Method for realizing comprehensive recovery of high-value metals through scandium ore first-stage sulfuric acid leaching

Through a sulfuric acid leaching method, the fineness and leaching conditions of grinding ore are controlled, and the problem of enrichment of Sc2O3 and TiO2 in scandium mines is solved, the comprehensive recovery of high-value metals and efficient enrichment of titanium and aluminum minerals is achieved, and the ore dressing process is simplified. .

CN118880073APending Publication Date: 2024-11-01中国冶金地质总局昆明地质勘查院
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410975475.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively enrich Sc2O3 and TiO2 in scandium ore. Conventional ore dressing methods such as reselecting, flotation, and magnetic separation cannot effectively achieve comprehensive recovery of high-value metals in scandium ore, and scandium ore is dispersed in the earth's crust and is associated with other elements. Co-generated ore is difficult to separate.

Method used

By controlling the grinding fineness, sulfuric acid leaching acid concentration, liquid-solid ratio and leaching time, the high leaching rate of Sc2O3, TiO2, Fe2O3 and Al2O3 is achieved, and suitable leaching liquid and leaching residue are obtained, further improving titanium and The monomer dissociation degree of aluminum minerals simplifies the ore dressing process.

Benefits of technology

The high leaching rates of Sc2O3, TiO2, Fe2O3 and Al2O3 are achieved, the ore dressing process is simplified, the necessity of second-stage leaching is avoided, the enrichment efficiency of titanium and aluminum minerals is improved, and the comprehensive recovery of high-value metals of scandium ore is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880073A_ABST
    Figure CN118880073A_ABST
Patent Text Reader

Abstract

The invention relates to a method for realizing comprehensive recovery of high-value metals by scandium ore first-stage sulfuric acid leaching. The method comprises the following steps: step 1) collecting raw ore; (2) ore grinding treatment is conducted, and the ore grinding fineness is controlled; (3) sulfuric acid leaching treatment is conducted, and the leaching acid concentration, the leaching time and the liquid-solid ratio are controlled; and (4) first-stage sulfuric acid leaching is finished, and leachate and leaching residues are collected. According to the method, suitable conditions and optimal conditions for first-stage sulfuric acid leaching of the raw scandium ore are found out. And crystallizing and extracting aluminum from the first-section leachate to obtain an aluminum ammonium sulfate product, concentrating and crystallizing iron to obtain a ferrous sulfate product, and extracting Sc2O3 and TiO2. The invention proves that the scandium ore is not necessary to be subjected to second-stage leaching after being subjected to first-stage sulfuric acid leaching.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of scandium ore dressing methods, and in particular to the technical field of methods for realizing comprehensive recovery of high-value metals by one-stage sulfuric acid leaching of scandium ore. Background Art

[0002] Although scandium is the first transition metal in the periodic table, with an atomic number of only 21, it was discovered relatively late. On the one hand, it is too rare and very dispersed, making it difficult to enrich. The average abundance in the earth's crust is 17×10 -6 (Li Tong, 2011), the second reason is that it is difficult to separate from the ore under the experimental conditions at that time. In terms of mineralization, scandium often has its own particularity. It is extremely dispersed in the earth's crust and generally does not appear with other lanthanide elements. Instead, it has a close relationship with basic rocks in mineralization. Therefore, it mainly forms minerals or co-formed minerals with elements such as iron, titanium, aluminum, and vanadium. Conventional mineral processing exploration tests have shown that gravity separation, flotation, and magnetic separation cannot effectively enrich Sc2O3 and TiO2. Therefore, Sc2O3 can only be extracted by chemical mineral processing. Therefore, it is necessary to find a leaching method to achieve comprehensive recovery of high-value metals in scandium ore. Summary of the invention

[0003] The present invention is to solve the above-mentioned problems and defects and provides a method for comprehensive recovery of high-value metals by one-stage sulfuric acid leaching of scandium ore.

[0004] The present invention is implemented by the following technical solution.

[0005] A method for comprehensive recovery of high-value metals by one-stage sulfuric acid leaching of scandium ore, the method of the present invention comprises the following steps:

[0006] Step 1) Collection of raw ore;

[0007] Step 2) grinding to control the grinding fineness;

[0008] Step 3) sulfuric acid leaching treatment, controlling the leaching acid concentration, leaching time and liquid-to-solid ratio;

[0009] Step 4) ends a stage of sulfuric acid leaching, and collects the leaching solution and leaching residue.

