Special cutting fluid for aluminum alloy and preparation method thereof
By using multi-walled carbon nanotubes and hyperbranched polyamide spherical structural particles as lubricating additives in special cutting fluid for aluminum alloys, the problem of insufficient lubrication performance of aluminum alloy cutting fluid in the prior art is solved, and efficient lubrication and corrosion protection are achieved Rust improves the efficiency and product life of aluminum alloy processing.
Patent Information
- Application Number
- CN202411155233.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The lubricating performance of existing aluminum alloy special cutting fluid is insufficient, making it difficult to meet the demand for efficient lubrication and corrosion-proof and rust during aluminum alloy processing.
The spherical structure particles with multi-walled carbon nanotubes as cores and hyperbranched polyamide as shells are used as lubricating additives to improve their dispersion and performance in the cutting fluid through specific synthesis methods, combining phosphate esters, polyether esters, By combining mechanical oil, anti-rust agent and other components, special cutting fluid for aluminum alloys with low friction, high extreme pressure and anti-wear, and good corrosion and rust resistance are prepared.
It significantly improves the lubricity, corrosion and rust resistance and cooling properties of special cutting fluid for aluminum alloys, enhances its application effect in aluminum alloy processing, extends service life and reduces energy consumption.
Smart Images

Figure BDA0005004770930000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal cutting fluids, and in particular to a special cutting fluid for aluminum alloys and a preparation method thereof. Background Art
[0002] Aluminum alloy materials have excellent physical properties, mechanical processing properties and corrosion resistance, and are widely used in mechanical processing fields such as automobiles and aviation. Due to its soft texture and high plasticity, its cutting efficiency is reduced. At present, the most widely used aluminum alloy cutting fluids on the market are cutting oils and emulsified oils, but most of them are only suitable for single alloy materials. Therefore, the research and development of multifunctional and efficient water-based aluminum alloy cutting fluids has attracted more and more attention.
[0003] Aluminum alloy cutting fluid is a semi-synthetic metal cutting fluid specially suitable for aluminum and aluminum alloy cutting. Compared with traditional saponified fluid, it is not easy to burn, non-irritating, non-combustible, non-odorous and non-polluting to the environment. It has good lubrication, cooling, cleaning and rust prevention effects. It can significantly improve the finish of workpiece processing, increase cutting volume, extend the anti-rust cycle, and increase service life. It can effectively improve production efficiency and reduce energy consumption and cutting fluid quota costs. It eliminates the adverse effects of anti-rust oil on subsequent processes and has great advantages in antioxidant capacity and lubrication performance among similar products. Aluminum alloy cutting fluid is widely used in hardware product cutting, turning, grinding and other processing, overcoming the shortcomings of insufficient lubrication of ordinary cutting fluid.
[0004] The prior art often adds di-n-butyl phosphite and tricresol phosphate as lubricants in the cutting fluid. For example, patent document CN109705970B discloses a method for preparing a fully synthetic aluminum alloy cutting fluid, which includes mixing phosphate ester and polyether ester in an alcohol amine compound; adding a rust inhibitor and oleic acid to mix; adding a coupling agent, a bactericide, a defoamer, and water to mix. The aluminum alloy cutting fluid prepared by this method has excellent corrosion resistance and cleaning performance, and can solve the problem of aluminum surface corrosion during aluminum alloy processing, but its lubrication performance is insufficient.
[0005] Therefore, according to the above-mentioned related technologies, it is urgent to develop a special cutting fluid for aluminum alloy and a preparation method thereof. Summary of the invention
[0006] In view of this, the purpose of the present invention is to provide a special aluminum alloy cutting fluid and a preparation method thereof, so as to alleviate the problem of insufficient lubricity of the special aluminum alloy cutting fluid in the prior art.
[0007] Based on the above purpose, the present invention provides a special cutting fluid for aluminum alloy and a preparation method thereof.
