Light color adjustable aluminosilicate fluorescent material as well as preparation method and application thereof
The Tb3+ and Eu3+ co-doped Y(2-x-y)MgAl4SiO12:xTb3+, yEu3+ type aluminosilicate fluorescent materials were synthesized by high-temperature solid phase method, and multi-color luminescence was achieved using the energy transfer of Tb3+ and Eu3+, which solved the existing technology in The problems of low luminous efficiency of fluorescent materials and uneven white light are suitable for white LED devices, improving luminous efficiency and color index.
Patent Information
- Application Number
- CN202410920016.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-01
AI Technical Summary
The existing three-primary color fluorescent materials have low luminescence efficiency, and there is a lack of Tb3+ and Eu3+ co-doped light-color adjustable aluminosilicate fluorescent materials in single-phase fluorescent materials, resulting in uneven white light and low luminescence efficiency of LED devices.
The high-temperature solid phase method is used to synthesize the Y(2-x-y)MgAl4SiO12:xTb3+, yEu3+ type aluminosilicate fluorescent materials co-doped in air atmosphere, and realize multi-color luminescence through the energy transfer of Tb3+ and Eu3+, which is suitable for White LED devices.
It achieves light-color adjustable performance, good chemical stability, high light conversion efficiency and simple operation. It is suitable for white LEDs and other photoluminescent devices, significantly improving the luminous efficiency of LED devices.
Smart Images

Figure CN118879323A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photoluminescent materials, and in particular relates to a light color-adjustable aluminosilicate fluorescent material and a preparation method and application thereof. Background Art
[0002] At present, the research on developing three-primary color fluorescent materials mainly focuses on doping rare earth (Eu 2+ 、Eu 3+ or Ce 3+ ) systems, such as sulfides, silicates, aluminates, and nitrides (oxy)ides, have made limited progress. Due to the inconsistency of the luminescence characteristics and luminescence reabsorption of different fluorescent materials, their luminescence efficiency is low. As an alternative, obtaining multicolor luminescence in single-phase fluorescent materials has become a hot research topic in recent years. Compared with multi-component emitters, single-phase fluorescent materials with multicolor output can not only improve the color rendering index of fluorescent emission, but also reduce the color temperature.
[0003] In single-phase fluorescent materials, co-doping sensitizers and activators is an effective scheme to achieve multiple luminescence by utilizing energy transfer from sensitizers to activators. 3+ ) is considered to be a red emission activator. 3+ ) is a well-known green emission activator. Recent studies have found that Tb 3+ 、Eu 3+ Co-doped luminescent materials have great potential in the fields of LED devices, temperature sensing, etc., and have great potential for Tb 3+ 、Eu 3+ Co-doped luminescent materials have been extensively studied. Among the numerous phosphor matrices, garnet-based materials have been widely studied as matrices for rare earth ion doping due to their outstanding chemical and physical stability, diverse crystal structures, high luminescence quantum efficiency, low synthesis cost, and low thermal expansion. 3+ 、Eu 3+ Related reports on co-doped color-tunable aluminosilicate fluorescent materials. Summary of the invention
[0004] The present invention provides a Tb 3+ 、Eu 3+A co-doped aluminosilicate fluorescent material with adjustable light color and a preparation method thereof. The method adopts a high-temperature solid-phase method to synthesize the fluorescent material in an air atmosphere. The obtained fluorescent material has adjustable light color performance, which provides a solution to the problems of uneven white light and low luminous efficiency of AC LED devices. The prepared fluorescent material has the advantages of good chemical stability, high light conversion efficiency, simple preparation method and high color index, and is suitable for white light LEDs and other photoluminescent device related fields. In addition, combining (near) ultraviolet (n-UV) LED chips with single-phase phosphors is beneficial to significantly improve the luminous efficiency of LED devices.
[0005] The present invention adopts the following technical solution to solve the above technical problems: a color-adjustable aluminosilicate fluorescent material, characterized in that: the chemical formula of the fluorescent material is Y (2-x-y) MgAl4SiO 12 :xTb 3+ ,yEu 3+ , where x is 0.05-0.30, y is 0.01-0.35, and its crystal structure is garnet type, composed of Tb 3+ 、Eu 3+ Replace Y 3+ Position made.
[0006] It is further defined that the value of x is 0.20.
