Silicate near-infrared fluorescent material as well as preparation method and application thereof
By combining the silicate near-infrared fluorescent material Ba9-xSrxSc1.98Cr0.02Si6O24 with a blue light LED chip, a high-efficiency and long-life near-infrared fluorescence conversion LED device is built, solving the low energy efficiency and spectral band of near-infrared light sources in the existing technology The narrow problem realizes broadband near-infrared spectral output and is suitable for multi-field detection.
Patent Information
- Application Number
- CN202410906879.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing near-infrared light sources such as incandescent lamps and tungsten halogen lamps have low energy efficiency, large size and narrow spectral bands of semiconductor LED lamps. They are not suitable for spectral detection and lack highly efficient, mature structure, low cost and adjustable near-infrared fluorescent materials.
A silicate near-infrared fluorescent material Ba9-xSrxSc1.98Cr0.02Si6O24 and its preparation method are provided. By firing raw materials at 1400°C to form a uniform powder, a broadband near-infrared fluorescent conversion LED device is constructed in combination with a blue light LED chip.
Achieve high-efficiency, long-life, green and pollution-free near-infrared light sources, with a wide coverage range, suitable for food, agricultural product testing, biomedical and environmental pollution detection and other fields. The emission intensity remains stable under temperature changes, and the fluorescence life reaches 56.51μs .
Smart Images

Figure CN118879321A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of near-infrared fluorescent materials, and in particular to a silicate near-infrared fluorescent material and a preparation method and application thereof. Background Art
[0002] Since the invention of blue light emitting diodes in the early 20th century, people have revolutionized the lighting industry by combining inorganic luminescent materials activated by rare earth ions with blue light LEDs, which has promoted the technological progress of the lighting industry. Today, white light emitting diodes (WLEDs) have become a new light source for lighting and backlighting displays in the 21st century. With the advancement of human technology and the demand for a high quality of life, people are paying more and more attention to their health, such as analyzing the ingredients of the food they eat and the growth status of the plants they grow. Ordinary visible light luminescent materials cannot achieve these functions.
[0003] In recent years, the application of near-infrared luminescent materials (NIR, 800-2500nm) in the fields of biological imaging, cancer research, non-destructive quality analysis of food / agricultural products, security monitoring, face recognition and 3D sensing has become the focus at home and abroad; especially the wide spectrum of 650nm-1050nm covers the double frequency and sum frequency characteristic information of the vibration of hydrogen-containing groups (OH, NH, CH). By scanning the near-infrared wide spectrum of the sample, the characteristic information of the hydrogen-containing groups of organic molecules in the sample can be obtained, which can be widely used in the field of food detection. In addition to being able to easily detect food related to our daily life and provide protection for our health, the wide spectrum or multi-spectrum of 850-1200nm and 1400-1800nm can be used in medical detection, biometrics and security monitoring.
[0004] Traditional near-infrared light sources such as incandescent lamps and halogen tungsten lamps can provide continuous near-infrared light output, but they have problems such as low energy efficiency, large size and high operating temperature. Semiconductor LED lamps are small in size and high in efficiency, but have a narrow spectral band and are not suitable for spectral detection. Using high-efficiency blue light LED chips to excite phosphors to achieve continuous broadband near-infrared output has become an ideal solution for building a new generation of near-infrared light sources. This broadband near-infrared fluorescent conversion LED (pc-LED) light source has the advantages of mature structure, low cost, small size, adjustable spectral bandwidth, high light efficiency, fast response speed and long life. As the core material for realizing light conversion function and providing broadband spectral output, high-performance near-infrared phosphors are the key to the large-scale application of pc-LED near-infrared light sources.
[0005] Therefore, it is necessary to provide a silicate near-infrared fluorescent material and a preparation method and application thereof, in order to solve the above problems. Summary of the invention
[0006] In view of the deficiencies in the prior art, an object of the embodiments of the present invention is to provide a silicate near-infrared fluorescent material and a preparation method and application thereof, so as to solve the problems in the above-mentioned background technology.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] A silicate near-infrared fluorescent material, the chemical formula of which is Ba 9- x Sr x Sc 1.98 Cr 0.02 SiO 24 , where 2≤x≤8.
[0009] A method for preparing a silicate near-infrared fluorescent material comprises the following steps:
[0010] Step S1, according to the chemical formula Ba 9-x Sr x Sc 1.98 Cr 0.02 SiO 24 , weighing raw materials according to the molar ratio of each element in the raw materials Ba: Sr: Sc: Cr: Si = 9-x: x: 1.98: 0.02: 6, x is 2≤x≤8, wherein the raw materials include compounds containing Ba, Sr, Sc, Cr and Si elements respectively;
[0011] Step S2, adding anhydrous ethanol as a dispersant to the weighed raw materials and grinding them fully until the alcohol evaporates to obtain a uniform white powder;
[0012] Step S3, calcining the ground white powder at 1400° C. for 4 hours, and then slowly cooling to room temperature until cooled, to obtain the silicate near-infrared fluorescent material.