[0008] A special cutting fluid for aluminum alloys, comprising the following raw materials in parts by weight: 10-12 parts of machine oil, 0.5-1 parts of phosphate ester, 5-10 parts of polyether ester, 2-5 parts of triethanolamine, 1-3 parts of lubricating additive, 1-3 parts of defoaming agent, 1-3 parts of surfactant, 2-6 parts of rust inhibitor, and 40-45 parts of water;
[0009] The lubricating auxiliary agent is a spherical structure particle with multi-walled carbon nanotubes as core and hyperbranched polyamide as shell.
[0010] Preferably, the preparation method of the lubricating agent is as follows:
[0011] Step S1. Pour multi-walled carbon nanotubes into a beaker, add mixed acid, react for 30-40 minutes, filter and dry to obtain multi-walled carbon nanotubes with carboxyl groups on the surface;
[0012] Step S2. tris(3-aminophenyl)phosphine oxide, adipic acid, N-methylpyrrolidone, pyridine and triphenyl phosphite are mixed and stirred at room temperature until dissolved to obtain a mixed solution A;
[0013] Step S3. adding multi-walled carbon nanotubes with carboxyl groups on the surface to the mixed solution A, ultrasonically dispersing for 30-35 minutes, reacting at room temperature for 2-3 hours, then heating to 70-80°C for reaction for 2-3 hours, then heating to 120-130°C for reaction for 8-9 hours, and cooling to room temperature to obtain a mixed solution B;
[0014] Step S4. The mixed solution B is filtered under reduced pressure using a polyvinylidene fluoride microporous filter membrane with a pore size of 0.2 μm, washed twice with N-methylpyrrolidone and then twice with acetone, and vacuum dried at 100-120° C. for 10-12 h to obtain a lubricating agent.
[0015] Preferably, in step S1, the ratio of the multi-walled carbon nanotubes to the mixed acid is 0.1-0.5 g:10-15 mL, and the mixed acid is a mixture of formic acid and acetic acid in a volume ratio of 1:1.
[0016] Preferably, in step S2, the mass ratio of tris(3-aminophenyl)phosphine oxide and adipic acid is 1-1.5 g:0.5-1 g; the volume ratio of N-methylpyrrolidone, pyridine and triphenyl phosphite is 20-25:5-10:6-10; wherein the dosage ratio of tris(3-aminophenyl)phosphine oxide and N-methylpyrrolidone is 1-1.5 g:20-25 mL.
[0017] Preferably, the number average molecular weight of the hyperbranched polyamide is 6000-9000 g / mol.
[0018] Preferably, the multi-walled carbon nanotubes are selected from multi-walled carbon nanotubes with a particle size of 30-40 nm.
[0019] Preferably, the defoaming agent is any one of emulsified dimethyl silicone oil, polyoxypropylene glyceryl ether and polyoxypropylene polyoxyethylene glyceryl ether.
[0020] Preferably, the surfactant is any one of sorbitan monooleate, sucrose fatty acid ester and glycerol monocaprate.
[0021] Preferably, the rust inhibitor is any one of CHB, triethanolamine oleate and sodium petroleum sulfonate.
[0022] Preferably, the method for preparing the aluminum alloy special cutting fluid is characterized by comprising the following steps:
[0023] Step S1. Weigh the phosphate ester and the polyether ester, dissolve them in triethanolamine and stir them evenly to obtain a mixture C;
[0024] Step S2. adding the rust inhibitor and the machine oil to the mixture C while stirring to obtain a mixture D;
[0025] Step S3. Add a lubricating agent, a defoaming agent, a surfactant and water to the mixture D in sequence and stir evenly. Take a sample and observe until it is completely transparent. After natural cooling, package it to obtain a special cutting fluid for aluminum alloy.
[0026] Beneficial effects of the present invention:
[0027] The lubricating agent provided by the present invention has excellent properties such as low friction, high extreme pressure and anti-wear, good corrosion and rust resistance, etc. Structurally, the lubricating agent is a spherical structure particle with multi-walled carbon nanotubes as the core and hyperbranched polyamide as the shell, and its surface carries a large number of functional groups, which makes it more dispersed in the cutting fluid, thereby improving the lubricity of the special cutting fluid for aluminum alloys.