[0007] The method for preparing the color-adjustable aluminosilicate fluorescent material of the present invention is characterized by the following specific steps: using Y2O3, MgO, Al2O3, SiO2, Tb4O7, and Eu2O3 as raw materials, and preparing the fluorescent material according to the chemical formula Y (2-x-y) MgAl4SiO 12 :xTb 3+ ,yEu 3+ The raw materials are accurately weighed in a stoichiometric ratio; the weighed raw materials are mixed, ground, and dried to obtain a mixed raw material; the obtained mixed raw material is calcined at 1350-1550° C. for 3-10 hours in an air atmosphere, cooled to room temperature, and ground again to obtain a color-adjustable aluminosilicate fluorescent material.
[0008] The application of the color-adjustable aluminosilicate fluorescent material in the preparation of a photoluminescent device is characterized in that: at the same excitation wavelength, by changing the Eu 3+ The doping concentration can achieve the regulation of the color of the fluorescent material from green to red, where the excitation wavelength is 275nm, 320nm, 353nm or 380nm.
[0009] The invention discloses an application of the light color adjustable aluminosilicate fluorescent material in preparing an AC white light LED device.
[0010] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0011] The high-temperature solid-phase reaction method adopted by the present invention is relatively simple, easy to operate, and has a rapid reaction. The aluminosilicate matrix material used has good thermal stability and chemical stability. The prepared fluorescent material has good single-phase property and can be mass-produced.
[0012] The Tb prepared by the present invention 3+ 、Eu 3+ Co-doped aluminosilicate Y2MgAl4SiO 12 Fluorescent material, activator Tb 3+ As both a green light emitting center and a sensitizer, Eu 3+ The direct excitation efficiency of the ff transition is low, but a higher luminescence efficiency can be achieved through the energy transfer process; and a red-green color-adjustable luminescence mode can be effectively realized, which has potential applications in white light LED devices and other photoluminescent devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is the XRD spectrum of the fluorescent material prepared in Comparative Examples 1-2.
[0014] Figure 2 The XRD patterns of the fluorescent materials prepared in Examples 1-2 and Comparative Example 3 are shown.
[0015] Figure 3a The photoemission spectrum and photoexcitation spectrum of the fluorescent material prepared in Comparative Example 1; Figure 3b and Figure 3c They are the photoemission spectra of the fluorescent materials prepared in Comparative Examples 1 to 3 respectively.
[0016] Figure 4 These are the photoexcitation spectrum and photoemission spectrum of the fluorescent material prepared in Comparative Example 3.
[0017] Figure 5 The photoexcitation spectra of the fluorescent materials prepared in Example 1, Comparative Example 1 and Comparative Example 3 are shown.
[0018] Figure 6a to Figure 6d The photoemission spectra of the fluorescent materials prepared in Examples 1 to 2, Comparative Example 1 and Comparative Example 3 under different excitation lights are shown respectively.
[0019] Figure 7 The chromaticity coordinate diagrams of the fluorescent materials prepared in Examples 1-2 and Comparative Example 1 under different excitation lights. DETAILED DESCRIPTION
[0020] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention.
[0021] Example 1
[0022] A Y (2-x-y) MgAl4SiO 12 :xTb 3+ ,yEu 3+ The co-doped color-adjustable aluminosilicate fluorescent material comprises the following steps:
[0023] According to the chemical formula Y 1.68 MgAl4SiO 12 :0.2Tb 3+ ,0.12Eu 3+ The required raw materials were accurately weighed in a stoichiometric ratio (the overall amount was calculated as 0.004 mol; the same below): 0.1612 g (0.004 mol × 1 × 40.3 g / mol) MgO, 0.8156 g (0.004 mol × 4÷2 × 101.96 g / mol) Al2O3, 0.2403 g (0.004 mol × 1 × 60.08 g / mol) SiO2, 0.1495 g (0.004 mol × 0.2÷4 × 747.7 g / mol) Tb4O7, 0.7587 g ( 0.004mol×1.68÷2×225.81g / mol)Y2O3, 0.0844g(0.004mol×0.12÷5×351.93g / mol)Eu2O3 (all raw materials used are analytical grade); the weighed raw materials are placed in an agate mortar, 5mL of ethanol is added, and ground for 40min until mixed evenly, and dried at 40°C to obtain a mixed raw material; the obtained mixed raw materials are mixed evenly and poured into a crucible, and placed in a tube furnace and calcined at 1485°C for 4h; after calcination, the mixture is cooled to room temperature, and then ground to obtain the fluorescent material Y 1.68 MgAl4SiO 12 :0.2Tb 3+ ,0.12Eu 3+ .