[0010] Furthermore, the method of the present invention does not include subsequent second-stage leaching.

[0011] Furthermore, in step 2) of the present invention, the grinding fineness is set to -200 mesh 82.52% to -200 mesh 93.22%.

[0012] Furthermore, in step 2) of the present invention, the grinding fineness is set to -200 mesh 85.44%.

[0013] Furthermore, in step 3) of the present invention, the leaching acid concentration is set to 40% to 60%.

[0014] Furthermore, in step 3) of the present invention, the leaching acid concentration is set to 50%.

[0015] Furthermore, in step 3) of the present invention, the leaching time is set to 30 to 90 minutes.

[0016] Furthermore, in step 3) of the present invention, the leaching time is set to 60 minutes.

[0017] Furthermore, in step 3) of the present invention, the liquid-to-solid ratio is set to 3:1 to 5:1.

[0018] Furthermore, in step 3) of the present invention, the liquid-to-solid ratio is set to 5:1.

[0019] The beneficial effects of the present invention are:

[0020] (1) The present invention has explored the suitable and optimal conditions for the first-stage sulfuric acid leaching of scandium ore. The optimal conditions are: grinding fineness -200 mesh 85.44%, sulfuric acid concentration 50%, liquid-solid ratio 5:1, leaching time 60min, and the leaching rates of Sc2O3, TiO2, Fe2O3, and Al2O3 obtained by the first-stage leaching are 92.85%, 65.54%, 97.40%, and 89.90%, respectively. Aluminum can be crystallized from the first-stage leaching liquid to obtain ammonium aluminum sulfate products, and ferrous sulfate products can be obtained by concentrating and crystallizing iron, and Sc2O3 and TiO2 can be extracted.

[0021] (2) After the first-stage slag leaching, a large amount of Al2O3 and Fe2O3 dissolved, which increased the monomer dissociation degree of titanium and aluminum minerals, and was beneficial to the beneficiation and enrichment of TiO2 and Al2O3. However, the first-stage slag beneficiation exploration test showed that neither gravity separation nor flotation could effectively enrich TiO2 and Al2O3, which further explained that the original ore scandium ore had a fine particle size and was difficult to enrich by conventional beneficiation. Moreover, the first-stage leaching slag contained Sc2O3, TiO2, Fe2O3, and Al2O3 of 15g / t, 1.52%, 1.02%, and 4.51%, respectively, so there was no need for a second-stage leaching.

[0022] The present invention will be further explained below in conjunction with the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the experimental principle flow of the leaching process of the present invention.

[0024] Figure 2 It is a flow chart of the reselection test of the present invention.

[0025] Figure 3 It is a flotation test flow chart of the present invention. DETAILED DESCRIPTION

[0026] The following examples are only a part of the technical solution of the present invention, and are not intended to limit the entire technical solution of the present invention. The examples of the present invention are provided to further explain and illustrate the details of the technical solution of the present invention.

[0027] 1. One-stage leaching test

[0028] The principle and process of the leaching process of scandium ore is as follows: Figure 1 The grinding equipment is XMQ-240×90 conical ball mill, the leaching equipment is mechanical stirring leacher, the heating equipment is electric furnace, the solid-liquid separation equipment is DZ-5C vacuum filter, and the drying equipment is HG101-3 electric heating blast drying oven. The sulfuric acid is high-grade pure, and the H2SO4 content is 97.7%.

[0029] 1.1 Grinding fineness test

[0030] Grinding fineness is an important parameter affecting leaching index. The fixed conditions are: feed 100g, sulfuric acid concentration 40%, leaching heating temperature 140℃, stirring leaching time 90min, and slurry liquid-solid ratio 4. The leaching test results of different grinding fineness are shown in Table 1.

[0031] Table 1 Leaching test results of different grinding fineness

[0032]

[0033]

[0034] Note: *Unit: g / t.

[0035] It can be seen from Table 1 that with the increase of grinding fineness, the leaching rates of scandium, titanium, iron and aluminum increase. When the grinding fineness is -200 mesh 85.44%, further increasing the grinding fineness has little effect on the leaching rates of scandium, titanium and iron. Therefore, the appropriate grinding fineness is -200 mesh 85.44%, and the leaching rates of Sc2O3, TiO2, Fe2O3 and Al2O3 are 87.66%, 51.31%, 97.52% and 85.15% respectively.

