Recovery treatment method of zinc anode slime
Through ball mill activation and multi-step separation treatment, the problem of difficulty in separation of zinc, manganese, lead and silver in zinc anode mud is solved, efficient recycling of zinc anode mud and effective utilization of manganese are achieved, and the electricity in the zinc electrostatic accumulation process is reduced. Consumption and production costs.
Patent Information
- Application Number
- CN202410958042.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-01
AI Technical Summary
The existing zinc anode mud recovery and treatment methods cannot effectively separate and enrich zinc, manganese, lead and silver, resulting in poor recycling effects.
After the zinc anode sludge is activated by ball mill, the zinc sulfate solution is leaching with sulfuric acid solution to obtain zinc sulfate solution and activated dezincification residue. Then, the acidic leaching is reduced in deionized water to separate the manganese sulfate solution and lead-silver leaching residue, and synthesis is carried out to obtain phosphoric acid by sodium phosphate synthesis Manganese products achieve efficient recycling of zinc, manganese, lead and silver.
It realizes efficient recycling of zinc, manganese, lead and silver in zinc anode mud, reduces the power consumption during zinc electrostatic accumulation, reduces production costs, and can make manganese series products.
Smart Images

Figure CN118880038A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of metallurgical technology, and in particular to a method for recovering and treating zinc anode mud. Background Art
[0002] At present, there are three main processes for recycling zinc anode mud. One is to return the zinc anode mud directly to the zinc leaching process as an oxidant; another is to directly feed the zinc anode mud into the lead system to recover lead and silver; and another is to separate the manganese from the lead and silver in the zinc anode mud by physical separation of the zinc anode mud, that is, flotation-gravity separation-magnetic separation or flotation-magnetic separation.
[0003] The first zinc anode mud treatment method can easily cause the manganese content in the electrolytic zinc system to increase, resulting in increased power consumption during zinc electrolysis, and low lead and silver recovery rates. The second zinc anode mud treatment method can effectively recover lead and silver, but due to the large amount of zinc anode mud and the high manganese content, the lead and silver recovery costs are high, and manganese and zinc cannot be effectively recycled. The third method cannot effectively recover the lead, silver, zinc, and manganese in the zinc anode mud due to the serious dispersion of silver in the concentrate and tailings. It can be seen that the recovery and treatment methods of the relevant technologies are unable to effectively separate and enrich zinc, manganese, lead, and silver in the zinc anode mud, and the recovery effect of the zinc anode mud is poor. Summary of the invention
[0004] In view of this, the present application provides a method for recovering and treating zinc anode mud, the main purpose of which is to solve the technical problem in the prior art that it is difficult to effectively separate and enrich zinc, manganese, lead and silver in zinc anode mud, resulting in poor recovery effect of zinc anode mud.
[0005] According to the first aspect of the present application, a method for recovering zinc anode mud is provided, the method comprising:
[0006] Ball milling activation treatment of zinc anode mud;
[0007] The zinc anode mud activated by ball milling is immersed in a sulfuric acid solution for leaching, and the activated zinc removal slag and zinc sulfate solution are obtained by filtering;
[0008] The zinc sulfate solution is transported to the zinc return system to recover zinc;
[0009] Adding activated dezincification slag and a reducing agent into deionized water for reduction acid leaching, filtering to obtain a manganese sulfate solution and lead-silver leaching slag;
[0010] The lead-silver leaching residue is transported to the lead return system to recover lead and silver;
[0011] The manganese phosphate product is synthesized by adding sodium phosphate into the manganese sulfate solution.
[0012] Optionally, the step of subjecting the zinc anode mud to ball milling activation treatment specifically comprises:
[0013] The zinc anode mud and the activator are added into the ball mill for ball milling activation treatment;
[0014] Obtaining the percentage value of zinc anode mud particles in the ball mill whose particle size is less than or equal to a preset particle size threshold;
[0015] When the data ratio is greater than or equal to the preset ratio, the ball milling activation operation is stopped.
[0016] Optionally, the step of adding the activated dezincification slag and the reducing agent into deionized water for reduction acid leaching, and filtering to obtain the manganese sulfate solution and the lead-silver leaching slag specifically comprises:
[0017] adding activated dezincification slag and a reducing agent into deionized water for reduction acid leaching to obtain a mixture;
[0018] The mixture is filtered through a filter press to obtain a manganese sulfate solution and lead-silver leaching residue.
[0019] Optionally, before adding the activated dezincification slag and the reducing agent into deionized water for reduction acid leaching and filtering to obtain the manganese sulfate solution and the lead-silver leaching slag, the process further comprises:
[0020] Obtain a preset amount of glucose;
[0021] Adding glucose into a sulfuric acid solution of a preset titer and stirring the solution to obtain a matured reducing agent;
[0022] The preset dosage of glucose is 1.05% to 1.3% of the theoretical dosage for reducing positive tetravalent manganese ions in activated dezincification slag to positive divalent manganese ions;
[0023] The preset titer range is 350g / L to 600g / L;
[0024] The temperature range for the aging operation is 45°C to 80°C;
[0025] The reaction time of the aging operation ranges from 1 hour to 5 hours.
[0026] Optionally, the step of adding sodium phosphate to the manganese sulfate solution to synthesize the manganese phosphate product specifically comprises:
[0027] adding a sulfuric acid solution dropwise into the manganese sulfate solution to control the pH value of the manganese sulfate solution to be within a first preset range;
[0028] adding sodium phosphate to a manganese sulfate solution and stirring the mixture, and dropping a sulfuric acid solution into the reaction solution to control the pH of the reaction solution to be within a second preset range, thereby forming a manganese phosphate precursor;
[0029] Slurry washing the manganese phosphate precursor according to a preset number of times;
[0030] The washed manganese phosphate precursor is spray dried to obtain a manganese phosphate product.