[0024] Example 2
[0025] A series of Y (1.8-y) MgAl4SiO 12 :0.20Tb 3+ ,yEu 3+ The co-doped color-adjustable aluminosilicate fluorescent material comprises the following steps:
[0026] According to the chemical formula Y (1.8-y)MgAl4SiO 12 :0.20Tb 3+ ,yEu 3+ The required raw materials 0.1612g (0.004mol×1×40.3g / mol) MgO, 0.8156g (0.004mol×4÷2×101.96g / mol) Al2O3 and 0.2403g (0.004mol×1×60.08g / mol) SiO2 were accurately weighed according to the stoichiometric ratio. Y2O3 was calculated according to the formula (0.004mol×(1.8-x)÷2×225.81g / mol). ÷2×351.93g / mol) to calculate Eu2O3, where y is 0.01, 0.03, 0.05, 0.08, 0.18, 0.25, 0.35 (all raw materials are analytical grade); the weighed raw materials are placed in an agate mortar, 5 mL of ethanol is added, and the mixture is ground for 40 min until it is evenly mixed, and then dried at 40°C to obtain a mixed raw material; the obtained mixed raw material is mixed evenly and poured into a crucible, and the mixture is placed in a tube furnace and calcined at 1485°C for 4 h; after the calcination, it is cooled to room temperature, and then ground to obtain the fluorescent material Y (1.8-y) MgAl4SiO 12 :0.20Tb 3+ ,yEu 3+ .
[0027] Comparative Example 1
[0028] A Y (2-x) MgAl4SiO 12 :xTb 3+ The single-doped aluminosilicate fluorescent material, the preparation method thereof comprises the following steps:
[0029] According to the chemical formula Y 1.8 MgAl4SiO 12 :0.2Tb 3+The required raw materials were accurately weighed in a stoichiometric ratio (the overall amount was calculated based on 0.004 mol; the same below): 0.1612 g (0.004 mol × 1 × 40.3 g / mol) MgO, 0.8156 g (0.004 mol × 4÷2 × 101.96 g / mol) Al2O3, 0.2403 g (0.004 mol × 1 × 60.08 g / mol) SiO2, 0.8129 g (0.004 mol × 1.8÷2 × 225 .81g / mol)Y2O3, 0.1495g (0.005mol×0.2÷4×747.7g / mol)Tb4O7 (all raw materials used are analytically pure); the weighed raw materials are placed in an agate mortar, 5mL of ethanol is added, and the mixture is ground for 40min until it is evenly mixed, and then dried at 40°C to obtain a mixed raw material; the obtained mixed raw materials are mixed evenly and poured into a crucible, and the mixture is placed in a tube furnace and calcined at 1485°C for 4h; after the calcination, it is cooled to room temperature, and then ground to obtain the fluorescent material Y 1.8 MgAl4SiO 12 :0.2Tb 3+ .
[0030] Table 1 shows the chromaticity coordinates of the fluorescent materials prepared in Examples 1-2 and Comparative Example 1 under different excitation lights.
[0031] Table 1
[0032]
[0033] Comparative Example 2
[0034] A series of Tb 3+ Single doped Y (2-x) MgAl4SiO 12 :xTb 3+ The fluorescent material, the preparation method thereof comprises the following steps:
[0035] According to the chemical formula Y (2-x) MgAl4SiO 12 :xTb 3+The required raw materials are accurately weighed in the stoichiometric ratio: 0.1612 g (0.004 mol × 1 × 40.3 g / mol) MgO, 0.8156 g (0.004 mol × 4÷2 × 101.96 g / mol) Al2O3, 0.2403 g (0.004 mol × 1 × 60.08 g / mol) SiO2, and Y2O3 is calculated according to the formula (0.004 mol × (2-x) ÷ 2 × 225.81 g / mol). ol×x÷4×747.7g / mol) to calculate Tb4O7, where x is 0.05, 0.10, 0.15, 0.25, and 0.30, respectively (all raw materials are analytically pure); the weighed raw materials are placed in an agate mortar, 5 mL of ethanol is added, and the mixture is ground for 40 min until it is evenly mixed, and then dried at 40°C to obtain a mixed raw material; the obtained mixed raw materials are mixed evenly and poured into a crucible, and the mixture is placed in a tube furnace and calcined at 1485°C for 4 h; after the calcination, the mixture is cooled to room temperature, and then ground to obtain the fluorescent material Y (2-x) MgAl4SiO 12 :xTb 3+ .