[0028] The core multi-walled carbon nanotubes of the present invention have excellent mechanical properties, excellent compressive resistance, ultra-high toughness, can reduce the friction coefficient and thus increase lubricity, and the multi-walled carbon nanotubes have good thermal conductivity, so that the aluminum alloy special cutting fluid has excellent cooling performance.
[0029] The grafted hyperbranched polyamide of the present invention greatly improves the agglomeration problem of multi-walled carbon nanotubes, thereby improving the lubrication performance of the special cutting fluid for aluminum alloys. At the same time, the nitrogen atoms thereon have lone pairs of electrons, and the metal has empty orbitals, and the two form a coordination bond, which makes it have an anti-corrosion and anti-rust effect. Therefore, the comprehensive performance of the special cutting fluid for aluminum alloys, such as lubricity, anti-corrosion and anti-rust, can be significantly improved, and the special cutting fluid has broad application prospects. DETAILED DESCRIPTION
[0030] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0031] The sources of some raw materials used in the present invention are as follows:
[0032] The mechanical oil was 26# mechanical oil, purchased from Wuhan Jiyesheng Chemical Co., Ltd.; the multi-walled carbon nanotubes were purchased from Suzhou Hengqiu Technology Co., Ltd.; the phosphate ester was purchased from Shanghai Yuanye Biotechnology Co., Ltd.; and the polyester ether was purchased from Dongguan Tianzhihong Plastic Chemical Co., Ltd.
[0033] Embodiment 1: A method for preparing a cutting fluid for aluminum alloy, comprising the following steps:
[0034] Step S1. Pour 0.1 g of multi-walled carbon nanotubes into a beaker, add 10 mL of mixed acid, react for 30 minutes, filter and dry to obtain multi-walled carbon nanotubes with carboxyl groups on the surface, wherein the mixed acid is formic acid: acetic acid in a volume ratio of 1:1, and the particle size of the multi-walled carbon nanotubes is 30 nm;
[0035] Step S2. 1 g of tris(3-aminophenyl)phosphine oxide, 0.5 g of adipic acid, 20 mL of N-methylpyrrolidone, 5 mL of pyridine and 6 mL of triphenyl phosphite were mixed and stirred at room temperature until dissolved to obtain a mixed solution A;
[0036] Step S3. adding multi-walled carbon nanotubes with carboxyl groups on the surface to the mixed solution A, ultrasonically dispersing for 30 minutes, reacting at room temperature for 2 hours, then heating to 70°C for 2 hours, then heating to 120°C for 8 hours, and cooling to room temperature to obtain a mixed solution B;
[0037] Step S4. The mixed solution B is filtered under reduced pressure using a polyvinylidene fluoride microporous filter membrane with a pore size of 0.2 μm, washed twice with N-methylpyrrolidone and then twice with acetone, and vacuum dried at 100° C. for 10 h to obtain a lubricating agent, wherein the number average molecular weight of the hyperbranched polyamide is 6000 g / mol.
[0038] Step S5. Weigh 0.5 mL of phosphate ester and 5 mL of polyether ester, dissolve them in 2 mL of triethanolamine and stir evenly to obtain a mixture C;
[0039] Step S6. Add 2 mL CHB and 10 mL 26# machine oil to the mixture C while stirring to obtain a mixture D;
[0040] Step S7. Add 1 g of lubricating agent, 1 mL of emulsified dimethyl silicone oil, 1 mL of sorbitan monooleate, and 40 mL of water to the mixture D in sequence and stir evenly. Take a sample and observe until it is completely transparent. After natural cooling, package it to obtain a special cutting fluid for aluminum alloy.