[0031] Optionally, before adding sodium phosphate to the manganese sulfate solution to synthesize the manganese phosphate product, the method further comprises:
[0032] adding ammonia water to the manganese sulfate solution to control the pH value of the manganese sulfate solution to be within a third preset range;
[0033] adding a purifying agent to the manganese sulfate solution for purification;
[0034] The manganese sulfate solution treated with a purifier is added to activated carbon for adsorption, and filtered to obtain a purified manganese sulfate solution.
[0035] Optionally, dilute sulfuric acid is used as the activator; in the ball milling activation operation, the titer range of the activator is 30 g / L to 50 g / L; and the weight ratio of zinc anode mud to the activator is 1:(1.5-3).
[0036] Optionally, in the reduction acid leaching operation on the activated dezincification slag, the initial titer of the sulfuric acid solution ranges from 90 g / L to 150 g / L; the liquid-to-solid ratio between deionized water, the activated dezincification slag and the reducing agent is (6-8):1; the temperature range of the reduction acid leaching operation is 90 degrees Celsius to 95 degrees Celsius; and the reaction time range of the reduction acid leaching operation is 5 hours to 8 hours.
[0037] Optionally, in the operation of synthesizing the manganese phosphate precursor, the amount of sodium phosphate added is 1.05% to 1.15% of the theoretical amount of manganese phosphate precipitate generated; the reaction temperature range of the operation of synthesizing the manganese phosphate precursor is 40 degrees Celsius to 50 degrees Celsius; the reaction time range of the operation of synthesizing the manganese phosphate precursor is 5 hours to 8 hours.
[0038] Optionally, the temperature range of the spray drying operation is 300 degrees Celsius to 350 degrees Celsius; the rotation speed range of the spray disk of the spray drying operation is 43 Hz to 48 Hz.
[0039] By means of the above technical scheme, the present application provides a method for recycling and treating zinc anode mud. Specifically, the zinc anode mud activated by ball milling is leached with sulfuric acid to obtain activated dezincification slag and zinc sulfate solution, so that zinc can enter the solution in the form of zinc sulfate, and other metals remain in the leached slag in solid form. Through solid-liquid separation, zinc is separated from manganese, lead and silver, thereby realizing the recycling of zinc. Thereafter, the activated dezincification slag is subjected to reduction acid leaching, and the solid manganese dioxide in the zinc anode mud is reduced to manganese sulfate and enters the solution through water leaching, while lead and silver remain in the leached slag in solid form. Through solid-liquid separation, manganese and silver and lead are separated, thereby realizing the enrichment and recovery of lead and silver. Finally, the purified manganese sulfate solution is synthesized and dried to obtain a manganese phosphate product, thereby realizing the recycling of manganese. Through the above method, efficient recovery of zinc, manganese, lead and silver in zinc anode mud is achieved. This method not only has a short process flow and easy-to-obtain low-value raw materials, but also allows manganese to be removed from the zinc system, reducing the impact of excessive manganese electroplating on power consumption, thereby reducing production costs in the zinc production process, and can be made into a series of manganese products.
[0040] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present application. Also, the same reference symbols are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:
[0042] Figure 1 A schematic flow chart of a method for recycling zinc anode mud provided in an embodiment of the present application is shown;
[0043] Figure 2 A schematic flow chart of another method for recovering and treating zinc anode mud provided in an embodiment of the present application is shown. DETAILED DESCRIPTION
[0044] The exemplary embodiments of the present application will be described in more detail below with reference to the accompanying drawings. Although the exemplary embodiments of the present application are shown in the accompanying drawings, it should be understood that the present application can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present application and to fully convey the scope of the present application to those skilled in the art.
[0045] The present application embodiment provides a method for recycling zinc anode mud, such as Figure 1 As shown, the method includes:
[0046] S101, performing ball milling activation treatment on zinc anode mud.
[0047] The method for recycling zinc anode mud provided in the embodiment of the present application is mainly used in the recycling and processing scenario of zinc anode mud. Among them, zinc anode mud is manganese ions discharged on the anode during zinc electrolysis, precipitated and oxidized to form acid-insoluble manganese dioxide, which falls into the electrolytic cell. At the same time, the lead-silver anode plate falls into the electrolytic cell in the form of precipitate due to electrochemical and chloride ion corrosion during the electrolysis process, and is mixed with the manganese dioxide that falls into the electrolytic cell to form slag mud. The anode mud is rich in manganese, lead, silver and zinc, and has a very high recovery value.
[0048] First, prepare zinc anode mud and activator, mix them evenly according to the required ratio, and the activator can promote the dissolution of zinc in zinc anode mud. After that, put the mixed zinc anode mud and activator into a ball mill. A ball mill is a grinding device with grinding balls inside, which grinds materials through the collision and friction of the balls. During the ball milling process, the materials are ground into finer particles, which helps the activator to react more fully with the zinc anode mud and improve the subsequent leaching efficiency.
[0049] In an embodiment of the present application, optionally, in step S101, the step of ball milling activation treatment of zinc anode mud specifically includes: adding zinc anode mud and an activator into a ball mill for ball milling activation treatment; obtaining the number percentage of zinc anode mud particles in the ball mill whose particle size is less than or equal to a preset particle size threshold; when the data percentage is greater than or equal to the preset percentage, stopping the ball milling activation operation.
[0050] In this embodiment, zinc anode mud and activator are added to a ball mill. The ball mill is started, and the materials are mixed and activated in the mill through mechanical action. During the ball milling process, the materials are impacted and rubbed by the high-speed moving steel balls, thereby achieving the effects of crushing, mixing and activation.