[0036] 1.2 Sulfuric acid leaching acid concentration test

[0037] Fixed conditions: feed 100g, grinding fineness -200 mesh 85.44%, stirring leaching time 60min, leaching slurry solid ratio 4, reaction heating temperature 140°C. Sulfuric acid concentration (sulfuric acid concentration is volume fraction, leaching acid concentration and sulfuric acid concentration are the same below) leaching test results are shown in Table 2.

[0038] Table 2 Sulfuric acid concentration leaching test results

[0039]

[0040] Note: *Unit: g / t.

[0041] As can be seen from Table 2, with the increase of sulfuric acid concentration, the leaching rates of scandium, titanium, iron and aluminum increase. Among them, the leaching rates of scandium and titanium are most affected by the sulfuric acid concentration, while aluminum and iron are relatively easy to leach. When the sulfuric acid concentration is 50%, the leaching rates of Sc2O3, TiO2, Fe2O3 and Al2O3 are 87.66%, 51.31%, 97.52% and 85.15% respectively. When the acidity reaches 60%, the leaching rates of Sc2O3, TiO2, Fe2O3 and Al2O3 are 88.74%, 62.64%, 94.91% and 86.20% respectively. The leaching rates of Sc2O3, Fe2O3 and Al2O3 are not greatly improved, but the leaching rate of TiO2 is still greatly improved. However, the excessively high acidity condition is difficult to control, so the appropriate acidity is 50%.

[0042] 1.3 Sulfuric acid leaching time test

[0043] Feeding material 100g, grinding fineness -200 mesh 85.44%, leaching slurry solid ratio 4, sulfuric acid concentration 50%, leaching time test results are shown in Table 3.

[0044] Table 3 Sulfuric acid leaching time test results

[0045]

[0046]

[0047] Note: *Unit: g / t.

[0048] It can be seen from Table 3 that with the extension of sulfuric acid leaching time, the leaching rates of scandium, titanium, iron and aluminum increase, except that the leaching rate of TiO2 increases from 52.56% to 64.73% at 150min. In fact, during the period of 60min to 120min, the leaching rates of Sc2O3, TiO2, Fe2O3 and Al2O3 do not change much. Therefore, the experimental leaching time is 60min, and the leaching rates of Sc2O3, TiO2, Fe2O3 and Al2O3 are 87.66%, 51.31%, 97.52% and 85.15% respectively.

[0049] 1.4 Sulfuric acid leaching liquid-to-solid ratio test

[0050] Fixed conditions: feed 100 g, grinding fineness -200 mesh 85.44%, sulfuric acid concentration 50%, stirring leaching time 60 min, the leaching liquid-solid ratio test results are shown in Table 4.

[0051] Table 4 Sulfuric acid leaching liquid-to-solid ratio test results

[0052]

[0053] Note: *Unit: g / t.

[0054] As can be seen from Table 4, increasing the liquid-to-solid ratio will not change the indicators much, but will cause excessive acid consumption. A liquid-to-solid ratio of 5:1 is more appropriate. Under this condition, the leaching rates of Sc2O3, TiO2, Fe2O3 and Al2O3 are 88.44%, 56.43%, 97.65% and 89.03% respectively.

[0055] In summary, the best conditions for the first stage sulfuric acid leaching are: grinding fineness -200 mesh 85.44%, sulfuric acid concentration 50%, liquid-solid ratio 5:1, and leaching time 60min. Under this comprehensive condition, the test feed amount was enlarged to 2000g, the purpose was to further verify the reliability of the above leaching conditions, and also to further prepare test samples for the subsequent test of the second stage leaching. The test results are shown in Tables 5 and 6.

[0056] Table 5 Results of the first stage leaching comprehensive conditions test

[0057]

[0058]

[0059] Note: *Unit: g / t.

[0060] Table 6 Analysis results of the first stage leaching solution

[0061]

[0062] The comprehensive condition test proves that the test scale is enlarged from 100g to 2000g. Comparing Table 5 with Table 6, the test repeatability is good, indicating that the leaching conditions are reliable. As can be seen from Table 5 and Table 6, the leaching rates of Sc2O3, TiO2, Fe2O3, and Al2O3 obtained by leaching are 92.85%, 65.54%, 97.40%, and 89.90%, respectively; aluminum can be crystallized from the leachate to obtain ammonium aluminum sulfate products, and iron can be concentrated to obtain ferrous sulfate products, and Sc2O3 and TiO2 can be extracted. The leaching residue contains 15g / t of Sc2O3, TiO2, Fe2O3, and Al2O3, respectively. 1.52%, 1.02%, and 4.51%.

