Precipitation strengthening type high-performance medical multi-principal-element alloy as well as preparation method and application thereof

By using the coordinated strengthening of strong lattice distortion and cognano-precipitation phase in multi-main alloys, the problems of insufficient bio-friction performance and poor wear resistance of medical metal materials in artificial joints are solved, and high strength and low elasticity are achieved Medical multi-main alloy with modulus and high wear resistance, suitable for artificial joints and dental implant materials.

CN118880147AInactive Publication Date: 2024-11-01HEYUAN CITY SHENHE PEOPLES HOSPITAL (THE FIFTH AFFILIATED HOSPITAL OF JINAN UNIV)
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410920373.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-07-24
Filing Date
2024-07-10
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure CN118880147A_ABST
    Figure CN118880147A_ABST
Patent Text Reader

Abstract

The invention discloses a precipitation strengthening type high-performance medical multi-principal-element alloy and a preparation method and application thereof. The problems that an existing biomedical metal material is high in elasticity modulus and poor in abrasion resistance and contains potential toxic elements are solved. The medical multi-principal-element alloy disclosed by the invention is composed of several high-biocompatibility elements such as Ti, Zr, Nb, Ta or Mo, and does not contain any potential toxic element. Through cooperative regulation and control of components, plastic deformation and heat treatment, the lattice distortion and nano precipitated phase cooperative strengthening novel medical multi-principal-element alloy is prepared. The alloy has high strength and high wear resistance, and can be used in the fields of artificial joint prostheses and dental implant materials. The preparation method of the alloy is simple and easy to implement, and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of alloy materials and preparation thereof, and in particular to a precipitation-strengthened high-performance medical multi-principal-element alloy and a preparation method and application thereof. Background Art

[0002] With the aging of the population, the continuous extension of life expectancy and the further improvement of the quality of life, the clinical demand for long-term surgical implants has gradually increased. Taking artificial joints as an example, the number of artificial knee and hip replacement surgeries in my country in 2019 has reached more than 900,000, and is growing rapidly at a rate of nearly 20% per year. However, clinical statistics show that some patients' artificial joint prostheses began to experience "service failure" about 10 years after surgery. An important reason for this is the mismatch between implant performance (biological properties, mechanical properties, biotribological properties, etc.) and human service conditions, resulting in aseptic loosening or breakage of the prosthesis, among which aseptic loosening caused by implant wear accounts for 80% of artificial joint revision surgeries. The development of new high-performance medical metal materials has become an important direction to solve the problem of long-term clinical service of artificial joints.

[0003] Artificial joints have a biological friction interface at the femoral head or femoral condyle. Under the dual effects of intense exercise load and complex physiological environment in the body, the quality of the material's biotribological properties at this surface interface will be the focus and key factor affecting the long-term effectiveness of artificial joints. 6 Al 4 V) A study on the recovery of three femoral head implants (polymer polyethylene acetabular cup) found that titanium alloy femoral head wear was the largest, with an average of 74.3%. At present, the medical metal material with the best tribological performance is cobalt-chromium-molybdenum alloy. However, the metal ions such as Co and Cr released during long-term use have very high biotoxicity, which can cause systemic poisoning reactions and even cause cancer. Although medical titanium alloys have extremely significant advantages over other metal long-term bone implant materials in terms of biocompatibility and biomechanical compatibility, the shortcomings of their tribological performance seriously restrict their widespread application in artificial joints. In order to improve the tribological properties of medical titanium alloys, most of the existing studies have adopted the method of surface modification to increase the surface hardness of the original titanium alloy or reduce the friction coefficient. However, the application of any surface modification means will cause new interface problems and increase production difficulty and cost. Therefore, it is urgent to develop new medical metal materials with excellent comprehensive mechanical properties, biocompatibility and biotribological properties.

