WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material and preparation method thereof

By uniformly distributing WC ceramic particles and graphite lubricating phase in an iron matrix, the problems of limited improvement in friction and wear performance and the complexity of preparation were solved, realizing the preparation of low-cost and high-efficiency self-lubricating wear-resistant materials suitable for parts under harsh friction and wear conditions.

CN118880155AActive Publication Date: 2024-11-01XIAN UNIV OF TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410926520.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-01
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

Existing technologies make it difficult to uniformly distribute ceramic particles and graphite lubricating phases in an iron matrix, which limits the improvement of tribological performance and makes the preparation of composite materials costly and complex.

Method used

By adding WC powder to molten iron and casting it with stirring, the liquid phase region is combined with large-scale supercooling for rapid solidification. This ensures that WC ceramic particles and spherical graphite are evenly distributed in the iron matrix, forming a metallurgical bond. Water-cooled graphite inner sleeves are used to suppress the agglomeration of WC particles, thus achieving rapid solidification.

Benefits of technology

A WC ceramic particle-reinforced iron-based self-lubricating wear-resistant bulk material with excellent tribological properties was prepared, reducing production costs and improving the service life and efficiency of parts under harsh working conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880155A_ABST
    Figure CN118880155A_ABST
Patent Text Reader

Abstract

The invention discloses a WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material which is formed by adding WC powder into molten iron, and the structure composition of the material is that WC ceramic particles and spheroidal graphite are uniformly distributed in an iron matrix; wherein the molten iron comprises the following raw materials in percentage by mass: 3.4%-3.7% of C, 2.4%-2.8% of Si, less than or equal to 0.6% of Mn, less than or equal to 0.02% of S, less than or equal to 0.1% of P, 0.02%-0.04% of Mg, 0.02%-0.04% of Re and the balance of Fe and inevitable impurities; and the mass of the WC powder is 10%-40% of the total mass of the WC powder and the molten iron. The invention also discloses a preparation method of the block material. The material provided by the invention has the characteristics of uniform distribution of WC ceramic particles and good frictional wear performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of iron-based composite materials, and in particular relates to a micron-sized WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material. The invention also relates to a preparation method of the block material. Background Art

[0002] With the continuous development of modern industry, there is an urgent need for steel parts that can be used under various extreme friction and wear conditions (such as high temperature, high speed, heavy load, and high wear), such as materials used in crusher hammers, excavator bucket teeth, high-speed train brake pads, rollers, etc. Traditional steel materials usually use heat treatment, alloying, or a combination of the two to improve the hardness of the material, thereby improving the friction and wear performance of the material, but these methods have limited improvement on the wear performance of steel materials, and gradually cannot meet the service conditions such as high temperature, high speed, and frequent wear. Therefore, researchers have tried to use composite means, using hard ceramic particles as the reinforcement phase, and proposed ceramic particle reinforced steel / iron-based composite materials.

[0003] Due to the high melting point of steel materials and the difficulty of uniformly distributing ceramic particles in molten iron, most of the current research on the preparation of steel / iron-based composites is limited to surface enhancement. The preparation technology of bulk ceramic particle-reinforced steel / iron-based composites is difficult, the process is complex, and the actual production cost is high. Therefore, it is urgent to develop a preparation technology for ceramic particle-reinforced iron-based bulk composites that is simple to operate and low-cost. In addition, reducing material wear by improving lubrication performance has become an important measure to extend the service life of parts. Graphite has stable chemical properties, a hexagonal lamellar structure, high thermal conductivity and low friction. It is a good solid lubricant. If it can be used as a composite phase and introduced into ceramic particle-reinforced steel / iron-based composites, its self-lubricating and friction-reducing effect will be exerted, which will greatly reduce the friction coefficient of steel / iron-based composites under friction and wear conditions, thereby improving the friction and wear performance of the material. In summary, how to simultaneously introduce a uniformly distributed graphite lubrication phase and a hard ceramic enhancement phase into the iron matrix to prepare a ceramic particle-reinforced iron-based self-lubricating bulk material with excellent friction and wear performance is a key problem that needs to be solved urgently. Summary of the invention

[0004] The invention aims to provide a WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material, which has the characteristics of uniform distribution of WC ceramic particles and good friction and wear performance.

[0005] Another object of the present invention is to provide a method for preparing the above-mentioned bulk material.

