in Table 1:

[0053] Table 1 Feeding amount of each component in Experimental Example 1

[0054]

[0055]

[0056] 1.1.2 Detection of component A

[0057] The rotational viscosity, solid content, relative molecular weight, acid value, hydroxyl value and glass transition temperature of component A at 25°C were tested. The test results are shown in Table 5.

[0058] 1.1.3 Preparation of component B

[0059] The reactor was heated to 80° C., 50% of carbodiimide-modified MDI and 50% of MDI oligomer were mixed to obtain an MDI mixture, the MDI mixture was stirred for 2 hours, and the temperature was lowered and discharged; component B having a rotational viscosity of 125 mPa.s at 25° C., a solid content of 97%, and an NCO content of 28% was obtained.

[0060] 1.2 Experimental Results

[0061] After the experiment, component A and component B were evenly mixed in a ratio of 7:1 to obtain a composite adhesive. Taihe New Materials Minshida aramid paper and commercially available PET film were used to test the performance of the composite adhesive. The test results are shown in Table 6.

[0062] Experimental Example 2: Adding bisphenol A epoxy resin to component A

[0063] 2.1 Experimental procedures

[0064] 2.1.1 Preparation of component A

[0065] The preparation steps of component A in this experimental example are different from those in the above experimental example 1 in that bisphenol A epoxy resin and solvent a, solvent b, and solvent c are added to the reaction kettle, and the temperature is raised to 100° C. The other steps are the same as those in the above experimental example 1. The feeding amounts of the components in this experimental example are shown in Table 2:

[0066] Table 2 Feeding amount of each component in Experimental Example 2

[0067]

[0068]

[0069] 2.1.2 Detection of component A

[0070] The rotational viscosity, solid content, relative molecular weight, acid value, hydroxyl value and glass transition temperature of component A at 25°C were tested. The test results are shown in Table 5.

[0071] 2.1.3 Preparation of component B

[0072] The preparation method of component B in this experimental example is the same as the preparation method of the above-mentioned experimental example 1.

[0073] 2.2 Experimental Results

[0074] After the experiment, component A and component B were evenly mixed in a ratio of 7:1 to obtain a composite adhesive. Taihe New Materials Minshida aramid paper and commercially available PET film were used to test the performance of the composite adhesive. The test results are shown in Table 6.

[0075] Experimental Example 3: Adding silicone intermediate to component A

[0076] 3.1 Experimental procedures

[0077] 3.1.1 Preparation of component A

[0078] The preparation steps of component A in this experimental example are different from those in the above experimental example 1 in that: solvent a, solvent b, and solvent c are added to the reaction kettle, the temperature is raised to 100° C., and a mixed solution consisting of methyl methacrylate, butyl methacrylate, styrene, isobornyl methacrylate, tert-butyl hydroperoxide, methacrylic acid, hydroxypropyl acrylate, and an organosilicon intermediate is added dropwise. The other steps are the same as those in the above experimental example 1. The feeding amounts of the components in this experimental example are shown in Table 3:

[0079] Table 3 Feeding amount of each component in Experimental Example 3

[0080]

[0081] 3.1.2 Detection of component A

[0082] The rotational viscosity, solid content, relative molecular weight, acid value, hydroxyl value and glass transition temperature of component A at 25°C were tested. The test results are shown in Table 5.

[0083] 3.1.3 Preparation of component B

[0084] The preparation method of component B in this experimental example is the same as the preparation method of component B in the above experimental example 1.

[0085] 3.2 Experimental Results

[0086] After the experiment, component A and component B were evenly mixed in a ratio of 7:1 to obtain a composite adhesive. Taihe New Materials Minshida aramid paper and commercially available PET film were used to test the performance of the composite adhesive. The test results are shown in Table 6.

[0087] Experimental Example 4: Adding bisphenol A epoxy resin and silicone intermediate to component A

[0088] 4.1 Experimental procedures

[0089] 4.1.1 Preparation of component A

[0090] The preparation steps of component A in this experimental example are different from those in the above experimental example 1 in that: bisphenol A epoxy resin and solvent a, solvent b, and solvent c are added to the reaction kettle, and the temperature is raised to 100° C.; a mixed solution consisting of methyl methacrylate, butyl methacrylate, styrene, isobornyl methacrylate, tert-butyl hydroperoxide, methacrylic acid, hydroxypropyl acrylate, and an organosilicon intermediate is added dropwise, and the other steps are the same as those in the above experimental example 1. The feeding amounts of the components in this experimental example are shown in Table 4:

[0091] Table 4 Feeding amount of each component in Experimental Example 4

[0092]

[0093] 4.1.2 Detection of component A

[0094] The rotational viscosity, solid content, relative molecular weight, acid value, hydroxyl value and glass transition temperature of component A at 25°C were tested. The test results are shown in Table 5.