[0004] Multi-principal component (medium and high entropy) alloys are a new type of metal material that has emerged in this century. Different from the traditional alloy design that mainly uses 1 to 2 elements and adds other elements as supplementary materials, multi-principal component alloys are composed of 4 or more elements in the form of principal components (content not less than 5at.%), and have a unique multi-component solid solution structure. The field of multi-principal component alloys has achieved remarkable results in less than 20 years of development history. Related research has been reported many times by authoritative journals such as "Nature" and "Science", solving many bottleneck problems in material performance. In view of the attractive prospects of multi-principal component alloys in the development of high-performance new materials, more and more scientists have turned their attention to the research of medical multi-principal component alloys. However, the medical multi-principal component alloys reported so far generally have poor plasticity and high modulus at room temperature. In addition, these medical multi-principal component alloys are mainly in cast state, and research on their organizational regulation process is relatively lacking. In summary, developing a new type of biomedical multi-principal component alloy with excellent performance will greatly expand the application prospects of multi-principal component alloys in the field of biomedical materials and provide greater space for the development of biomedical materials. Summary of the invention

[0005] In order to overcome the shortcomings of the prior art, one of the objects of the present invention is to provide a precipitation-strengthened high-performance medical multi-principal component alloy, which utilizes the strong lattice distortion effect of the multi-principal component alloy and the synergistic strengthening effect of the coherent nano-precipitate phase. The alloy has good biocompatibility and can obtain high strength, low elastic modulus and high wear resistance under certain process control; the second object of the present invention is to provide an application of a precipitation-strengthened high-performance medical multi-principal component alloy, which is applied to biomedical materials; the third object of the present invention is to provide a preparation method of a precipitation-strengthened high-performance medical multi-principal component alloy, which can in-situ generate a coherent nano-precipitate phase in the medical multi-principal component alloy, while improving the strength and wear resistance of the alloy without significantly reducing the plasticity of the alloy and increasing the elastic modulus.

[0006] One of the purposes of the present invention is achieved by the following technical solution:

[0007] A precipitation-strengthened high-performance medical multi-principal alloy comprises the following chemical components in terms of atomic percentage: Ti 35-45 at.%, Zr 35-45 at.%, Nb 10-20 at.%, and Ta 5-15 at.%.

[0008] Furthermore, a precipitation-strengthened high-performance medical multi-principal alloy includes the chemical components, in terms of atomic percentage, of Ti 35-45 at.%, Zr 35-45 at.%, Nb 10-20 at.%, Ta 5-15 at.%, and Mo 0.1-6 at.%.

[0009] The second object of the present invention is achieved by adopting the following technical solution:

[0010] The above-mentioned precipitation-strengthened high-performance medical multi-principal component alloy is applied to biomedical materials.

[0011] The third object of the present invention is achieved by adopting the following technical solution:

[0012] The preparation method of the above-mentioned precipitation-strengthened high-performance medical multi-principal alloy comprises the following steps:

[0013] 1) First, the corresponding pure metals in the precipitation-strengthened high-performance medical multi-principal alloy are melted in proportion to obtain a rod-shaped alloy ingot; the alloy ingot has a single-phase equiaxed crystal structure without nano-precipitated phase;

[0014] 2) subjecting the alloy ingot to plastic deformation treatment;

[0015] 3) Annealing the alloy ingot after plastic deformation, then taking it out and quenching it in water to room temperature to obtain a precipitation-strengthened high-performance medical multi-principal alloy.

[0016] Furthermore, in step 1), the smelting is one of arc melting, induction melting and vacuum suspension melting.

[0017] Furthermore, in step 1), the arc melting method is carried out in an Ar gas environment with a purity of ≥99.999%.

[0018] Furthermore, in step 2), the plastic deformation treatment is one of rolling, forging, extrusion and high-pressure torsion.

[0019] Furthermore, in step 2), the deformation amount of the alloy ingot plastic deformation is not less than 60%, and the deformation amount each time does not exceed 5% of the original ingot size.

[0020] Furthermore, in step 2), the temperature of the plastic deformation treatment is 20-40°C.