[0006] The technical scheme adopted by the present invention is that WC ceramic particles reinforce the iron-based self-lubricating wear-resistant block material, the block material is formed by adding WC powder into molten iron, and the tissue composition of the material is that WC ceramic particles and spheroidal graphite are evenly distributed in the iron matrix; wherein the raw materials of the molten iron include scrap steel, primary iron, ferrosilicon, carburizer, inoculant and spheroidizer, which are composed of the following raw material components according to mass percentage: C: 3.4%-3.7%, Si: 2.4%-2.8%, Mn: ≤0.6%, S: ≤0.02%, P: ≤0.1%, Mg: 0.02%-0.04%, Re: 0.02%-0.04%, and the remainder is Fe and unavoidable impurities; the mass of the WC powder is 10%-40% of the total mass of the WC powder and the molten iron.

[0007] Another technical solution adopted by the present invention is a method for preparing a WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material, which is specifically implemented according to the following steps:

[0008] Step 1, weighing molten iron raw materials and WC powder, the molten iron raw materials include: scrap steel, raw iron, ferrosilicon, recarburizer, inoculant and spheroidizer, and then heating and melting the weighed scrap steel, raw iron, ferrosilicon and recarburizer into molten iron;

[0009] Step 2, pouring the molten iron into a ladle with a spheroidizing agent, an inoculant and iron filings on the bottom for spheroidizing and inoculating treatment;

[0010] Step 3, dispersing the cast WC powder through a sieve and adding it into the molten iron in step 2;

[0011] Step 4, quickly pouring the mixed melt of WC and molten iron obtained in step 3 into a crystallizer with a water-cooled graphite inner sleeve;

[0012] Step 5: retain the mixed melt in the crystallizer for 1 to 3 minutes, then quickly pull out the crystallizer and continue solidification, and after complete solidification, obtain a WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material.

[0013] Another technical solution of the present invention is also characterized in that:

[0014] The mass percentage of each element in the molten iron raw material in step 1 is: C: 3.4% to 3.7%, Si: 2.4% to 2.8%, Mn: ≤0.6%, S: ≤0.02%, P: ≤0.1%, Mg: 0.02% to 0.04%, Re: 0.02% to 0.04%, and the remainder is Fe and unavoidable impurities; and the mass of WC powder is 10% to 40% of the total mass of WC powder and molten iron raw material.

[0015] In step 1, the raw iron is breaded iron.

[0016] The heating and melting temperature in step 1 is 1570-1650° C., and the holding time is 2-4 minutes.

[0017] In step 1, the spheroidizing agent is Si-Mg-Ca-Re, which is composed of the following raw material components in mass percentage: Si: 43-47%, Mg: 5.7-6.1%, Ca: 2.5-2.8%, Re: 0.9-1.1%, and the balance is Fe and unavoidable impurities; the amount of the spheroidizing agent accounts for 1.0-1.2% of the total mass of the molten iron raw material.

[0018] In step 1, the inoculant is Si-Ba-Ca, which is composed of the following raw material components in terms of mass percentage: Si: 66-69%, Ba: 3.9-4.0%, Ca: 1.3-1.7%, and the remainder is Fe and unavoidable impurities; the amount of the inoculant accounts for 0.6-0.8% of the total mass of the molten iron raw material.

[0019] In step 2, the spheroidizer is laid at the bottom of the ladle, and is covered with inoculant and iron chips in turn.

[0020] In step 2, the temperature of the molten iron after spheroidizing and inoculation treatment is controlled at 1520-1580°C.

[0021] Step 3: During the process of adding WC powder into the molten iron, stirring should be continued, and the temperature of the mixed melt of WC ceramic particles and molten iron should be controlled at 1350-1400°C.

[0022] The beneficial effects of the present invention are:

[0023] (1) The method of the present invention first melts the iron raw material to form molten iron, and after spheroidization and inoculation treatment, WC powder is dispersed and added into the high-temperature molten iron through a screen. During the stirring process, since the WC ceramic particles are almost completely wetted by the molten iron, they are very easy to be evenly dispersed and react with the high-temperature molten iron to form a metallurgical bond. During the casting process, a crystallizer with a water-cooled graphite inner sleeve is used for rapid solidification. This method of rapid solidification in the liquid phase region with large supercooling effectively inhibits the downward aggregation of WC ceramic particles due to high density and gravity during the solidification process, thereby making the WC particles evenly distributed in the iron matrix block material, ensuring the anti-wear effect of the WC ceramic particles. In addition, the method of rapid solidification in the liquid phase region with large supercooling is also conducive to the precipitation of spheroidal graphite in the molten iron in a high-density dispersed distribution state, thereby ensuring the self-lubricating and friction-reducing effect of the spheroidal graphite. During the friction and wear process, the high-density dispersed spheroidal graphite precipitated from the iron matrix will form a graphite lubricating film on the friction interface, which plays a role in reducing friction, while the evenly distributed WC ceramic particles support and protect the iron matrix during the friction and wear process, so that the material has excellent friction and wear performance, and can be used as a component material under harsh friction and wear service conditions, and improve the working efficiency and life of the components;