[0013] As a further embodiment of the present invention, the compound containing Ba is any one of BaCO3, BaO and BaCl2.
[0014] As a further embodiment of the present invention, the Sr-containing compound is any one of SrO, SrCO3, SrO2, SrWO4 and C4H6O4Sr.
[0015] As a further embodiment of the present invention, the Sc-containing compound is any one of Sc2O3, Sc(NO3)3 and Sc2(CO3)3.
[0016] As a further embodiment of the present invention, the Cr-containing compound is any one of Cr2O3, Cr(NO3)3 and (CH3COO)3Cr.
[0017] As a further embodiment of the present invention, the Si-containing compound is SiO2, H2SiO3 and C8H 20 Any one of O4Si.
[0018] As a further solution of the present invention, the grinding time in step S2 is 30 minutes.
[0019] An application of the silicate near-infrared fluorescent material in constructing a broadband near-infrared fluorescent conversion LED device.
[0020] In summary, compared with the prior art, the embodiments of the present invention have the following beneficial effects:
[0021] The present invention provides a silicate near-infrared fluorescent material Ba 9-x Sr x Sc 1.98 Cr 0.02 SiO 24 , in the chemical formula Ba 2+ The ions can be mostly replaced by Sr 2+ ion substitution, forming a solid solution, and with the Sr 2+ Ion substitution Ba 2+ In the process of ionization, there is no concentration quenching phenomenon, and the near-infrared emission intensity increases with the increase of substitution concentration, reaching a maximum value when x=8; under the excitation of 470nm blue light, the near-infrared emission with the best emission wavelength at 980nm is obtained; the variable temperature spectrum of the fluorescent material in the temperature range of 20-200℃ is tested. Under the excitation of 470nm wavelength blue light, when the temperature rises to 413K (140℃), its emission intensity maintains 26.83% of the initial intensity, and its fluorescence lifetime is 56.51μs. This near-infrared fluorescent material can be combined with a blue light LED chip to make a near-infrared fluorescence conversion LED device;
[0022] The raw material resource reserves in the preparation method of the present invention are abundant, the preparation method is simple and easy, the physicochemical stability is good, the fluorescence lifetime is ideal, it is green and pollution-free, can be excited by a blue light source to produce a wide spectrum, has a wide coverage range, can be combined with a blue light LED chip to form a broadband near-infrared fluorescence conversion type LED device, has strong applicability, has high luminous intensity, covers a wide wavelength range, and has application prospects in the fields of non-destructive testing, food and agricultural product testing, biomedicine, environmental pollution detection, tracer labeling, etc.
[0023] In order to more clearly illustrate the structural features and effects of the present invention, the present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The XRD patterns of Examples 1-4 and Comparative Example 1 are shown.
[0025] Figure 2 The excitation spectra of Examples 1-4 and Comparative Example 1 under 980nm monitoring are shown.
[0026] Figure 3 The emission spectra of Examples 1-4 and Comparative Example 1 under 470 m excitation are shown.
[0027] Figure 4 It is a thermal quenching curve diagram of Example 4 and Comparative Example 1.
[0028] Figure 5 It is the fluorescence decay curve diagram of Examples 1-4 and Comparative Example 1. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0030] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.
[0031] A method for preparing a silicate near-infrared fluorescent material comprises the following steps:
[0032] Step S1, according to the chemical formula Ba 9-x Sr x Sc 1.98 Cr 0.02 SiO 24 , accurately weigh the corresponding raw materials using an electronic balance according to the molar ratio of each element in the raw materials Ba: Sr: Sc: Cr: Si = 9-x: x: 1.98: 0.02: 6, x is 2≤x≤8, wherein the raw materials include Ba source, Sr source, Sc source, Cr source and Si source;
[0033] Wherein, the Ba-containing compound is any one of BaCO3, BaO and BaCl2, preferably BaCO3;
[0034] The Sr-containing compound is any one of SrO, SrCO3, SrO2, SrWO4 and C4H6O4Sr, preferably SrCO3;
[0035] The Sc-containing compound is any one of Sc2O3, Sc(NO3)3 and Sc2(CO3)3, preferably Sc2O3;
[0036] The Cr-containing compound is any one of Cr2O3, Cr(NO3)3 and (CH3COO)3Cr, preferably Cr2O3;
[0037] The Si-containing compound is SiO2, H2SiO3 and C8H 20 Any one of O4Si, preferably SiO2;
[0038] Step S2, put the weighed raw materials into an agate mortar, add anhydrous ethanol as a dispersant and grind them fully until the alcohol evaporates to obtain a uniform white powder, sinter the ground white powder at 1400° C. for 4 hours, then slowly cool to room temperature until cooled, to obtain the silicate near-infrared fluorescent material.