[0051] While ball milling, the particle size of the powder needs to be controlled. It is usually required that 80% of the particle size is less than or equal to 325 mesh (i.e., the aperture size of a 325 mesh screen) to ensure that the uniformity and fineness of the obtained powder meet the standards. Therefore, during the ball milling process, a certain amount of zinc anode mud particles are taken out regularly for particle size analysis. If the percentage of the number of zinc anode mud particles taken out with a particle size less than or equal to the preset particle size threshold reaches the preset percentage value, it means that the ideal particle size distribution has been achieved at this time, and the ball milling activation operation can be stopped; if the number of zinc anode mud particles taken out with a particle size less than or equal to the preset particle size threshold does not reach the preset percentage value, ball milling needs to be continued until the ideal particle size distribution is achieved.
[0052] Optionally, the preset particle size threshold may be 325 meshes; and the preset proportion value may be 80%.
[0053] Optionally, the activator can be selected as dilute sulfuric acid; in the ball milling activation operation, the titer range of the activator is 30g / L to 50g / L; the weight ratio of zinc anode mud to the activator is 1:(1.5-3).
[0054] By the above method, the particle size is controlled to ensure that the obtained powder particles are uniform in size, avoid incomplete or uneven reaction caused by large particles, and ensure the stability of subsequent processes and product quality.
[0055] S102, immersing the zinc anode mud after ball milling activation in a sulfuric acid solution for leaching, and filtering to obtain zinc leaching residue and zinc sulfate solution.
[0056] In this step, the zinc anode mud powder that has been activated by ball milling is immersed in a sulfuric acid solution. The sulfuric acid reacts with the activated zinc anode mud to dissolve the zinc therein and form a zinc sulfate solution. At the same time, some undissolved slag or impurities will be produced during the dissolution process, which are the activated dezincification slag. The activated dezincification slag after leaching is separated from the zinc sulfate solution by a solid-liquid separation device (such as a filter).
[0057] Optionally, in the leaching and dezincification operation of zinc anode mud, the dezincification temperature ranges from 80 degrees Celsius to 85 degrees Celsius; and the dezincification reaction time is 1.5 hours to 3 hours.
[0058] In actual application scenarios, the milled and activated zinc anode mud powder is pumped into a leaching tank, which is a container used for chemical leaching process. In the leaching tank, sulfuric acid solution is added to complete the leaching process.
[0059] S103, transporting the zinc sulfate solution to a zinc return system to recover zinc.
[0060] In this step, the zinc return system is a process system for treating zinc-containing waste or solution to recover and purify zinc metal therefrom. The zinc sulfate solution containing zinc ions is transported to the zinc return system to further recover and purify the zinc metal therein.
[0061] In actual application scenarios, the zinc sulfate solution is introduced into the zinc return system. The system separates impurities and other metals in the solution through a series of chemical treatment steps (such as precipitation, filtration, dissolution, electrolysis, etc.), thereby purifying the zinc-containing substances. After treatment, the system further processes the obtained zinc-containing solution or solid to extract and recover the zinc. It usually includes electrolysis process (reducing zinc to metallic zinc), extraction process (separating zinc ions with an extractant), deposition process (depositing zinc on an electrode) and other methods to finally obtain metallic zinc with higher purity.
[0062] Through the above method, zinc resources can be effectively recovered and reused from discarded zinc anode mud, saving raw materials and reducing environmental impact.
[0063] S104, adding the activated dezincification slag and the reducing agent into deionized water for reduction acid leaching, and filtering to obtain the manganese sulfate solution and the lead-silver leaching slag.
[0064] In this step, activated dezincification slag and a reducing agent are added to deionized water. The activated dezincification slag contains metals such as manganese, lead, and silver, and the role of the reducing agent is to reduce high-valent metal ions to low-valent states, which is conducive to the dissolution and extraction of metals. In addition, deionized water can provide a high-purity reaction environment to avoid the influence of impurities on the reaction. Under acidic conditions, a reducing agent is used to promote the transfer of metal ions in the activated dezincification slag from the solid phase to the liquid phase to form a sulfate solution. After leaching is completed, the solution in the mixture is separated from the residue by filtering. Soluble metal sulfate (i.e., manganese sulfate) will remain in the solution, while metals such as lead and silver that are difficult to dissolve in acid will be separated in the form of residues, and lead-silver leaching residues will be formed after high enrichment.
[0065] In an embodiment of the present application, optionally, in step S104, the step of adding the activated dezincification slag and the reducing agent to deionized water for reduction acid leaching, and filtering to obtain a manganese sulfate solution and lead-silver leaching slag specifically includes: adding the activated dezincification slag and the reducing agent to deionized water for reduction acid leaching to obtain a mixture; and filtering the mixture by a filter press to obtain a manganese sulfate solution and lead-silver leaching slag.
[0066] In this embodiment, activated dezincification slag and reducing agent are prepared to ensure that their ratio meets the process requirements. A suitable reaction tank is selected to ensure that it can accommodate the raw materials and the reaction solution, and has a stirring function to ensure that the reaction is carried out evenly. Thereafter, the activated dezincification slag and the reducing agent are added to the reaction tank. The activated dezincification slag contains manganese, lead, and silver, and the reducing agent is conducive to dissolving these metals. An appropriate amount of deionized water is added to the reaction tank, and stirring is started to ensure that the dissolution and mixing are uniform. After the reaction is completed, a mixture is obtained. The mixture is filtered through a filter press to separate the solid and the liquid, thereby obtaining a manganese-containing sulfuric acid solution leached from the activated dezincification slag and a lead-silver leached slag after high enrichment.
[0067] Optionally, in the reduction acid leaching operation on the activated dezincification slag, the initial titer of the sulfuric acid solution ranges from 90 g / L to 150 g / L; the liquid-solid ratio between deionized water, the activated dezincification slag and the reducing agent is (6-8):1; the temperature range of the reduction acid leaching operation is 90 degrees Celsius to 95 degrees Celsius; and the reaction time of the reduction acid leaching operation is 5 hours to 8 hours.