[0024] (2) The method of the present invention adopts a stirring casting method combined with a large undercooling and rapid solidification method in the liquid phase to prepare a WC ceramic particle-reinforced iron-based self-lubricating wear-resistant block material with uniform structure, which solves the current problem of limited improvement in the friction and wear performance of single steel materials and the difficulty in preparing particle-reinforced iron-based block composite materials. The method is simple, easy to operate and has low production cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a flow chart of the preparation method of the present invention;

[0026] Figure 2 This is a scanning electron microscope image of the WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material prepared in Example 2 of the present invention;

[0027] Figure 3 This is a characterization of the wear surface morphology of the WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0028] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0029] The WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material of the invention is formed by adding WC powder into molten iron. The material has the structure of WC ceramic particles and spheroidal graphite uniformly distributed in the iron matrix. The raw materials of the molten iron include scrap steel, primary iron, ferrosilicon, a carburizer, an inoculant and a spheroidizer. The material is composed of the following raw material components according to mass percentage: C: 3.4%-3.7%, Si: 2.4%-2.8%, Mn: ≤0.6%, S: ≤0.02%, P: ≤0.1%, Mg: 0.02%-0.04%, Re: 0.02%-0.04%, and the balance is Fe and unavoidable impurities. In addition, the mass of the added WC powder is 10%-40% of the total mass of the WC powder and the molten iron.

[0030] The preparation method of the WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material of the present invention is as follows: Figure 1 As shown, the specific implementation steps are as follows:

[0031] Step 1: Melting of ingredients and raw materials:

[0032] According to the above raw material component composition, the raw materials are calculated, prepared and weighed, and the raw materials include: scrap steel, raw iron, ferrosilicon, carburizer, inoculant, spheroidizer and WC powder; then the weighed scrap steel, raw iron, ferrosilicon and carburizer are placed in a medium frequency induction furnace and heated to melt into molten iron.

[0033] Among them, the primary iron is bread iron, the smelting temperature is 1570-1650°C, and the holding time is 2-4 minutes.

[0034] The spheroidizing agent is Si-Mg-Ca-Re, which is composed of the following raw material components in percentage by mass: Si: 43-47%, Mg: 5.7-6.1%, Ca: 2.5-2.8%, Re: 0.9-1.1%, and the balance is Fe and unavoidable impurities; the amount of the spheroidizing agent accounts for 1.0-1.2% of the total mass of the molten iron, and ensures that the residual Mg content in the prepared block material is 0.02-0.04%.

[0035] The inoculant is Si-Ba-Ca, which is composed of the following raw material components according to mass percentage: Si: 66-69%, Ba: 3.9-4.0%, Ca: 1.3-1.7%, and the balance is Fe and inevitable impurities; the amount of the inoculant accounts for 0.6-0.8% of the total mass of the molten iron.

[0036] Step 2: Pour the molten iron obtained in step 1 into a ladle with a spheroidizing agent, an inoculant and iron filings at the bottom for spheroidization and inoculation treatment. After spheroidization and inoculation treatment, the temperature of the molten iron is controlled at 1520-1580°C.

[0037] Among them, the spheroidizer is laid at the bottom of the ladle, and is covered with inoculant and iron chips in turn.

[0038] Step 3, adding the cast WC powder to the molten iron in step 2 through a screen, and stirring while adding to make it evenly dispersed. During this process, the temperature of the mixed melt of WC ceramic particles and molten iron is controlled at 1350-1400° C.;

[0039] Step 4, quickly pouring the mixed melt of WC and molten iron obtained in step 3 into a crystallizer with a water-cooled graphite inner sleeve;

[0040] Step 5: retain the mixed melt of WC and molten iron in the crystallizer for 1 to 3 minutes, then quickly pull out the crystallizer and continue solidification, and after complete solidification, obtain a WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material.