[0036] Comparative Example 3
[0037] Eu 3+ Single doped Y (2-y) MgAl4SiO 12 :yEu 3+ The fluorescent material, the preparation method thereof comprises the following steps:
[0038] According to the chemical formula Y 1.88 MgAl4SiO 12 :0.12Eu 3+ The required raw materials were accurately weighed in the stoichiometric ratio: 0.1612 g (0.004 mol × 1 × 40.3 g / mol) MgO, 0.8156 g (0.004 mol × 4÷2 × 101.96 g / mol) Al2O3, 0.2403 g (0.004 mol × 1 × 60.08 g / mol) SiO2, 0.8490 g (0.004 mol × 1.88÷2 × 225.81 g / mol) Y2O 3, 0.0844g (0.004mol × 0.12÷2 × 351.93g / mol) Eu2O3 (all raw materials used are analytical grade); the weighed raw materials are placed in an agate mortar, 5mL of ethanol is added, and the mixture is ground for 40min until it is evenly mixed, and then dried at 40°C to obtain a mixed raw material; the obtained mixed raw material is mixed evenly and poured into a crucible, and then placed in a tube furnace and calcined at 1485°C for 4h; after the calcination, it is cooled to room temperature, and then ground to obtain the fluorescent material Y 1.88 MgAl4SiO 12 :0.12Eu3+ .
[0039] Figure 1 , 2 The XRD patterns of the fluorescent materials prepared in Examples 1 to 2 and Comparative Examples 1 to 3 were measured by an X-ray diffractometer (model: Empyrean, Netherlands). The results showed that the samples prepared in Comparative Examples 1 to 2 had the same XRD patterns as Y3Al5O 12 Corresponding to the crystal structure, doping with rare earth ions will not change the crystal structure of the fluorescent material, no impurity peaks appear, and the powder samples are all pure phase (single phase).
[0040] Figure 3 is a photoemission spectrum and a photoexcitation spectrum of the fluorescent materials prepared in Comparative Examples 1 and 2. The test results show that at λ em =545nm monitoring, it was found that there were excitation peaks at 200-390nm, and the strongest peak was at 275nm. Figure 3a As shown. Figure 3b As shown, the four most obvious peaks are located at 493nm, 545nm, 586nm, and 627nm, which are from Tb 3+ of 5 D4→ 7 F6, 7 F5, 7 F4, 7 F3 transition. It is found that the emission spectrum maintains the same shape at different contents, and the emission intensity of the sample increases continuously when the doping concentration increases from x = 0.05 to x = 0.20. When the doping concentration exceeds x = 0.20, it decreases monotonically due to concentration quenching.
[0041] Figure 4 The photoexcitation spectrum and photoemission spectrum of the fluorescent material prepared in Comparative Example 3 are shown in FIG. em =592nm monitoring, the excitation spectrum consists of a charge transfer band in the range of 200-285nm and a series of ff transition emission peaks at 292nm, 320nm, 362nm, 380nm, 394nm and 404nm, which are respectively attributed to Eu 3+ Ionic 7 F0→ 5 H6, 7 F0→ 5 H3, 7 F0→ 5 D4, 7 F0→ 5 G3, 7 F0→ 5 L6 and 7 F0→ 5 D3 transition. The position of the migration band depends largely on the nature of the ligand, mainly involving Eu3+ -O 2- Bond covalency and Eu 3+ For the emission spectrum, under 394nm excitation, the emission spectrum of the phosphor consists of a series of emission peaks located at 567nm, 592nm, 611nm, 631nm, 653nm, 711nm and 746nm, which are respectively attributed to 5 D0→ 7 F J (J=0-4) transition.
[0042] Figure 5 The photoexcitation spectra of the fluorescent materials prepared in Example 1, Comparative Example 1 and Comparative Example 3 are Y 1.88 MgAl4SiO 12 :0.12Eu 3+ Fluorescent materials in λ em =592nm, Y 1.8 MgAl4SiO 12 :0.20Tb 3+ Fluorescent materials in λ em =545nm and Y 1.68 MgAl4SiO 12 :0.20Tb 3+ ,0.12Eu 3+ Fluorescent materials in λ em =592nm monitoring, for Y 1.68 MgAl4SiO 12 :0.20Tb 3+ ,0.12Eu 3+ Fluorescent materials that monitor Eu 3+ The emission excitation spectrum contains Eu 3+ -O 2- Charge transfer band, Eu 3+ and Tb 3+ The characteristic excitation lines of Tb 3+ To Eu 3+ There is energy transfer between ions.