[0068] In an embodiment of the present application, optionally, in order to improve the reactivity of the reducing agent with chemical substances in other solutions, the activated dezincification slag and the reducing agent are added to deionized water for reduction acid leaching, and before filtering to obtain the manganese sulfate solution and the lead-silver leaching slag, the method further includes: obtaining a preset amount of glucose; adding the glucose to a sulfuric acid solution of a preset titer and stirring to obtain a matured reducing agent.
[0069] In this embodiment, glucose has the advantages of reliable source, fast reaction, low cost, no interfering elements, etc., and strong reducing property, so that manganese can be completely leached, and the recovery rate of manganese products is effectively improved. Therefore, glucose is selected as the reducing agent, and the reducing agent glucose is obtained according to the required preset dosage (preset dosage), and the glucose is added to the sulfuric acid solution of the preset titer for continuous stirring and maturation, so that the glucose and the sulfuric acid solution fully react to obtain the matured reducing agent.
[0070] Optionally, the preset dosage of the reducing agent glucose is 1.05% to 1.3% of the theoretical dosage for reducing the positive tetravalent manganese ions in the activated dezincification slag to positive divalent manganese ions. By using a slightly excessive amount of glucose, it can be ensured that the positive tetravalent manganese ions (Mn 4+ ) is completely reduced to positive divalent manganese atoms (Mn 2+ ), avoid incomplete reaction due to insufficient reducing agent and ensure the stability and reliability of the reaction.
[0071] Optionally, the preset titer of the sulfuric acid solution ranges from 350 g / L to 600 g / L; the temperature range of the aging operation ranges from 45 degrees Celsius to 80 degrees Celsius; and the reaction time range of the aging operation ranges from 1 hour to 5 hours.
[0072] In actual application scenarios, glucose, a carbon source for synthesizing lithium iron phosphate (LiFeMnPO4 / C) and lithium manganese oxide (LiMnPO4 / C) composites, is used as a reducing agent to change the morphology and particle size of the manganese phosphate precursor. This manganese phosphate product is used as one of the raw materials for synthesizing LiFeMnPO4 / C and LiMnPO4 / C composites, which can improve the electrical properties of the composites.
[0073] In the above manner, glucose is used as a reducing agent, and the reducing agent glucose is matured in advance, so that the reducing agent has better solubility and stability, and the reactivity of the reducing agent with other chemical substances in the solution is improved, thereby enhancing the reaction efficiency and accelerating the reaction rate.
[0074] S105, transporting the lead-silver leaching residue to the lead return system to recover lead and silver.
[0075] In this step, the lead return system is a process system specially used to process lead powder. The highly enriched lead-silver leaching residue is transported to the lead return system, where it is smelted and then refined to purify lead and silver, thus achieving efficient recovery and treatment of lead and silver.
[0076] S106. Adding sodium phosphate to the manganese sulfate solution to synthesize a manganese phosphate product.
[0077] In this step, sodium phosphate is added to the manganese sulfate solution as a synthesizing agent to convert manganese sulfate into manganese phosphate, which is then dried to obtain a powdered manganese phosphate product to achieve manganese recovery. The manganese phosphate product can be collected for further industrial application.
[0078] In the embodiment of the present application, optionally, in step S106, the step of adding sodium phosphate to the manganese sulfate solution to synthesize the manganese phosphate product specifically includes: dripping sulfuric acid solution into the manganese sulfate solution to control the pH of the manganese sulfate solution within a first preset range; adding sodium phosphate to the manganese sulfate solution for stirring, and dripping sulfuric acid solution into the reaction solution to control the pH of the reaction solution within a second preset range to form a manganese phosphate precursor; slurrying the manganese phosphate precursor according to a preset number of times; and spray drying the washed manganese phosphate precursor to obtain a manganese phosphate product.
[0079] In this embodiment, in order to ensure the stability of the subsequent reaction, an appropriate amount of sulfuric acid solution is first dripped into the manganese sulfate solution to adjust the pH value of the manganese sulfate solution. Thereafter, the synthetic agent sodium phosphate is gradually added to the manganese sulfate solution and stirred continuously to ensure that it is dissolved and evenly distributed in the liquid. Sodium phosphate can react with manganese ions in the solution to form a precipitate. During or after the addition of sodium phosphate, sulfuric acid solution is dripped into the reaction solution to adjust the pH value of the solution to promote the reaction. With the addition of sodium phosphate and the adjustment of the pH value, the precursor of manganese phosphate will gradually precipitate out. After the reaction is completed, the manganese phosphate precursor is repeatedly washed to remove the by-products and unreacted raw materials and impurities generated in the reaction to ensure the purity and stability of the final product. The washed manganese phosphate precursor is treated by spray drying technology, and the solution is converted into a powdered spherical manganese phosphate product by high-speed spraying, thereby realizing manganese recovery.
[0080] In actual application scenarios, the manganese phosphate slurry is quickly dried by spray drying equipment, and the manganese phosphate is granulated into spheres at the same time; after air flow crushing, the product particle size distribution is uniform, D50 = 1.0μm-1.8μm, and the electrical properties of LiFeMnPO4 / C and LiMnPO4 / C composites can also be improved.
[0081] Optionally, in the operation of synthesizing the manganese phosphate precursor, the amount of sodium phosphate added is 1.05% to 1.15% of the theoretical amount of manganese phosphate precipitation; the reaction temperature range of the operation of synthesizing the manganese phosphate precursor is 40 degrees Celsius to 50 degrees Celsius; the reaction time range of the operation of synthesizing the manganese phosphate precursor is 5 hours to 8 hours. In addition, the mass concentration of manganese in the solution is 45% to 55%; the first preset range is pH = 1.5-3.0; the second preset range is pH = 2.5-4.0.
[0082] Optionally, the temperature range of the spray drying operation is 300 degrees Celsius to 350 degrees Celsius; the rotation speed range of the spray disk of the spray drying operation is 43 Hz to 48 Hz.