[0021] Furthermore, in step 3), the annealing temperature is 0.35 to 0.45 of the melting point of the alloy, and then the temperature is kept for 0.5 to 2 hours.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) The element composition of the precipitation-strengthened high-performance medical multi-principal alloy of the present invention is Ti, Zr, Nb and Ta. There is a miscibility gap, a high shear modulus difference and an atomic size difference between the above elements, which can induce a high lattice distortion alloy component combination, so that the matrix alloy component has high strength and high wear resistance. Furthermore, by utilizing the miscibility gap between Nb and Ta elements and Ti and Zr elements and the principle that high melting point elements have a lower diffusion rate, the alloy can precipitate a nanoscale coherent secondary phase under the action of plastic deformation and heat treatment processes. The second phase particle composition is close to the matrix and can coordinate deformation with the matrix alloy, which significantly improves the strength and wear resistance of the material without significantly increasing the elastic modulus or reducing the plasticity of the alloy.

[0024] (2) The element composition of the alloy of the present invention may include Mo in addition to Ti, Zr, Nb and Ta. The Mo element has a strong lattice distortion effect. Adding this element to the medical multi-principal alloy system can significantly improve the basic strength and wear resistance of the alloy, but it will increase the elastic modulus of the alloy to a certain extent.

[0025] (3) The precipitation-strengthened high-performance medical multi-principal alloy of the present invention solves the problems of existing biomedical metal materials with high elastic modulus, poor wear resistance and potentially toxic elements. The present invention prepares a new medical multi-principal alloy with lattice distortion and nano-precipitation phase synergistic strengthening through coordinated regulation of composition, plastic deformation and heat treatment. The tensile yield strength at room temperature can reach more than 1GPa, the tensile plasticity exceeds 18%, the elastic modulus is less than 85GPa, and the wear resistance is up to 7 times that of the traditional medical titanium alloy TC4. It can be used in the field of artificial joint prostheses and dental implant materials.

[0026] (4) The preparation method of the medical multi-principal alloy of the present invention comprises the following steps: firstly, a single metal is smelted, then plastically deformed, and then annealed to obtain a medical multi-principal alloy. The alloy has a single-phase BCC structure in the cast state, and forms a micrometer-scale BCC1 phase and a nanometer-scale BCC2 phase after plastic deformation and annealing. The preparation method is simple, easy to implement, and has broad application prospects. The tensile yield strength of the medical multi-principal alloy obtained by the above preparation method is between 800 and 1150 MPa, the fracture strain is between 10 and 25%, and the elastic modulus is between 66 and 86 GPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the phase diagram simulation result of the product in Example 1 of the present invention.

[0028] Figure 2 This is a picture of the as-cast microstructure of the product of Example 1 of the present invention.

[0029] Figure 3This is a microstructure picture of the product of Example 1 of the present invention after rolling and annealing.

[0030] Figure 4 This is the XRD spectrum of the product of Example 1 of the present invention after rolling and annealing.

[0031] Figure 5 It is a comparison chart of the mechanical properties of the product of Example 1 in the present invention.

[0032] Figure 6 It is a comparison chart of the wear rates of the products in Example 1 of the present invention.

[0033] Figure 7 This is a microstructure picture of the product of Example 2 of the present invention after rolling and annealing. DETAILED DESCRIPTION

[0034] The present invention is further described below in conjunction with specific implementation methods. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form a new embodiment.

[0035] Example 1

[0036] A precipitation-strengthened high-performance medical multi-principal alloy and a preparation method thereof, comprising the following steps:

[0037] The chemical composition expression of the medical multi-principal alloy in this embodiment is Ti 37.5 Zr 37.5 Nb 15 Ta 5 Mo 5 , wherein the atomic percentages of Ti, Zr, Nb, Ta and Mo are 37.5%, 37.5%, 15%, 5% and 5% respectively. 37.5 Zr 37.5 Nb 15 Ta 5 Mo 5 The preparation method of the medical multi-principal alloy comprises the following steps:

[0038] S1: The raw materials used in this experiment are high-purity metals Ti, Zr, Nb, Ta and Mo (purity greater than 99.95%). The metal raw materials are polished with sandpaper to remove the surface oxide scale before weighing, and then placed in anhydrous ethanol for ultrasonic vibration to remove residual impurities. The mass of each component is weighed using an electronic balance with an accuracy of 0.001g (sartorius, GL124l-1SCN), and the error is controlled within ±0.005g, and the ingredients are prepared according to 72g of each alloy ingot.