[0041] Embodiment 2: A method for preparing a cutting fluid for aluminum alloy, comprising the following steps:
[0042] Step S1. Pour 0.2 g of multi-walled carbon nanotubes into a beaker, add 11 mL of mixed acid, react for 31 minutes, filter and dry to obtain multi-walled carbon nanotubes with carboxyl groups on the surface, wherein the mixed acid is formic acid: acetic acid in a volume ratio of 1:1, and the particle size of the multi-walled carbon nanotubes is 32 nm;
[0043] Step S2. 1.2 g of tris(3-aminophenyl)phosphine oxide, 0.7 g of adipic acid, 22 mL of N-methylpyrrolidone, 6 mL of pyridine and 7 mL of triphenyl phosphite were mixed and stirred at room temperature until dissolved to obtain a mixed solution A;
[0044] Step S3. Add multi-walled carbon nanotubes with carboxyl groups on the surface to the mixed solution A, disperse by ultrasonic for 31 minutes, react at room temperature for 2.1 hours, then heat to 71°C for 2.1 hours, then heat to 121°C for 8.1 hours, and cool to room temperature to obtain a mixed solution B;
[0045] Step S4. The mixed solution B is filtered under reduced pressure using a polyvinylidene fluoride microporous filter membrane with a pore size of 0.2 μm, washed twice with N-methylpyrrolidone and then twice with acetone, and vacuum dried at 101° C. for 10.1 h to obtain a lubricating agent, wherein the number average molecular weight of the hyperbranched polyamide is 7000 g / mol.
[0046] Step S5. Weigh 0.6 mL of phosphate ester and 6 mL of polyether ester, dissolve them in 3 mL of triethanolamine and stir evenly to obtain a mixture C;
[0047] Step S6. 3 mL of triethanolamine oleate and 11 mL of 26# machine oil were added to the mixture C while stirring to obtain a mixture D;
[0048] Step S7. Add 2 g of lubricating agent, 2 mL of polyoxypropylene glycerol ether, 2 mL of sucrose fatty acid ester, and 41 mL of water to the mixture D in sequence and stir evenly. Take a sample and observe until it is completely transparent. After natural cooling, package it to obtain a special cutting fluid for aluminum alloy.
[0049] Embodiment 3: A method for preparing a cutting fluid for aluminum alloy, comprising the following steps:
[0050] Step S1. Pour 0.3 g of multi-walled carbon nanotubes into a beaker, add 13 mL of mixed acid, react for 36 minutes, filter and dry to obtain multi-walled carbon nanotubes with carboxyl groups on the surface, wherein the mixed acid is formic acid: acetic acid in a volume ratio of 1:1, and the particle size of the multi-walled carbon nanotubes is 36 nm;
[0051] Step S2. 1.3 g of tris(3-aminophenyl)phosphine oxide, 0.8 g of adipic acid, 24 mL of N-methylpyrrolidone, 8 mL of pyridine and 9 mL of triphenyl phosphite were mixed and stirred at room temperature until dissolved to obtain a mixed solution A;
[0052] Step S3. adding multi-walled carbon nanotubes with carboxyl groups on the surface to the mixed solution A, ultrasonically dispersing for 34 minutes, reacting at room temperature for 2.6 hours, then heating to 76°C for 2.6 hours, then heating to 126°C for 8.6 hours, and cooling to room temperature to obtain a mixed solution B;
[0053] Step S4. The mixed solution B is filtered under reduced pressure using a polyvinylidene fluoride microporous filter membrane with a pore size of 0.2 μm, washed twice with N-methylpyrrolidone and then twice with acetone, and vacuum dried at 116° C. for 11.6 h to obtain a lubricating agent, wherein the number average molecular weight of the hyperbranched polyamide is 8000 g / mol.
[0054] Step S5. Weigh 0.8 mL of phosphate ester and 8 mL of polyether ester, dissolve them in 4 mL of triethanolamine and stir evenly to obtain a mixture C;
[0055] Step S6. 5 mL of sodium petroleum sulfonate and 11.5 mL of 26# machine oil were added to the mixture C while stirring to obtain a mixture D;
[0056] Step S7. Add 2.5 g of lubricating agent, 2.5 mL of polyoxypropylene polyoxyethylene glycerol ether, 2.5 mL of glycerol monocaprate, and 44 mL of water to the mixture D in sequence and stir evenly. Take a sample and observe until it is completely transparent. After natural cooling, package it to obtain a special cutting fluid for aluminum alloy.