[0083] In the embodiment of the present application, optionally, in order to improve the quality of the manganese phosphate product, before adding sodium phosphate to the manganese sulfate solution to synthesize the manganese phosphate product, it also includes: dripping ammonia water into the manganese sulfate solution to control the pH of the manganese sulfate solution within a third preset range; adding a purifier to the manganese sulfate solution for purification; adding the manganese sulfate solution treated with the purifier to activated carbon for adsorption, and filtering to obtain a purified manganese sulfate solution.
[0084] In this embodiment, the pH value of manganese sulfate solution is first adjusted to 7-7.5 using ammonia water. Thereafter, manganese sulfate solution is added with a purifying agent, which reacts with the impurities in the manganese sulfate solution to form a precipitate or other removable products. The solution treated with the purifying agent is added to activated carbon, which has a strong adsorption capacity and can effectively remove organic matter and some inorganic substances in the solution, further improving the purity of manganese sulfate solution. After the reaction is completed, activated carbon and precipitate are separated by filtration to obtain a purified solution (manganese sulfate solution) and purified slag (unreacted purifying agent, activated carbon adsorbed substances and other solid impurities).
[0085] Optionally, the purifier may be ammonium fluoride (NH4F) or ammonium sulfide ((NH4)2S). The pH value of the manganese sulfate solution is adjusted to 7-7.5 (third preset range) using aqueous ammonia; the amount of the purifier added is 1.25-1.48 times the theoretical amount; the temperature of the purification operation is room temperature; and the reaction time of the purification operation is 90 minutes to 120 minutes.
[0086] In the above manner, by adjusting the pH value of the manganese sulfate solution, adding a purifier, and performing adsorption and filtering operations on activated carbon, the purity of the manganese sulfate leaching solution is effectively improved, which is suitable for subsequent extraction and application requirements.
[0087] The recovery and treatment method of zinc anode mud provided in the embodiment of the present application uses sulfuric acid to leach the zinc anode mud after ball milling activation to obtain activated dezincification slag and zinc sulfate solution, which can make zinc enter the solution in the form of zinc sulfate, and other metals remain in the leached slag in solid form. Through solid-liquid separation, zinc is separated from manganese, lead and silver, thereby realizing the recovery and utilization of zinc. Thereafter, the activated dezincification slag is subjected to reduction acid leaching, and the solid manganese dioxide in the zinc anode mud is reduced to manganese sulfate and enters the solution through water leaching, and lead and silver are enriched in the leached slag in solid form. Through solid-liquid separation, manganese and silver and lead are separated, thereby realizing the enrichment and recovery of lead and silver. Finally, the purified manganese sulfate solution is synthesized and dried to obtain a manganese phosphate product, thereby realizing the recovery and utilization of manganese. Through the above method, efficient recovery of zinc, manganese, lead and silver in zinc anode mud is achieved. This method not only has a short process flow and easy-to-obtain low-value raw materials, but also allows manganese to be removed from the zinc system, reducing the impact of excessive manganese electroplating on power consumption, thereby reducing production costs in the zinc production process, and can be made into a series of manganese products.
[0088] The present application further provides another method for recycling zinc anode mud as a refinement and expansion of the above-mentioned specific implementation methods, in order to fully illustrate the specific implementation process of the present embodiment, such as Figure 2 The figure shows a schematic flow chart of a method for recovering zinc anode mud, which includes the following five steps:
[0089] Step A: Activated dezincification: zinc anode mud and activator are added into ball mill according to proportion and then ball milled for activation. The ball milling particle size is controlled to be 80% ≤ 325 mesh. After passing the test, it is pumped into the leaching tank for leaching and dezincification to obtain activated dezincification slag and zinc sulfate solution.
[0090] Among them, the activator for ball milling zinc anode mud is dilute sulfuric acid (H2SO4) with a titer of 30g / L-50g / L, the weight ratio of zinc anode mud to activator is 1:(1.5-3), the dezincification temperature is 80℃-85℃, and the time is 1.5h-3.0h.
[0091] Step B: reducing agent maturation: Add the required reducing agent glucose into a sulfuric acid solution with a titer of 350g / L-600g / L and stir and mature it continuously at a maturation temperature of 45°C-80°C for 1h-5h to obtain a matured reducing agent.
[0092] The amount of reducing agent glucose is to activate the Mn in the dezincification slag. 4+ Reduction to Mn 2+ 1.05-1.30 times of the theoretical dosage.
[0093] Step C: Reduction acid leaching: The activated dezincification slag obtained in step A and the mature reducing agent obtained in step B are added to a reaction tank which is added with appropriate water and continuously stirred for reduction acid leaching. After the reaction is completed, the manganese sulfate solution and the highly enriched lead and silver leaching slag are obtained by filter pressing.
[0094] The initial titer of sulfuric acid is 90 g / L-150 g / L, the liquid-to-solid weight ratio is (6-8):1, the temperature is 90° C.-95° C., and the time is 5 hours-8 hours.
[0095] Step D: Purification and deoiling: The manganese sulfate leaching solution obtained in step C is purified by adding a purifier NH4F or (NH4)2S, and then adsorbed with activated carbon. After the reaction is completed, the purified liquid and purified residue are obtained by filtering.
[0096] The pH value of the manganese sulfate leaching solution is adjusted to 7-7.5 with ammonia water, and the amount of metal precipitants ammonium sulfide and ammonium fluoride added is 1.25-1.48 times of the required theoretical amount; the temperature is room temperature, and the time is 90min-120min.
[0097] Step E: synthesis of manganese phosphate: sodium phosphate as a synthesis agent is added to the purified solution obtained in step D, and the pH value of the solution is adjusted to obtain a manganese phosphate precursor. The manganese phosphate precursor is washed three times and then spray-dried to obtain a manganese phosphate product.