[0095] 4.1.3 Preparation of component B

[0096] The preparation method of component B in this experimental example is the same as the preparation method of component B in the above experimental example 1.

[0097] 4.2 Experimental Results

[0098] After the experiment, the properties of component A obtained in the above embodiments 1 to 4 were tested, and the test data are shown in Table 5; component A and component B were evenly mixed in a ratio of 7:1 to obtain a composite adhesive, and Taihe New Materials Minshida aramid paper and commercially available PET film were used to test the performance of the composite adhesive. The test results are shown in Table 6.

[0099] Table 5 Test table of component properties of Experimental Examples 1 to 4A

[0100]

[0101] From the data in Table 5, it can be seen that the relative molecular mass of component A in Experimental Example 4 is 25,000, the acid value is 3 mgKOH / g, and the glass transition temperature is -3°C. Compared with component A in Experimental Examples 1, 2, and 3, the performance is better.

[0102] Table 6 Product performance test table of Experimental Examples 1 to 4

[0103]

[0104] The data in Table 6 show that in Experimental Example 1, the component A does not contain bisphenol A epoxy resin and silicone intermediate, and the prepared adhesive has low peel strength, low heat resistance, insufficient oil resistance, and low strength, and can only be used for Class B insulating paper composite materials;

[0105] In Experimental Example 2, bisphenol A epoxy resin is added to component A without adding silicone intermediates, and the oil resistance of the prepared adhesive is improved, but its heat resistance, peel strength and breakdown voltage resistance are insufficient, and it can only be used for H-class insulating paper composite materials;

[0106] In Experimental Example 3, the silicone intermediate is added to the component A, and the bisphenol A epoxy resin is not added. The peel strength and heat resistance of the prepared adhesive are improved, but the oil resistance is not improved, and the breakdown voltage resistance is low. When the adhesive is used for the C-grade aramid paper insulation paper composite material, it cannot meet the requirements for bonding, oil resistance, corrosion resistance, alkali resistance and other properties;

[0107] In Experimental Example 4, bisphenol A epoxy resin and silicone intermediate are added to component A, and the prepared adhesive has improved peel strength, improved heat resistance, enhanced oil resistance, and good breakdown voltage resistance. When the adhesive is used for C-grade aramid paper insulation paper composite materials, it can meet the requirements for bonding, oil resistance, heat resistance, corrosion resistance, alkali resistance and other properties.

[0108] Experimental Example 5: Changing the amount of bisphenol A epoxy resin in component A

[0109] 5.1 Experimental procedures

[0110] 5.1.1 Preparation of Component A

[0111] The difference between the preparation steps of component A in this experimental example and the preparation steps of component A in the above experimental example 4 is that when the feeding amount of the organosilicon intermediate is 5 g, the feeding amount of the bisphenol A epoxy resin is changed, and the other steps are the same as the preparation steps of component A in the above experimental example 1. The feeding amount of the bisphenol A epoxy resin is shown in Table 7:

[0112] Table 7 Feeding amount of bisphenol A epoxy resin in Experimental Example 5

[0113]

[0114] Note: The other raw materials for preparing component A in this experimental example are the same as the raw materials for preparing component A in the above experimental example 4, and are not listed in this table.

[0115] 5.1.2 Preparation of component B

[0116] The preparation method of component B in this experimental example is the same as the preparation method of component B in the above experimental example 4.

[0117] 5.2 Experimental Results

[0118] After the experiment, component A and component B were mixed evenly in a ratio of 7:1 to obtain a composite adhesive. Taihe New Materials Minshida aramid paper and commercially available PET film were used to test the performance of the composite adhesive. The test results are shown in Table 8:

[0119] Table 8 Experimental Example 5 Product Performance Test Table

[0120]

[0121] It can be seen from the experimental data in Table 8 that when the feed amount of the organosilicon intermediate is 5%, when the feed amount of the bisphenol A epoxy resin is less than 5%, the heat resistance and oil resistance of the prepared adhesive are insufficient;

[0122] When the dosage of the organosilicon intermediate is 5%, and the dosage of the bisphenol A epoxy resin is greater than 10%, component A is turbid and has gel, and the properties of the prepared product are poor;

[0123] When the dosage of the organosilicon intermediate is 5% and the dosage of the bisphenol A epoxy resin is 5% to 10%, the oil resistance of the prepared adhesive can be improved. When the adhesive is used for C-grade aramid paper insulation paper composite materials, it can meet the requirements for bonding, oil resistance, heat resistance, corrosion resistance, alkali resistance and other properties, and the best effect is achieved when the dosage of the bisphenol A epoxy resin is 7%.