[0039] S2: Use a non-consumable vacuum arc furnace to melt the sample. Place the metal raw materials in the crucible in the furnace in order from low to high melting points. After the raw materials are placed, use a mechanical pump and a molecular pump to evacuate the furnace. When the vacuum reaches 5×10 -3 After Pa, 0.5 atmospheres of high-purity argon (purity ≥ 99.999%) is filled, and then the above operation is repeated twice to ensure the purity of the atmosphere in the furnace and eliminate the influence of elements such as C, O, and N on the experiment. During the smelting process, the pre-placed Ti ingot must be melted for about 60 seconds before each smelting of the alloy raw materials to further remove impurities in the furnace. The liquid retention time of each alloy ingot is 90 seconds during smelting, and electromagnetic stirring is turned on to stir the molten metal. After the alloy ingot is cooled, it is turned over, and the smelting is repeated for more than 10 times to ensure that the alloy composition is uniform. After the smelting is completed, vacuum suction casting is carried out using a 15mm×15mm×50mm water-cooled copper mold equipped with the smelting furnace.

[0040] S3: The ingot is placed in a double-roll rolling mill for cold rolling. The total ingot pressure is 9 mm (deformation is 60%). The rolling passes are 30 times, and the pressure is 0.3 mm each time. The final size of the sample after cold rolling is about 20 mm × 6 mm × 100 mm.

[0041] S4: After cold rolling, the sample is cut into the required size and placed in a vacuum tube furnace for annealing. Before annealing, the furnace is evacuated by a mechanical pump, and then high-purity argon gas is continuously introduced as a protective atmosphere. The annealing temperature is the melting point of 740°C, the holding time is 1h, and water quenching is performed after the annealing is completed.

[0042] Figure 1 This is the phase diagram simulation result of the medical multi-principal alloy of this embodiment. It can be seen from the figure that the alloy has a miscibility gap. Figure 2 The SEM image and EDS surface distribution image of the medical multi-principal alloy in the present embodiment in the cast state are shown in the figure. It can be seen from the figure that the alloy in the cast state is an equiaxed crystal structure, dendritic segregation can be seen in the grains, but no second phase is observed.

[0043] Figure 2 The SEM and TEM images of the medical multi-principal alloy of this embodiment after rolling and annealing are shown. From the figure, it can be seen that dispersed nano-second phases are precipitated in the alloy matrix. Figure 4 From the XRD diagram in, we can see that both the matrix and the precipitated phase have BCC structure.

[0044] 2) Mechanical properties test

[0045] The tensile test samples were taken from the middle of the ingot and cut into dog bone plates using an EDM wire cutting machine. The parallel section size of the sample was 15mm×4mm×2mm. Before the test, it was smoothed with sandpaper (the last sandpaper was 2000#), and the final size was measured with a vernier caliper. The tensile test equipment was an MTS electronic universal tensile testing machine, and a mechanical extensometer with a gauge length of 10mm was used to measure the strain of the sample. The experiment was carried out at room temperature, and the strain rate was 1×10 -3 s -1 To ensure the reliability of the experimental results, each group of samples was tested four times in parallel, and the final result was taken as the average value. By measuring the stress-strain curve, the yield strength, elongation after fracture, elastic modulus and other data were finally obtained.

[0046] Figure 5 The Ti in Example 1 is shown 37.5 Zr 37.5 Nb 15 Ta 5 Mo 5 The tensile properties test results of the precipitation-strengthened medical multi-principal alloy product (TZNTM-CR-740) are compared with the traditional medical alloy TC4 (Ti 6 Al 4 V) is the control group. It can be seen from the figure that the yield strength of the alloy can reach 1080MPa, which is significantly higher than the 900MPa of TC4, while the elastic modulus of the TZNTM-CR-740 alloy is about 86GPa, which is lower than the 110GPa of TC4.