[0098] The pH value of the purified solution is first adjusted to 1.5-3.0 with sulfuric acid, and sulfuric acid is used to ensure that the pH value during the process and at the end point is 2.5-4.0. The amount of sodium phosphate added is 1.05-1.15 times the theoretical amount of manganese phosphate precipitation, the mass concentration of manganese in the solution is 45%-55%, and the reaction temperature is controlled to be 40°C-50°C and the reaction time is 5h-8h under continuous stirring.
[0099] Furthermore, in step E, the manganese phosphate precursor after deionized water slurry washing and impurity removal is spray dried, the spray drying temperature is 300° C.-350° C., and the rotation speed of the spray turntable is 43 Hz-48 Hz.
[0100] Furthermore, in step E, the manganese phosphate dried at high temperature is powdered by air flow crushing, and the particle size distribution of the product after air flow crushing is uniform, and the medium particle size D50 is 1.0 μm-1.8 μm.
[0101] By activating and dezincifying the zinc anode mud, the water-soluble zinc and acid-soluble zinc in the zinc anode mud are removed to the greatest extent possible, and the zinc recovery rate is high; by efficiently purifying and de-oiling, the organic phase in the reduction leaching solution is removed while removing impurities such as lead (Pb), zinc (Zn), calcium (Ca), and magnesium (Mg), so as to obtain a high-quality high-purity manganese phosphate product for preparing lithium manganese iron phosphate or lithium manganese phosphate raw materials, in which the manganese (Mn) content is greater than 32%, the phosphorus (P) content is 18-19%, the impurity sulfur (S) and sodium (Na) content are less than 0.03% and 0.01% respectively, and the concentration of impurities such as Pb, Zn, Ca, and Mg is very low, usually at the level of one part per million (i.e., ppm level). At the same time, the recovery rates of manganese and zinc in the zinc anode mud exceed 97% and 96% respectively, and more than 98.5% of lead and silver are enriched in the lead-silver leaching slag.
[0102] In order to make the technical problems, technical solutions and beneficial effects solved by the present application clearer, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. The raw materials used in the embodiments and comparative examples are all commercially available.
[0103] Example 1
[0104] High-quality and high-purity manganese phosphate, a raw material of lithium manganese iron phosphate, is prepared using zinc anode mud with the composition of Zn: 2.15wt%, Mn: 38.16wt%, Pb: 14.28wt%, and Ag: 0.0541wt%, and the remaining valuable metals are comprehensively recovered.
[0105] Step A, zinc anode mud and 30g / L dilute sulfuric acid activator are added into a ball mill at a ratio of 1:1.5, and then ball milled for activation, with a ball milling particle size of 80% and a particle size of 350 meshes. After passing the test, the mixture is pumped into a leaching tank for leaching and dezincification, with a dezincification temperature of 85°C and a time of 1.5h, to obtain activated dezincification slag and zinc sulfate solution;
[0106] Step B: Activate the Mn in the dezincification slag 4+ Reduction to Mn 2+ The reducing agent glucose which is 1.30 times of the theoretical amount is added into a sulfuric acid solution with a titer of 350 g / L, and the mixture is continuously stirred and aged at a temperature of 80° C. for 1 h to obtain an aged reducing agent;
[0107] Step C, adding the activated dezincification slag obtained in step A and the mature reducing agent obtained in step B into a reaction tank added with appropriate water and continuously stirred for reduction acid leaching, wherein the initial sulfuric acid titer in the solution is 90 g / L, the liquid-solid weight ratio is 8:1, the temperature is 95° C., the time is 5 hours, and after the reaction is completed, filter pressing is performed to obtain a manganese sulfate solution and a highly enriched lead and silver leaching slag;
[0108] Step D, first adjust the pH value of the manganese sulfate leaching solution obtained in step C to 7 with ammonia water, add 1.48 times the theoretical amount of the required purifier NH4F or (NH4)2S for purification, the temperature is room temperature, the time is 90 minutes, and then use activated carbon for adsorption and deoiling. After the reaction is completed, filter to obtain the purified liquid and purified residue;
[0109] Step E: first adjust the pH value of the purified liquid obtained in step D to 1.5 with sulfuric acid, slowly add manganese to complete the formation of 1.15 times the theoretical amount of manganese phosphate precipitation and a mass concentration of 55% synthetic agent sodium phosphate, use sulfuric acid to ensure that the process and end point pH value is 2.5, control the reaction temperature to 40°C, and the reaction time is 8h to obtain a manganese phosphate precursor. The manganese phosphate precursor after slurry washing 3 times is spray dried at a spray drying temperature of 300°C and a spray turntable speed of 48Hz. After air flow crushing, a manganese phosphate product with a medium particle size of D50=1.0μm is obtained.
[0110] Through the comprehensive recovery of the zinc anode mud samples, the recovery rates of manganese and zinc in the zinc anode mud were 98.5% and 99.2% respectively, and 99.5% of lead and silver were enriched in the lead-silver leaching slag; at the same time, the Mn and P contents in the prepared product were 32.52% and 18.19% respectively, and the impurity S and Na contents were 0.01% and 0.006% respectively. The impurities such as Pb, Zn, Ca, and Mg were at the ppm level. The manganese iron phosphate lithium positive electrode material prepared with this product as raw material has excellent physical and chemical properties, and the 1C discharge specific capacity is 150.47mAh / g.
[0111] Example 2
[0112] High-quality and high-purity manganese phosphate, a raw material of lithium manganese iron phosphate, is prepared using zinc anode mud with the composition of Zn: 1.89wt%, Mn: 32.81wt%, Pb: 11.94wt%, and Ag: 0.0489wt%, and the remaining valuable metals are comprehensively recovered.