[0124] Experimental Example 6: Changing the amount of the organosilicon intermediate in component A

[0125] 6.1 Experimental procedures

[0126] 6.1.1 Preparation of Component A

[0127] The difference between the preparation steps of component A in this experimental example and the preparation steps of component A in the above experimental example 4 is that when the feeding amount of the bisphenol A epoxy resin is 7g, the feeding amount of the organosilicon intermediate is changed, and the other steps are the same as the preparation steps of component A in the above experimental example 4. The feeding amount of the organosilicon intermediate is shown in Table 9:

[0128] Table 9 Feeding amount of organic silicon intermediate in Experimental Example 6

[0129]

[0130] Note: The other raw materials for preparing component A in this experimental example are the same as the raw materials for preparing component A in the above experimental example 4, and are not listed in this table.

[0131] 6.1.2 Preparation of component B

[0132] The preparation method of component B in this experimental example is the same as the preparation method of component B in the above experimental example 4.

[0133] 6.2 Experimental Results

[0134] After the experiment, component A and component B were mixed evenly in a ratio of 7:1 to obtain a composite adhesive. Taihe New Materials Minshida aramid paper and commercially available PET film were used to test the performance of the composite adhesive. The test results are shown in Table 10:

[0135] Table 10 Experimental Example 6 Product Performance Test Table

[0136]

[0137] It can be seen from the data in Table 10 that when the feed amount of the bisphenol A epoxy resin is 7% and the feed amount of the organosilicon intermediate is less than 3%, the heat resistance of the prepared product is poor and can only be used for Class F aramid paper insulation paper composite materials at most;

[0138] When the feed amount of the bisphenol A epoxy resin is 7%, and the feed amount of the organosilicon intermediate is greater than 8%, component A is turbid, the organosilicon intermediate is incompatible with other raw materials, and the properties of the prepared product are poor;

[0139] When the feed amount of the bisphenol A epoxy resin is 7% and the feed amount of the silicone intermediate is 3% to 8%, the peel strength, heat resistance, oil resistance and breakdown voltage resistance of the prepared product are improved. When the adhesive is used for C-grade aramid paper insulation paper composite materials, it can meet the requirements for bonding, oil resistance, heat resistance, corrosion resistance, alkali resistance and other properties, and the best effect is achieved when the feed amount of the silicone intermediate is 5%.

[0140] Experimental Example 7: Changing the amount of carbodiimide-modified MDI in component B

[0141] 7.1 Experimental procedures

[0142] 7.1.1 Preparation of Component A

[0143] The preparation steps of component A in this experimental example are the same as the preparation steps of component A in the above-mentioned experimental example 4.

[0144] 7.1.2 Preparation of component B

[0145] The difference between the preparation method of component B in this experimental example and the preparation steps of component B in the above-mentioned experimental example 4 is that the feeding amount of the carbodiimide-modified MDI is changed. The feeding amount of the carbodiimide-modified MDI is shown in Table 11:

[0146] Table 11 Feeding amount of carbodiimide modified MDI in Experimental Example 7

[0147]

[0148] 7.2 Experimental Results

[0149] After the experiment, component A and component B were mixed evenly in a ratio of 7:1 to obtain a composite adhesive. Taihe New Materials Minshida aramid paper and commercially available PET film were used to test the performance of the composite adhesive. The test results are shown in Table 12:

[0150] Table 12 Experimental Example 7 Product Performance Test Table

[0151]

[0152] The data in Table 12 above show that by changing the ratio of carbodiimide MDI to MDI oligomer, the higher the MDI oligomer content in the eleventh group, the better the adhesion of the adhesive; the higher the carbodiimide content in the twelfth group, the better the breakdown voltage; and it has little effect on heat resistance and oil resistance.

[0153] Experimental Example 8: Determining the weight ratio of component A to component B

[0154] 8.1 Experimental procedures

[0155] 8.1.1 Preparation of Component A

[0156] The preparation steps of component A in this experimental example are the same as the preparation steps of component A in the above-mentioned experimental example 4.

[0157] 8.1.2 Preparation of component B

[0158] The preparation method of component B in this experimental example is the same as the preparation steps of component B in the above experimental example 4.