[0047] 3) Tribological performance test

[0048] The samples for the tribological performance test were cut from the middle of the ingot using a wire cutting machine to obtain a 10mm×10mm×2mm block, ensuring that the upper and lower surfaces were parallel. The samples were used after mechanical grinding + electrolytic polishing + ultrasonic vibration. The experiment was carried out on the RTECMFT-5000 multifunctional friction and wear tester, using the ball-plate reciprocating friction and wear test method. The friction test stroke was 5mm, the frequency was 2Hz, the sliding speed was 20mm / s, and the load was 5N. Each test cycle was set to 1800s, and the total sliding distance was 36m. The grinding material was a zirconia ball. The experiments were carried out in a simulated saliva fluid (SSF) environment at 37±0.5℃, and the composition of the two media is shown in Table 1. Each group of experiments was conducted at least three times in parallel. The friction coefficient was obtained by taking the highest 20% of the data recorded in real time by the machine as the valid data points and then performing arithmetic averaging. The wear scar profile and the wear scar cross-sectional area were obtained using a three-dimensional profilometer, and finally the wear volume was calculated using the following Archard formula.

[0049]

[0050] Where Wr is the wear rate, V is the wear volume, F_n is the applied load, and L is the wear distance.

[0051] Table 1 Reagents and amounts required to prepare 1000 mL of simulated saliva

[0052]

[0053] Prepare simulated saliva according to Table 1. Figure 6 The results of the wear resistance test of the product of Example 1 (TZNTM-CR-740) are shown, and the conventional medical alloy TC4 is used as the control group. Figure 6 It can be seen that under simulated saliva, the wear resistance of TZNTM-CR-740 alloy can reach 7.4 times that of TC4.

[0054] Example 2

[0055] A precipitation-strengthened high-performance medical multi-principal alloy and a preparation method thereof, comprising the following steps:

[0056] The chemical composition expression of the refractory high entropy alloy in this embodiment is Ti 42.5 Zr 42.5 Nb 5 Ta 10 , wherein the atomic percentages of Ti, Zr, Nb and Ta are 42.5%, 42.5%, 5% and 10% respectively.

[0057] This embodiment Ti 42.5 Zr 42.5 Nb 5 Ta 10 The preparation method of the medical multi-principal alloy comprises the following steps:

[0058] S1: The raw materials used in this experiment are high-purity metals Ti, Zr, Nb and Ta (purity greater than 99.95%). The metal raw materials are polished with sandpaper to remove the surface oxide scale before weighing, and then placed in anhydrous ethanol for ultrasonic vibration to remove residual impurities. The mass of each component is weighed using an electronic balance with an accuracy of 0.001g (sartorius, GL124l-1SCN), and the error is controlled within ±0.005g, and the ingredients are prepared according to 72g of each alloy ingot.

[0059] S2: Use a non-consumable vacuum arc furnace to melt the sample. Place the metal raw materials in the crucible in the furnace in order from low to high melting points. After the raw materials are placed, use a mechanical pump and a molecular pump to evacuate the furnace. When the vacuum reaches 5×10 -3After Pa, 0.5 atmospheres of high-purity argon (purity ≥ 99.999%) is filled, and then the above operation is repeated twice to ensure the purity of the atmosphere in the furnace and eliminate the influence of elements such as C, O, and N on the experiment. During the smelting process, the pre-placed Ti ingot must be melted for about 60 seconds before each smelting of the alloy raw materials to further remove impurities in the furnace. The liquid retention time of each alloy ingot is 90 seconds during smelting, and electromagnetic stirring is turned on to stir the molten metal. After the alloy ingot is cooled, it is turned over, and the smelting is repeated for more than 10 times to ensure that the alloy composition is uniform. After the smelting is completed, vacuum suction casting is carried out using a 15mm×15mm×50mm water-cooled copper mold equipped with the smelting furnace.

[0060] S3: The ingot is placed in a double-roll rolling mill for cold rolling. The total ingot pressure is 9 mm (deformation is 60%). The rolling passes are 30 times, and the pressure is 0.3 mm each time. The final size of the sample after cold rolling is about 20 mm × 6 mm × 100 mm.