[0113] Step A, zinc anode mud and 50g / L dilute sulfuric acid activator are added into a ball mill at a ratio of 1:3, and then ball milled and activated, the ball milling particle size is controlled to be 80% particle size = 338 mesh, and after passing the test, it is pumped into a leaching tank for leaching and dezincification, the dezincification temperature is 80°C, the time is 3.0h, and activated dezincification slag and zinc sulfate solution are obtained;
[0114] Step B: Activate the Mn in the dezincification slag 4+ Reduction to Mn 2+ The reducing agent glucose which is 1.05 times of the theoretical amount is added into a sulfuric acid solution with a titer of 600 g / L, and the mixture is continuously stirred and aged at a temperature of 45° C. for 5 h to obtain an aged reducing agent;
[0115] Step C, adding the activated dezincification slag obtained in step A and the mature reducing agent obtained in step B into a reaction tank added with appropriate water and continuously stirred for reduction acid leaching, wherein the initial sulfuric acid titer in the solution is 150 g / L, the liquid-solid weight ratio is 6:1, the temperature is 90° C., the time is 8 hours, and after the reaction is completed, filter pressing is performed to obtain a manganese sulfate solution and a highly enriched lead and silver leaching slag;
[0116] Step D, first adjust the pH value of the manganese sulfate leaching solution obtained in step C to 7.5 with ammonia water, add 1.25 times the theoretical amount of the required purifier NH4F or (NH4)2S for purification, the temperature is room temperature, the time is 120 minutes, and then use activated carbon for adsorption and deoiling. After the reaction is completed, filter to obtain the purified liquid and purified residue;
[0117] Step E: first adjust the pH value of the purified liquid obtained in step D to 3.0 with sulfuric acid, slowly add manganese to complete the formation of 1.05 times the theoretical amount of manganese phosphate precipitation and a mass concentration of 45% synthetic agent sodium phosphate, use sulfuric acid to ensure that the process and end point pH value is 4.0, control the reaction temperature to 50°C, and the reaction time is 5h to obtain a manganese phosphate precursor. The manganese phosphate precursor after slurry washing 3 times is spray dried at a spray drying temperature of 350°C and a spray turntable speed of 43Hz. After air flow crushing, a manganese phosphate product with a medium particle size of D50=1.8μm is obtained.
[0118] Through the comprehensive recovery of the zinc anode mud samples, the recovery rates of manganese and zinc in the zinc anode mud were 99.3% and 99.1% respectively, and 99.4% of lead and silver were enriched in the lead-silver leaching slag; at the same time, the Mn and P contents in the prepared product were 33.16% and 18.62% respectively, the impurity S and Na contents were 0.008% and 0.004% respectively, and the impurities such as Pb, Zn, Ca, and Mg were at the ppm level. The manganese iron phosphate lithium positive electrode material prepared with this product as raw material has excellent physical and chemical properties, and the 1C discharge specific capacity is 151.05mAh / g.
[0119] Example 3
[0120] High-quality and high-purity manganese phosphate, a raw material of lithium manganese iron phosphate, is prepared using zinc anode mud with the composition of Zn: 2.61wt%, Mn: 35.93wt%, Pb: 14.82wt%, and Ag: 0.0745wt%, and the remaining valuable metals are comprehensively recovered.
[0121] Step A, zinc anode mud and 40g / L dilute sulfuric acid activator are added into a ball mill at a ratio of 1:2.5, and then ball milled for activation, the ball milling particle size is controlled to be 80% particle size = 350 mesh, and after passing the test, it is pumped into a leaching tank for leaching and dezincification, the dezincification temperature is 82°C, the time is 2.5h, and activated dezincification slag and zinc sulfate solution are obtained;
[0122] Step B: Activate the Mn in the dezincification slag 4+ Reduction to Mn2+ The reducing agent glucose which is 1.20 times of the theoretical amount is added into a sulfuric acid solution with a titer of 450 g / L, and the mixture is continuously stirred and aged at a temperature of 60° C. for 3 h to obtain an aged reducing agent;
[0123] Step C, adding the activated dezincification slag obtained in step A and the mature reducing agent obtained in step B into a reaction tank added with appropriate water and continuously stirred for reduction acid leaching, wherein the initial sulfuric acid titer in the solution is 120 g / L, the liquid-solid weight ratio is 7:1, the temperature is 92° C., the time is 7 hours, and after the reaction is completed, filter pressing is performed to obtain a manganese sulfate solution and a highly enriched lead and silver leaching slag;
[0124] Step D, first adjust the pH value of the manganese sulfate leaching solution obtained in step C to 7.2 with ammonia water, add 1.35 times the theoretical amount of the required purifier NH4F or (NH4)2S for purification, the temperature is room temperature, the time is 100 minutes, and then use activated carbon for adsorption and deoiling. After the reaction is completed, filter to obtain the purified liquid and purified residue;
[0125] Step E: first adjust the pH value of the purified liquid obtained in step D to 2.5 with sulfuric acid, slowly add manganese to complete the formation of 1.10 times the theoretical amount of manganese phosphate precipitation and a mass concentration of 50% synthetic agent sodium phosphate, use sulfuric acid to ensure that the process and end point pH value is 3.5, control the reaction temperature to 45°C, and the reaction time is 6 hours to obtain a manganese phosphate precursor. The manganese phosphate precursor after slurry washing 3 times is spray dried at a spray drying temperature of 320°C and a spray turntable speed of 46 Hz. After air flow crushing, a manganese phosphate product with a medium particle size of D50=1.32 μm is obtained.
[0126] Through the comprehensive recovery of the zinc anode mud samples, the recovery rates of manganese and zinc in the zinc anode mud were 99.4% and 99.3% respectively, and 99.2% of lead and silver were enriched in the lead-silver leaching slag; at the same time, the Mn and P contents in the prepared product were 33.21% and 18.83% respectively, the impurity S and Na contents were 0.005% and 0.003% respectively, and the impurities such as Pb, Zn, Ca, and Mg were at the ppm level. The manganese iron phosphate lithium positive electrode material prepared with this product as raw material has excellent physical and chemical properties, and the 1C discharge specific capacity is 153.16mAh / g.