[0159] 8.2 Experimental Results

[0160] After the experiment, component A and component B were mixed evenly according to different proportions. The specific proportions are shown in Table 13:

[0161] Table 13 Ratio of component A to component B

[0162] Experimental groups The ratio of component A to component B Group 13 1:1 Group 14 3:1 Group 15 5:1 Group 16 7:1 Group 17 9:1

[0163] Component A and component B were mixed according to the ratio in Table 13 to obtain a composite adhesive. Taihe New Materials Minshida aramid paper and commercially available PET film were used to test the performance of the composite adhesive. The test results are shown in Table 14:

[0164] Table 14 Experimental Example 8 Product Performance Test Table

[0165]

[0166] Please refer to Table 14. When the weight ratio of the component A to the component B is less than 5:1, the peel strength of the product is lower than 25, and its adhesion is poor and cannot be used. When the weight ratio of the component A to the component B is greater than 7:1, the peel strength of the product is lower than 30, and its adhesion is also poor and cannot be used. Therefore, when the weight ratio of the component A to the component B is (5 to 7):1, it is effective, and when it is 7:1, the effect is optimal.

[0167] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or substitutions within the technical scope disclosed by the present invention, and these modifications or substitutions should be included in the protection scope of the present invention.

Claims

1. An aramid paper composite adhesive, characterized in that: Comprising a component A and a component B, wherein the weight ratio of the component A to the component B is (5 to 7):1; Wherein, the A component is prepared by the following steps: S10. dissolving bisphenol A epoxy resin in a solvent and heating the mixture to 80° C. to 130° C. to obtain a bisphenol A epoxy resin solution; S20. Mixing hydroxy acrylate, an auxiliary agent and an organosilicon intermediate to obtain an organosilicon intermediate mixture; S30. Adding the organosilicon intermediate mixture dropwise to the bisphenol A epoxy resin solution to react, and after the reaction is completed, keeping the mixture warm for a predetermined time, cooling the mixture, and obtaining a composite modified hydroxy acrylic resin, i.e., the component A; wherein the weight ratio of the bisphenol A epoxy resin to the organosilicon intermediate is (5 to 10):(3 to 8); The B component is prepared by the following steps: K10. Carbodiimide-modified MDI and polymeric MDI are mixed to obtain an MDI mixture; K20. The MDI mixture is heated to a first temperature and stirred for reaction. After the reaction is completed, the temperature is lowered and the material is discharged to obtain a modified isocyanate, namely, the B component.

2. The aramid paper composite material adhesive according to claim 1, characterized in that: The auxiliary agent is: methacrylate monomer, methacrylic acid, styrene and initiator, and the weight ratio of the methacrylate monomer, methacrylic acid, styrene and initiator is: (10 to 35): (3 to 8): (10 to 35): (0.5 to 3).

3. The aramid paper composite material adhesive according to claim 1, characterized in that: The rotational viscosity of component A at 25°C is 500mPa.s to 2000mPa.s, and the solid content is 50% to 70%; the relative molecular mass of component A is 10000 to 50000, the acid value is less than 5mgKOH / g, the hydroxyl value is 5mgKOH / g to 25mgKOH / g, and the glass transition temperature is -10°C to 5°C.

4. The aramid paper composite material adhesive according to claim 1, characterized in that: The organosilicon intermediate is one or more organosilicon intermediates containing epoxy or unsaturated double bonds.

5. The aramid paper composite material adhesive according to claim 1, characterized in that: The solvent is at least one of xylene, ethyl acetate, butyl acetate, propylene glycol butyl ether, propylene glycol methyl ether, ethylene glycol methyl ether and ethylene glycol butyl ether.

6. The aramid paper composite material adhesive according to claim 2, characterized in that: The methacrylate monomer is at least one of methyl methacrylate, butyl methacrylate, ethyl methacrylate and isobornyl methacrylate.

7. The aramid paper composite material adhesive according to claim 1, characterized in that: The hydroxy acrylate is at least one of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate and hydroxypropyl methacrylate.

8. The aramid paper composite material adhesive according to claim 2, characterized in that: The initiator is at least one of azobisisobutyronitrile, azobisisovaleronitrile, tert-butyl hydroperoxide, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide.

9. The aramid paper composite material adhesive according to claim 1, characterized in that: In step K10, the weight ratio of the carbodiimide-modified MDI to the polymeric MDI is (1:9) to (9:1).

10. The aramid paper composite material adhesive according to claim 1, characterized in that: The B component has a rotational viscosity of 50 to 500 mPa.s at 25° C., a solid content of 90 to 100%, and an NCO content of 25 to 35%.

Citation Information

Patent Citations

  • Adhesive for C-grade insulation paper composite material and preparation method thereof

    CN114085639A

  • Female glue film structure that arranges of stromatolite that resistant humid tropical insulating properties is stable

    CN206558295U