[0057] Embodiment 4: A method for preparing a cutting fluid for aluminum alloy, comprising the following steps:
[0058] Step S1. Pour 0.5 g of multi-walled carbon nanotubes into a beaker, add 15 mL of mixed acid, react for 40 minutes, filter and dry to obtain multi-walled carbon nanotubes with carboxyl groups on the surface, wherein the mixed acid is formic acid: acetic acid in a volume ratio of 1:1, and the particle size of the multi-walled carbon nanotubes is 40 nm;
[0059] Step S2. 1.5 g of tris(3-aminophenyl)phosphine oxide, 1 g of adipic acid, 25 mL of N-methylpyrrolidone, 10 mL of pyridine and 10 mL of triphenyl phosphite were mixed and stirred at room temperature until dissolved to obtain a mixed solution A;
[0060] Step S3. adding multi-walled carbon nanotubes with carboxyl groups on the surface to the mixed solution A, ultrasonically dispersing for 35 minutes, reacting at room temperature for 3 hours, then heating to 80°C for 3 hours, then heating to 130°C for 9 hours, and cooling to room temperature to obtain a mixed solution B;
[0061] Step S4. The mixed solution B is filtered under reduced pressure using a polyvinylidene fluoride microporous filter membrane with a pore size of 0.2 μm, washed twice with N-methylpyrrolidone and then twice with acetone, and vacuum dried at 120° C. for 12 h to obtain a lubricating agent, wherein the number average molecular weight of the hyperbranched polyamide is 9000 g / mol.
[0062] Step S5. Weigh 1 mL of phosphate ester and 10 mL of polyether ester, dissolve them in 5 mL of triethanolamine and stir evenly to obtain a mixture C;
[0063] Step S6. 6 mL of sodium petroleum sulfonate and 12 mL of 26# machine oil were added to the mixture C while stirring to obtain a mixture D;
[0064] Step S7. Add 3 g of lubricating agent, 3 mL of polyoxypropylene polyoxyethylene glycerol ether, 3 mL of glycerol monocaprate, and 45 mL of water to the mixture D in sequence and stir evenly. Take a sample and observe until it is completely transparent. After natural cooling, package it to obtain a special cutting fluid for aluminum alloy.
[0065] Comparative Example 1:
[0066] Compared with Example 1, this comparative example does not add a lubricating agent, and the remaining steps and parameters are the same, which will not be repeated here. Finally, a special cutting fluid for aluminum alloy is obtained.
[0067] Comparative Example 2:
[0068] Compared with Example 1, in this comparative example, multi-walled carbon nanotubes were not grafted with hyperbranched polyamide, and the remaining steps and parameters were the same, which will not be repeated in this comparative example. Finally, a special cutting fluid for aluminum alloy was obtained.
[0069] Comparative Example 3:
[0070] Compared with Example 1, this comparative example does not add multi-walled carbon nanotubes during the preparation of the special cutting fluid for aluminum alloys. The remaining steps and parameters are the same and will not be repeated in this comparative example. Finally, a special cutting fluid for aluminum alloys is obtained.
[0071] Comparative Example 4:
[0072] Compared with Example 1, this comparative example only changes the number average molecular weight of the hyperbranched polyamide from 6000 g / mol to 150000 g / mol, and the remaining steps and parameters are the same, which will not be repeated in this comparative example. Finally, a special cutting fluid for aluminum alloy is obtained.
[0073] Comparative Example 5:
[0074] Compared with Example 1, this comparative example only changes the number average molecular weight of the hyperbranched polyamide from 6000 g / mol to 2000 g / mol, and the remaining steps and parameters are the same, which will not be repeated in this comparative example. Finally, a special cutting fluid for aluminum alloy is obtained.
[0075] Performance Test:
[0076] Lubrication performance test:
[0077] Referring to the standard requirements of GB / T3142-1982, add the aluminum alloy special cutting fluid prepared in Example 1-Example 4 and Comparative Example 1-Comparative Example 5 to the special oil box for lubricity testing, and add it to 2 / 3 of the oil box. Fix the upper ball seat and the oil box to the four-ball machine, and adjust the friction coefficient to zero at the same time. The speed of the four-ball machine is set to 1200mp, the setting time is 30min, and the test force is set to 392N. Turn on the hydrostatic oil pump, press the oil cylinder up button, and after the four steel balls are in contact, fix the friction coefficient sensor. Set the test force to automatic correction and click to start the test. After the test is over, turn off the automatic correction and adjust it to manual correction; press the oil cylinder down button to turn off the hydrostatic oil pump. Copy the instrument test data and use the software to calculate the average value of the friction coefficient.