[0127] The process of the present application is reliable, and a high-quality high-purity manganese phosphate product for preparing lithium iron manganese phosphate or lithium manganese phosphate raw material is obtained. The impurity content of Pb, Zn, Ca, Mg and the like in the product is at the ppm level. At the same time, the manganese recovery rate exceeds 97%, the zinc recovery rate reaches 96%, and more than 98.5% of the lead and silver are enriched in the lead-silver leaching residue.
[0128] Those skilled in the art will appreciate that the accompanying drawings are merely schematic diagrams of a preferred implementation scenario, and the modules or processes in the accompanying drawings are not necessarily required for implementing the present application.
[0129] The above application serial numbers are for description only and do not represent the advantages or disadvantages of the implementation scenarios.
[0130] The above disclosure only discloses several specific implementation scenarios of the present application. However, the present application is not limited thereto, and any changes that can be conceived by technicians in this field should fall within the scope of protection of the present application.
Claims
1. A method for recycling zinc anode mud, characterized in that: include: Ball milling and activation treatment of zinc anode mud; The zinc anode mud after ball milling activation is immersed in a sulfuric acid solution for leaching, and filtered to obtain activated dezincification slag and zinc sulfate solution; transporting the zinc sulfate solution to a zinc return system to recover zinc; The activated dezincification slag and the reducing agent are added into deionized water for reduction acid leaching, and filtered to obtain a manganese sulfate solution and lead-silver leaching slag; The lead-silver leaching residue is transported to a lead return system to recover lead and silver; Sodium phosphate is added to the manganese sulfate solution to synthesize a manganese phosphate product.
2. The method according to claim 1, characterized in that The step of ball milling and activating the zinc anode mud specifically comprises: Adding the zinc anode mud and the activator into a ball mill for ball milling activation treatment; Obtaining a value of the percentage of zinc anode mud particles having a particle size less than or equal to a preset particle size threshold in the ball mill; When the data proportion value is greater than or equal to the preset proportion value, the ball milling activation operation is stopped.
3. The method according to claim 1, characterized in that The step of adding the activated dezincification slag and the reducing agent into deionized water for reduction acid leaching, and filtering to obtain the manganese sulfate solution and the lead-silver leaching slag specifically comprises: adding the activated dezincification slag and a reducing agent into deionized water for reduction acid leaching to obtain a mixture; The mixture is filtered by a filter press to obtain the manganese sulfate solution and the lead-silver leaching residue.
4. The method according to claim 1, characterized in that: Before adding the activated dezincification slag and the reducing agent into deionized water for reduction acid leaching and filtering to obtain the manganese sulfate solution and the lead-silver leaching slag, the method further comprises: Obtain a preset amount of glucose; Adding the glucose into a sulfuric acid solution of a preset titer and stirring the solution to obtain a matured reducing agent; Wherein, the preset dosage of the glucose is 1.05% to 1.3% of the theoretical dosage for reducing positive tetravalent manganese ions in the activated dezincification slag to positive divalent manganese ions; The preset titer ranges from 350 g / L to 600 g / L; The temperature range for the aging operation is 45°C to 80°C; The reaction time of the aging operation ranges from 1 hour to 5 hours.
5. The method according to claim 1, characterized in that The step of adding sodium phosphate to the manganese sulfate solution to synthesize the manganese phosphate product specifically comprises: adding a sulfuric acid solution dropwise into the manganese sulfate solution to control the pH value of the manganese sulfate solution to be within a first preset range; adding the sodium phosphate into the manganese sulfate solution and stirring, and dropping a sulfuric acid solution into the reaction solution to control the pH of the reaction solution to be within a second preset range, to form a manganese phosphate precursor; Slurry washing the manganese phosphate precursor according to a preset number of times; The washed manganese phosphate precursor is spray dried to obtain the manganese phosphate product.
6. The method according to claim 1, characterized in that Before adding sodium phosphate to the manganese sulfate solution to synthesize the manganese phosphate product, the method further comprises: adding ammonia water to the manganese sulfate solution to control the pH value of the manganese sulfate solution to be within a third preset range; adding a purifying agent to the manganese sulfate solution for purification; The manganese sulfate solution treated with a purifier is added to activated carbon for adsorption, and filtered to obtain a purified manganese sulfate solution.
7. The method according to any one of claims 1 to 6, characterized in that The activator is dilute sulfuric acid; In the ball milling activation operation, the titer of the activator ranged from 30 g / L to 50 g / L; The weight ratio of zinc anode mud to activator is 1:(1.5-3).
8. The method according to any one of claims 1 to 6, characterized in that In the reduction acid leaching operation of activated dezincification slag, the initial titer of the sulfuric acid solution ranges from 90 g / L to 150 g / L; The liquid-to-solid ratio of deionized water, activated dezincification slag and reducing agent is (6-8):1; The temperature range for reducing acid leaching operation is 90 degrees Celsius to 95 degrees Celsius; The reaction time for the reductive acid leaching operation ranges from 5 hours to 8 hours.
9. The method according to any one of claims 1 to 6, characterized in that In the operation of synthesizing the manganese phosphate precursor, the amount of sodium phosphate added is 1.05% to 1.15% of the theoretical amount of manganese phosphate precipitate; The reaction temperature range for synthesizing the manganese phosphate precursor is 40 degrees Celsius to 50 degrees Celsius; The reaction time for synthesizing the manganese phosphate precursor is in the range of 5 hours to 8 hours.
10. The method according to any one of claims 1 to 6, characterized in that The temperature range for spray drying operation is 300°C to 350°C; The spray disk speed range for spray drying operation is 43 Hz to 48 Hz.