[0039] Example 1
[0040] A method for preparing a silicate near-infrared fluorescent material comprises the following steps:
[0041] Step S1: According to the chemical formula Ba 9-x Sr x Sc 1.98 Cr 0.02 SiO 24 (x=2), the initial raw materials are BaCO3, SrCO3, Sc2O3, Cr2O3 and SiO2 and are accurately weighed according to the stoichiometric ratio, and an appropriate amount of anhydrous ethanol is added as a dispersant and fully ground for 30 minutes to make the raw materials uniformly mixed to obtain a mixed powder;
[0042] Step S2: Put the mixed powder into an alumina crucible, and then place the crucible in a muffle furnace at 1400°C and slowly cool it to room temperature after firing for 4 hours until it cools down to obtain the corresponding silicate near-infrared fluorescent material.
[0043] Example 2
[0044] A method for preparing a silicate near-infrared fluorescent material comprises the following steps:
[0045] Step S1: According to the chemical formula Ba 9-x Sr x Sc 1.98 Cr 0.02 SiO 24 (x=4), the initial raw materials are BaCO3, SrCO3, Sc2O3, Cr2O3 and SiO2 and are accurately weighed according to the stoichiometric ratio, and an appropriate amount of anhydrous ethanol is added as a dispersant and fully ground for 30 minutes to make the raw materials evenly mixed to obtain a mixed powder;
[0046] Step S2: Put the mixed powder into an alumina crucible, and then place the crucible in a muffle furnace at 1400°C and slowly cool it to room temperature after firing for 4 hours until it cools down to obtain the corresponding silicate near-infrared fluorescent material.
[0047] Example 3
[0048] A method for preparing a silicate near-infrared fluorescent material comprises the following steps:
[0049] Step S1: According to the chemical formula Ba 9-x Sr x Sc 1.98 Cr 0.02 SiO 24 (x=6), the initial raw materials are BaCO3, SrCO3, Sc2O3, Cr2O3 and SiO2 and are accurately weighed according to the stoichiometric ratio, and an appropriate amount of anhydrous ethanol is added as a dispersant and fully ground for 30 minutes to make the raw materials evenly mixed to obtain a mixed powder;
[0050] Step S2: Put the mixed powder into an alumina crucible, and then place the crucible in a muffle furnace at 1400°C and slowly cool it to room temperature after firing for 4 hours until it cools down to obtain the corresponding silicate near-infrared fluorescent material.
[0051] Example 4
[0052] A method for preparing a silicate near-infrared fluorescent material comprises the following steps:
[0053] Step S1: According to the chemical formula Ba 9-x Sr x Sc 1.98 Cr 0.02 SiO 24 (x=8), the initial raw materials are BaCO3, SrCO3, Sc2O3, Cr2O3 and SiO2 and are accurately weighed according to the stoichiometric ratio, and an appropriate amount of anhydrous ethanol is added as a dispersant and fully ground for 30 minutes to make the raw materials evenly mixed to obtain a mixed powder;
[0054] Step S2: Put the mixed powder into an alumina crucible, and then place the crucible in a muffle furnace at 1400°C and slowly cool it to room temperature after firing for 4 hours until it cools down to obtain the corresponding silicate near-infrared fluorescent material.
[0055] Comparative Example 1
[0056] A method for preparing a silicate near-infrared fluorescent material comprises the following steps:
[0057] Step S1: According to the chemical formula Ba9Sc 1.98 Cr 0.02 SiO 24 The initial raw materials are BaCO3, Sc2O3, Cr2O3 and SiO2, which are accurately weighed according to the stoichiometric ratio, and an appropriate amount of anhydrous ethanol is added as a dispersant to fully grind for 30 minutes to mix the raw materials evenly to obtain a mixed powder;
[0058] Step S2: Put the mixed powder into an alumina crucible, and then place the crucible in a muffle furnace at 1400°C and slowly cool it to room temperature after firing for 4 hours until it cools down to obtain the corresponding silicate near-infrared fluorescent material.