[0078] Extreme pressure test:
[0079] Referring to the standard requirements of GB / T3142-1982, add the emulsion to be tested to the special oil box for extreme pressure test. Same as the operation of lubricity test, fix and install the steel ball, oil box and upper ball seat, and add the emulsion to about 2 / 3 of the oil box. Adjust the friction coefficient to zero, set the speed of the four-ball machine to 1400±50rmp, set the time to 10s, and set the initial test force according to the characteristics of the cutting fluid. Turn on the hydrostatic oil pump and press the cylinder up button until the four steel balls are fully in contact. Click to start the test. After the test is over, press the cylinder down button to turn off the hydrostatic oil pump. Take out the oil box, pour out the cutting fluid, and wipe the surface of the steel ball with absorbent cotton. Measure the wear scar diameter under an optical microscope and calculate the average value. Refer to the corresponding table. If the wear spot diameter is much smaller than the corresponding value, continue to increase the test force. Repeat the above process until the average wear spot diameter under a certain test force is slightly lower than the corresponding value. This test force is the maximum non-seizure load P of this cutting fluid. B value;
[0080] Single piece anti-rust performance test:
[0081] Referring to the SHT0356-1992 standard, HT300 first-grade gray cast iron with a size of Ф35×20mm was selected as the test specimen, and the anti-rust specimen was treated. The specific operation is as follows: Use 400-mesh sandpaper to polish the specimen in one direction. After the surface is polished and smooth, use tweezers to hold the absorbent cotton and dip it in anhydrous ethanol and acetone to scrub it repeatedly, then use a hair dryer to dry it for standby use. Use a disposable straw to absorb 5% of the aluminum alloy special cutting fluid prepared in Example 1-Example 4 and Comparative Example 1-Comparative Example 5, and drop 5 drops of about 45mm on the surface of the treated specimen. A certain distance should be maintained between each drop, and no connection is allowed. Then place the specimen on a porcelain plate in a dryer with a diameter of Ф300mm. The bottom of the dryer is filled with distilled water accounting for about 13 volumes. Close the dryer cover tightly, place it in a constant temperature blast drying oven at 35±2℃ and let it stand for 48h. Take it out and observe whether there is rust on the specimen;
[0082] Lamination anti-rust performance test:
[0083] With reference to the ST0356-1992 standard, prepare the same iron sheet as that for the single-piece anti-rust test and 5% of the aluminum alloy-specific cutting fluid prepared in Example 1-Example 4 and Comparative Example 1-Comparative Example 5. Place the prepared test piece flat on the porcelain plate of the dryer, apply the cutting fluid to the polished side of the test piece, and then overlap the polished smooth side of another test piece on it. After the operation is completed, cover with a glass cover and place the dryer in a constant temperature forced air drying oven at 35±2°C and let it stand for 8 hours. After the test period expires, take out the two first-grade gray cast iron test pieces, separate them, and wipe the emulsified residual liquid on the contact surface of the two test pieces with anhydrous ethanol absorbent cotton, observe and determine whether they meet the standard requirements. If there is no rust and no obvious overprinting on the two overlapping surfaces within 1mm from the edge of the first-grade gray cast iron test piece, it can be judged as qualified;
[0084] Corrosion resistance test:
[0085] With reference to GB / T6144-2010 standard, 70 mL of the aluminum alloy cutting fluid prepared in Example 1 to Example 4 and Comparative Example 1 to Comparative Example 5 was poured into a stoppered test tube, and the test piece was placed in the test tube with tweezers, and the whole test piece was immersed in the test solution. The stopper was plugged, and the test piece was placed in a drying oven, and the test was continuously tested at a constant temperature of 55°C ± 2°C for 36 hours. The test piece was taken out and observed for corrosion and discoloration;
[0086] Defoaming test:
[0087] With reference to the SHT0356-1992 standard, a 100 mL stoppered measuring cylinder was prepared. The aluminum alloy-specific cutting fluid prepared in Examples 1 to 4 and Comparative Examples 1 to 5 was diluted 20 times with distilled water in the measuring cylinder, and 70 mL of the cutting fluid was measured and the stopper was tightly plugged. The stoppered measuring cylinder was vigorously shaken up and down for 1 min, and the up and down shaking distance was about 0.33 m. The shaking speed was roughly controlled at 100-120 times / min. After the shaking was completed, the emulsion was placed on a laboratory bench at a room temperature of 15-35°C and allowed to stand for 10 min. The foam in the measuring cylinder was observed to be eliminated. If the volume of the foam remaining on the liquid surface in the measuring cylinder did not exceed 2 mL, the defoaming performance of the cutting fluid was evaluated as qualified, otherwise it was unqualified.