[0061] S4: After cold rolling, the sample is cut into the required size and placed in a vacuum tube furnace for annealing. Before annealing, the furnace is evacuated by a mechanical pump, and then high-purity argon gas is continuously introduced as a protective atmosphere. The annealing temperature is 680°C, the holding time is 1h, and water quenching is performed after the annealing is completed.

[0062] 2) Performance testing

[0063] The mechanical property test and tribological property test involved in Example 2 are the same as those in Example 1.

[0064] Figure 7 The figure shows the SEM image of the medical multi-principal alloy of this embodiment after rolling and annealing. From the figure, it can be seen that a dispersed nano-second phase is precipitated in the alloy matrix, wherein the size of the second phase is about 172nm.

[0065] In summary, the alloy has good biocompatibility and can obtain high strength, low elastic modulus and high wear resistance under certain process control, which is suitable for the requirements of biomedical materials.

[0066] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.

Claims

1. A precipitation-strengthened high-performance medical multi-principal alloy, It is characterized in that The invention comprises chemical components in terms of atomic percentage: Ti 35-45 at. %, Zr 35-45 at. %, Nb 10-20 at. % and Ta 5-15 at. %.

2. The precipitation-strengthened high-performance medical multi-principal alloy according to claim 1, It is characterized in that The invention comprises the chemical components calculated by atomic percentage: Ti 35-45 at.%, Zr 35-45 at.%, Nb 10-20 at.%, Ta 5-15 at.% and Mo 0.1-6 at.%.

3. Application of the precipitation-strengthened high-performance medical multi-principal alloy according to claim 1 or 2, It is characterized in that The precipitation-strengthened high-performance medical multi-principal-component alloy is applied to biomedical materials.

4. The method for preparing the precipitation-strengthened high-performance medical multi-principal alloy according to claim 1 or 2, It is characterized in that The following steps are involved: 1) First, the corresponding pure metals in the precipitation-enhanced high-performance medical multi-principal alloy are melted in proportion to obtain an alloy ingot; 2) subjecting the alloy ingot to plastic deformation treatment; 3) Annealing the alloy ingot after plastic deformation to obtain a precipitation-strengthened high-performance medical multi-principal alloy.

5. The method for preparing the precipitation-strengthened high-performance medical multi-principal alloy according to claim 4, It is characterized in that In step 1), the smelting is one of arc melting, induction melting and vacuum suspension melting.

6. The method for preparing the precipitation-strengthened high-performance medical multi-principal alloy according to claim 5, It is characterized in that In step 1), the arc melting method is carried out in an Ar gas environment with a purity of ≥99.999%.

7. The method for preparing the precipitation-strengthened high-performance medical multi-principal alloy according to claim 4, It is characterized in that In step 2), the plastic deformation treatment is one of rolling, forging, extrusion and high-pressure torsion.

8. The method for preparing the precipitation-strengthened high-performance medical multi-principal alloy according to claim 4 or 7, It is characterized in that In step 2), the deformation amount of the alloy ingot plastic deformation is not less than 60%, and the deformation amount each time does not exceed 5% of the original ingot size.

9. The method for preparing the precipitation-strengthened high-performance medical multi-principal alloy according to claim 4, It is characterized in that In step 2), the temperature of the plastic deformation treatment is 20-40°C.

10. The method for preparing the precipitation-strengthened high-performance medical multi-principal alloy according to claim 4, It is characterized in that In step 3), the annealing temperature is 0.35 to 0.45 of the melting point of the alloy, and then the temperature is kept for 0.5 to 2 hours.

Citation Information

Patent Citations

  • Biomedical TiZrNbTa high-entropy alloy and preparation method thereof

    CN105734312A

  • High-entropy alloy stable nano-metallic material MxNy series alloy and preparation method

    CN109182867A

  • High-performance TiZrNb alloy as well as preparation method and application thereof

    CN113249632A

  • Ti-Zr type alloy and medical appliance formed thereof

    US6767418B1