[0059] Performance Test:
[0060] The samples prepared in Examples 1-4 and Comparative Example 1 were analyzed using powder X-ray diffraction (XRD) technology to obtain XRD patterns as shown in Figure 1 As shown; it can be seen that Ba 9-x Sr x Sc 1.98 Cr 0.02 SiO 24 (2≤x≤8) and Comparative Example 1Ba 9-x Sr x Sc 1.98 Cr 0.02 SiO 24 All of them can match well with the standard card PDF#82-1119, indicating that the prepared fluorescent materials are all pure phase;
[0061] Figure 2 , Figure 3 The excitation and emission spectra of the samples prepared in Examples 1-4 and Comparative Example 1 are given; it can be seen that the excitation spectra of the samples under 980nm monitoring show a broadband excitation peak in the range of 250 to 750nm, and there is strong excitation near 470nm, indicating that it can be applied to near-infrared fluorescence conversion LED devices excited by blue light LED chips. Under 470nm excitation, the samples show near-infrared emission, the range extends from 600nm to around 1600nm, and the main emission peak wavelength is located near 980nm;
[0062] Figure 4 This is a thermal quenching curve of the sample prepared in Example 4 under 470nm excitation. It can be seen that the sample has relatively good thermal stability at 20°C to 200°C, and the emission intensity at 413K (140°C) remains at 26.83% of the initial intensity (20°C);
[0063] Figure 5 The fluorescence lifetime decay curves of the samples prepared in Examples 1-4 and Comparative Example 1 are given. It can be seen that the fluorescence decay lifetimes of the samples in Examples 1-4 and Comparative Example 1 are all in the microsecond range and the decay lifetime of Example 4 is 56.51 μs.
[0064] In summary, the silicate near-infrared fluorescent material Ba provided by the present invention 9-x Sr x Sc1.98 Cr 0.02 SiO 24 , in the chemical formula Ba 2+ The ions can be mostly replaced by Sr 2+ ion substitution, forming a solid solution, and with the Sr 2+ Ion substitution Ba 2+ There is no concentration quenching phenomenon in the process of ions, and the near-infrared emission intensity increases with the increase of substitution concentration and reaches the maximum intensity when x=8. Under the excitation of 470nm blue light, the near-infrared emission with the best emission wavelength at 980nm is obtained. The variable temperature spectrum of the fluorescent material in the temperature range of 20-200℃ is tested. When the temperature rises to 413K (140℃) under the excitation of 470nm wavelength blue light, its emission intensity maintains 26.83% of the initial intensity. The fluorescence lifetime of the sample reaches 56.51μs when x=8, which meets the needs of practical applications.
[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A silicate near-infrared fluorescent material, characterized in that: The chemical formula of the fluorescent material is Ba 9- x Sr x Sc 1.98 Cr 0.02 SiO 24 , where 2≤x≤8.
2. The method for preparing the silicate near-infrared fluorescent material according to claim 1, characterized in that: The following steps are involved: Step S1, according to the chemical formula Ba 9-x Sr x Sc 1.98 Cr 0.02 SiO 24 , weighing raw materials according to the molar ratio of each element in the raw materials Ba: Sr: Sc: Cr: Si = 9-x: x: 1.98: 0.02: 6, x is 2≤x≤8, wherein the raw materials include compounds containing Ba, Sr, Sc, Cr and Si elements respectively; Step S2, adding anhydrous ethanol as a dispersant to the weighed raw materials and grinding them fully until the alcohol evaporates to obtain a uniform white powder; Step S3, calcining the ground white powder at 1400° C. for 4 hours, and then slowly cooling to room temperature until cooled, to obtain the silicate near-infrared fluorescent material.
3. The method for preparing the silicate near-infrared fluorescent material according to claim 2, characterized in that: The compound containing Ba is any one of BaCO3, BaO and BaCl2.
4. The method for preparing the silicate near-infrared fluorescent material according to claim 2, characterized in that: The compound containing Sr is any one of SrO, SrCO3, SrO2, SrWO4 and C4H6O4Sr.
5. The method for preparing the silicate near-infrared fluorescent material according to claim 2, characterized in that: The Sc-containing compound is any one of Sc2O3, Sc(NO3)3 and Sc2(CO3)3.
6. The method for preparing the silicate near-infrared fluorescent material according to claim 2, characterized in that: The Cr-containing compound is any one of Cr2O3, Cr(NO3)3 and (CH3COO)3Cr.
7. The method for preparing the silicate near-infrared fluorescent material according to claim 2, characterized in that: The compounds containing Si are SiO2, H2SiO3 and C8H 20 Any one of O4Si.
8. The method for preparing the silicate near-infrared fluorescent material according to claim 2, characterized in that: The grinding time in step S2 is 30 min.
9. Use of the silicate near-infrared fluorescent material according to claim 1 in a broadband near-infrared fluorescence conversion type LED device.
Citation Information
Cited By
Fluorescent ceramic with high light extraction efficiency and concentration gradient as well as preparation method and application of fluorescent ceramic
CN119930329A
High light extraction efficiency concentration gradient fluorescent ceramic, preparation method and application
CN119930329B