[0088] Table 1 Summary of experimental data in Examples 1-4 and Comparative Examples 1-5
[0089]
[0090] Data Analysis:
[0091] It can be seen from Table 1 that when the lubricating additive in the aluminum alloy cutting fluid prepared by the present invention is used for cutting aluminum alloy, the comprehensive performance of the aluminum alloy cutting fluid can be significantly improved. This is because the lubricating additive provided by the present invention has a multi-walled carbon nanotube as a core and a hyperbranched polyamide as a shell, and its spherical structure has good dispersibility, a low friction coefficient, and excellent lubrication performance; the multi-walled carbon nanotube has excellent thermal conductivity, and can quickly cool the aluminum alloy cutting fluid; the grafted hyperbranched polyamide greatly improves the agglomeration problem of the carbon nanotube, and improves the lubrication performance of the aluminum alloy cutting fluid. At the same time, the nitrogen atoms thereon have lone pairs of electrons, and the metal has an empty orbital, and the two form a coordination bond, so that it has an anti-corrosion and anti-rust effect, so the lubricity, anti-corrosion and anti-rust and other comprehensive properties of the aluminum alloy cutting fluid can be significantly improved.
[0092] In Comparative Example 1, no lubricating agent is added. As can be seen from Table 1, friction increases, extreme pressure and wear resistance decreases, and anti-rust and anti-corrosion performance decreases. This may be because the spherical structure of the lubricating agent is lost, and the dispersibility of the cutting fluid decreases, resulting in a decrease in mechanical properties; in Comparative Example 2, no hyperbranched polyamide is grafted. As can be seen from Table 1, the lubrication performance, anti-corrosion and anti-rust performance decrease. This may be because the multi-walled carbon nanotubes lose the grafting of hyperbranched polyamide, making it easier to agglomerate, and the lubrication performance decreases. At the same time, the nitrogen atoms of the hyperbranched polyamide are lost and cannot form coordination bonds with the metal, resulting in a decrease in anti-corrosion and anti-rust performance; in Comparative Example 3, no multi-walled carbon nanotubes are added. As can be seen from Table 1, friction increases and extreme pressure and wear resistance decreases. This may be because the carbon atom hybrid structure of the multi-walled carbon nanotubes is sp 2structure, has excellent mechanical properties, and the carbon nanotubes have a high thermal conductivity, so that the cutting fluid can be cooled quickly; in comparative example 4, the number average molecular weight of the hyperbranched polyamide is changed from 6000g / mol to 150000g / mol. It can be seen from Table 1 that the friction increases, which may be because the molecular weight is too high, so that the modified multi-walled carbon nanotubes are no longer spherical structures, resulting in a decrease in their dispersibility and lubrication performance; in comparative example 4, the number average molecular weight of the hyperbranched polyamide is changed from 6000g / mol to 2000g / mol. It can be seen from Table 1 that the friction increases, which may be because the molecular weight is too small, resulting in part of the multi-walled carbon nanotubes being exposed, causing the carbon nanotubes to easily agglomerate and the lubrication performance to decrease.
[0093] It should be understood by those skilled in the art that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.