[0043] Figure 6a to Figure 6d The photoemission spectra of the fluorescent materials prepared in Examples 1-2, Comparative Example 1 and Comparative Example 3 are shown in Figure 1. The test results show that Y (1.8-y) MgAl4SiO 12 :0.20Tb 3+ ,yEu 3+The dual-doped fluorescent material shows several obvious emission peaks at 493nm, 545nm, 592nm, 611nm, 631nm and 711nm. These emission peaks are attributed to Tb 3+ and Eu 3+ Characteristic transition of ions. Under the excitation of 275nm and 353nm, Y 1.88 MgAl4SiO 12 :0.12Eu 3+ Fluorescent materials do not emit light. Figure 5 The excitation spectrum of Y is consistent with that of 1.88 MgAl4SiO 12 :0.12Eu 3+ The characteristic radiation of fluorescent materials is significantly weaker than that of Y (1.8-y) MgAl4SiO 12 :0.20Tb 3+ ,yEu 3+ co-doped fluorescent materials, these results also strongly support the 3+ To Eu 3+ Energy transfer does exist. And as Eu 3 + The increase in Tb concentration 3+ The characteristic radiation of Eu gradually weakens. 3+ When the doping concentration of Eu 3+ The emission intensity of Tb 3+ To Eu 3+ The energy transfer of Eu 3+ When the concentration of Eu continues to increase, due to concentration quenching, 3+ The characteristic radiation decreases.
[0044] Figure 7 The chromaticity coordinate diagram of the fluorescent materials prepared in Examples 1 to 2 and Comparative Example 1 is specifically the chromaticity coordinates of the double-doped phosphor tested under excitation at 275nm, 320nm, 353nm and 380nm. As shown in the figure, under the same excitation wavelength, by changing the Eu 3+ The doping concentration can be adjusted to achieve the color regulation of the fluorescent material from green to red.
[0045] The present invention adopts high temperature solid phase method to synthesize a series of Tb 3+ 、Eu 3+ Co-doped Y2MgAl4SiO 12 Fluorescent materials, the XRD diffraction patterns of the samples were tested and confirmed that Tb 3+ and Eu 3+ Ion doping into Y2MgAl4SiO 12No impurities are generated in the matrix. Co-doped fluorescent materials are obtained by adjusting the Eu 3+ The ion concentration can be adjusted from green to red. By comparing the fluorescence spectra, the present invention proves that Tb 3+ and Eu 3+ There is energy transfer between them. The results show that the fluorescent material has potential application value in the field of white light LED devices and other photoluminescent devices.
[0046] The above embodiments describe the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the scope of the principles of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of protection of the present invention.
Claims
1. A color-adjustable aluminosilicate fluorescent material, Features: The chemical formula of the fluorescent material is Y (2-x-y) MgAl 4 SiO 12 :xTb 3+ ,yEu 3+ , where x is 0.05-0.30, y is 0.01-0.35, and its crystal structure is garnet type, composed of Tb 3+ 、Eu 3+ Replace Y 3+ Position made.
2. The color-adjustable aluminosilicate fluorescent material according to claim 1, Features: The value of x is 0.
20.
3. A method for preparing the color-adjustable aluminosilicate fluorescent material according to claim 1, Features The specific steps are: 2 O 3 、MgO、Al 2 O 3 、SiO 2 , Tb 4 O 7 、Eu 2 O 3 As raw materials, according to the chemical formula Y (2-x-y) MgAl 4 SiO 12 :xTb 3+ ,yEu 3+ The raw materials are accurately weighed in a stoichiometric ratio; the weighed raw materials are mixed, ground, and dried to obtain a mixed raw material; the obtained mixed raw material is calcined at 1350-1550° C. for 3-10 h in an air atmosphere, cooled to room temperature, and ground again to obtain a color-adjustable aluminosilicate fluorescent material.
4. Use of the color-adjustable aluminosilicate fluorescent material according to claim 1 or 2 in the preparation of a photoluminescent device.
5. The use according to claim 4, Features: At the same excitation wavelength, by changing the Eu 3+ The doping concentration can achieve the regulation of the color of the fluorescent material from green to red, where the excitation wavelength is 275nm, 320nm, 353nm or 380nm.
6. Use of the color-adjustable aluminosilicate fluorescent material according to claim 1 or 2 in the preparation of white light LED devices.