[0063] 2. Leaching slag beneficiation exploration test

[0064] After the first stage of slag leaching, the leached slag contains 15g / t of Sc2O3, 1.52%, 1.02% of TiO2, and 4.51% of Fe2O3, respectively. A large amount of Al2O3 and Fe2O3 dissolved, which improves the monomer dissociation degree of titanium and aluminum minerals, is conducive to the concentration and enrichment of TiO2 and Al2O3. Therefore, conventional beneficiation is expected to enrich TiO2 and Al2O3, and return leaching to increase the leaching rate of titanium and aluminum. The exploration process of gravity separation and flotation is shown in Figure 2 , Figure 3 The test results are shown in Table 7 and Table 8 respectively.

[0065] Table 7 Results of reselection exploration test

[0066]

[0067] Table 8 Flotation exploration test results

[0068]

[0069]

[0070] It can be seen from Tables 7 and 8 that neither gravity separation nor flotation can effectively enrich TiO2 and Al2O3. This further shows that the original scandium ore has fine particle size and is difficult to enrich by conventional mineral processing. Therefore, it is impossible to further enrich TiO2 and Al2O3 and return to leaching to increase the leaching rate of titanium and aluminum, and there is no need for secondary leaching.

[0071] The above are only some specific embodiments of the present invention (since the present invention includes numerical content, the embodiments cannot be exhaustive, and the protection scope recorded in the present invention includes the numerical content and other technical key points of the present invention). The well-known specific content or common sense in the scheme is not described in detail here (including but not limited to abbreviations, abbreviations, and units commonly used in the art). It should be pointed out that the above embodiments do not limit the present invention in any way. For those skilled in the art, all technical solutions obtained by equivalent substitution or equivalent transformation fall within the protection scope of the present invention. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A method for comprehensive recovery of high-value metals by one-stage sulfuric acid leaching of scandium ore, characterized in that: The method comprises the following steps: Step 1) Collection of raw ore; Step 2) grinding to control the grinding fineness; Step 3) sulfuric acid leaching treatment, controlling the leaching acid concentration, leaching time and liquid-to-solid ratio; Step 4) ends a stage of sulfuric acid leaching, and collects the leaching solution and leaching residue.

2. The method for realizing comprehensive recovery of high-value metals by one-stage sulfuric acid leaching of scandium ore according to claim 1, characterized in that: The method does not include subsequent secondary leaching.

3. The method for realizing comprehensive recovery of high-value metals by one-stage sulfuric acid leaching of scandium ore according to claim 1, characterized in that: In the step 2), the grinding fineness is set to -200 mesh 82.52% to -200 mesh 93.22%.

4. The method for realizing comprehensive recovery of high-value metals by one-stage sulfuric acid leaching of scandium ore according to claim 3, characterized in that: In the step 2), the grinding fineness is set to -200 mesh 85.44%.

5. The method for realizing comprehensive recovery of high-value metals by one-stage sulfuric acid leaching of scandium ore according to claim 1, characterized in that: In the step 3), the leaching acid concentration is set to 40% to 60%.

6. The method for realizing comprehensive recovery of high-value metals by one-stage sulfuric acid leaching of scandium ore according to claim 5, characterized in that: In step 3), the leaching acid concentration is set to 50%.

7. The method for realizing comprehensive recovery of high-value metals by one-stage sulfuric acid leaching of scandium ore according to claim 1, characterized in that: In the step 3), the leaching time is set to 30 to 90 minutes.

8. The method for realizing comprehensive recovery of high-value metals by one-stage sulfuric acid leaching of scandium ore according to claim 7, characterized in that: In the step 3), the leaching time is set to 60 minutes.

9. The method for realizing comprehensive recovery of high-value metals by one-stage sulfuric acid leaching of scandium ore according to claim 1, characterized in that: In the step 3), the liquid-to-solid ratio is set to 3:1 to 5:

1.

10. The method for realizing comprehensive recovery of high-value metals by one-stage sulfuric acid leaching of scandium ore according to claim 1, characterized in that: In the step 3), the liquid-to-solid ratio is set to 5:1.