[0094] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A special cutting fluid for aluminum alloy, characterized in that: The invention is prepared from the following raw materials by weight: 10-12 parts of machine oil, 0.5-1 parts of phosphate ester, 5-10 parts of polyether ester, 2-5 parts of triethanolamine, 1-3 parts of lubricating agent, 1-3 parts of defoaming agent, 1-3 parts of surfactant, 2-6 parts of rust inhibitor and 40-45 parts of water; The lubricating auxiliary agent is a spherical structure particle with multi-walled carbon nanotubes as core and hyperbranched polyamide as shell.
2. The aluminum alloy cutting fluid according to claim 1, characterized in that: The lubricating agent preparation method is as follows: Step S1. Pour multi-walled carbon nanotubes into a beaker, add mixed acid, react for 30-40 minutes, filter and dry to obtain multi-walled carbon nanotubes with carboxyl groups on the surface; Step S2. tris(3-aminophenyl)phosphine oxide, adipic acid, N-methylpyrrolidone, pyridine and triphenyl phosphite are mixed and stirred at room temperature until dissolved to obtain a mixed solution A; Step S3. adding multi-walled carbon nanotubes with carboxyl groups on the surface to the mixed solution A, ultrasonically dispersing for 30-35 minutes, reacting at room temperature for 2-3 hours, then heating to 70-80°C for reaction for 2-3 hours, then heating to 120-130°C for reaction for 8-9 hours, and cooling to room temperature to obtain a mixed solution B; Step S4. The mixed solution B is filtered under reduced pressure using a polyvinylidene fluoride microporous filter membrane with a pore size of 0.2 μm, washed twice with N-methylpyrrolidone and then twice with acetone, and vacuum dried at 100-120° C. for 10-12 h to obtain a lubricating agent.
3. The aluminum alloy cutting fluid according to claim 2, characterized in that: In step S1, the amount ratio of the multi-walled carbon nanotubes to the mixed acid is 0.1-0.5 g:10-15 mL, and the mixed acid is obtained by mixing formic acid and acetic acid in a volume ratio of 1:
1.
4. The aluminum alloy cutting fluid according to claim 2, characterized in that: The mass ratio of tris(3-aminophenyl)phosphine oxide and adipic acid in step S2 is 1-1.5 g:0.5-1 g; the volume ratio of N-methylpyrrolidone, pyridine and triphenyl phosphite is 20-25:5-10:6-10; wherein the amount ratio of tris(3-aminophenyl)phosphine oxide and N-methylpyrrolidone is 1-1.5 g:20-25 mL.
5. The aluminum alloy cutting fluid according to claim 1, characterized in that: The number average molecular weight of the hyperbranched polyamide is 6000-9000 g / mol.
6. The aluminum alloy cutting fluid according to claim 1, characterized in that: The multi-walled carbon nanotubes are selected from multi-walled carbon nanotubes with a particle size of 30-40 nm.
7. The aluminum alloy cutting fluid according to claim 1, characterized in that: The defoaming agent is any one of emulsified dimethyl silicone oil, polyoxypropylene glyceryl ether and polyoxypropylene polyoxyethylene glyceryl ether.
8. The aluminum alloy cutting fluid according to claim 1, characterized in that: The surfactant is any one of sorbitan monooleate, sucrose fatty acid ester and glycerol monocaprate.
9. The aluminum alloy cutting fluid according to claim 1, characterized in that: The rust inhibitor is any one of CHB, triethanolamine oleate and sodium petroleum sulfonate.
10. The method for preparing a special aluminum alloy cutting fluid according to any one of claims 1 to 9, characterized in that: The following steps are involved: Step S1. Weigh the phosphate ester and the polyether ester, dissolve them in triethanolamine and stir them evenly to obtain a mixture C; Step S2. adding the rust inhibitor and the machine oil to the mixture C while stirring to obtain a mixture D; Step S3. Add a lubricating agent, a defoaming agent, a surfactant and water to the mixture D in sequence and stir evenly. Take a sample and observe until it is completely transparent. After natural cooling, package it to obtain a special cutting fluid for aluminum alloy.
Citation Information
Patent Citations
A fully synthetic cutting fluid for aluminum alloys and its preparation method
CN109705970B