[0041] Example 1

[0042] Step 1, the composition of the molten iron is C: 3.5%, Si: 2.4%, Mn: ≤0.3%, S: ≤0.02%, P: ≤0.1%, Mg: 0.02%, Re: 0.02%, and the balance is Fe and inevitable impurities; wherein, the amount of the spheroidizing agent accounts for 1.0% of the total mass of the molten iron, the composition of the spheroidizing agent is Si: 45%, Mg: 6%, Ca: 2.5%, Re: 1.0%, and the balance is Fe and inevitable impurities; the amount of the inoculant accounts for 0.6% of the total mass of the molten iron, the composition of the inoculant is Si: 66%, Ba: 4.0%, Ca: 1.5%, and the balance is Fe and inevitable impurities. The particle size of the WC powder is 80-100 μm, and its mass is 10% of the total mass of the WC powder and the molten iron.

[0043] According to the mass percentage, various raw materials are calculated, prepared and weighed: scrap steel, breaded iron, ferrosilicon, carburizer, inoculant, spheroidizer and WC powder; the weighed scrap steel, breaded iron, ferrosilicon and carburizer are placed in a medium frequency induction furnace, heated to 1570°C and kept warm for 3 minutes to melt them into molten iron.

[0044] Step 2: Pour the molten iron obtained in step 1 into a ladle with a spheroidizing agent, an inoculant and iron filings at the bottom for spheroidization and inoculation treatment. After spheroidization and inoculation treatment, the temperature of the molten iron is controlled at 1520°C.

[0045] Step 3: Add the WC powder to the molten iron in step 2 through a sieve, stirring while adding to make it evenly dispersed. During the process, the temperature of the mixed melt of the WC ceramic particles and the molten iron is controlled at 1400°C.

[0046] Step 4, quickly pouring the mixed melt of WC and molten iron obtained in step 3 into a crystallizer with a water-cooled graphite inner sleeve;

[0047] Step 5: retain the mixed melt of WC and molten iron in the crystallizer for 1 minute, then quickly pull out the crystallizer and continue solidification, and after complete solidification, obtain a WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material.

[0048] Example 2

[0049] Step 1, the composition of the molten iron is C: 3.6%, Si: 2.5%, Mn: ≤0.3%, S: ≤0.02%, P: ≤0.1%, Mg: 0.02%, Re: 0.03%, and the balance is Fe and inevitable impurities; wherein, the amount of the spheroidizing agent accounts for 1.2% of the total mass of the molten iron, the composition of the spheroidizing agent is Si: 43%, Mg: 6%, Ca: 2.5%, Re: 1.0%, and the balance is Fe and inevitable impurities; the amount of the inoculant accounts for 0.8% of the total mass of the molten iron, the composition of the inoculant is Si: 69%, Ba: 4.0%, Ca: 1.7%, and the balance is Fe and inevitable impurities. The particle size of the WC powder is 53-75 μm, and its mass is 20% of the total mass of the WC powder and the molten iron.

[0050] According to the mass percentage, various raw materials are calculated, prepared and weighed: scrap steel, breaded iron, ferrosilicon, carburizer, inoculant, spheroidizer and WC powder; the weighed scrap steel, breaded iron, ferrosilicon and carburizer are placed in a medium frequency induction furnace and heated to 1600° C. and kept warm for 3 minutes to melt them into molten iron.

[0051] Step 2: Pour the molten iron obtained in step 1 into a ladle with a spheroidizing agent, an inoculant and iron filings at the bottom for spheroidization and inoculation treatment. After spheroidization and inoculation treatment, the temperature of the molten iron is controlled at 1540°C.

[0052] Step 3: Add the WC powder to the molten iron in step 2 through a sieve, stirring while adding to make it evenly dispersed. During the process, the temperature of the mixed melt of the WC ceramic particles and the molten iron is controlled at 1390°C.

[0053] Step 4, quickly pouring the mixed melt of WC and molten iron obtained in step 3 into a crystallizer with a water-cooled graphite inner sleeve;

[0054] Step 5: retain the mixed melt of WC and molten iron in the crystallizer for 2 minutes, then quickly pull out the crystallizer and continue solidification, and after complete solidification, obtain a WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material.

[0055] like Figure 2 , which is a scanning electron microscope image of the bulk material prepared in this embodiment, it can be seen that this embodiment successfully prepared the WC ceramic particles and spherical graphite reinforced iron-based bulk material, and the WC ceramic particles and spherical graphite were evenly distributed in the iron matrix.

[0056] The friction and wear performance of the block material prepared in this example was tested under the following test conditions: load 20N, grinding time 40min, the friction coefficient of the material was measured to be 0.38, and the wear rate was 2×10 -6 mm 3 / N·m, the surface of the material after friction and wear is Figure 3 As shown, it can be seen that the WC particles play a good role in protecting and supporting the iron matrix, and the graphite plays a certain self-lubricating role. This result shows that the material has excellent friction and wear properties.

[0057] Example 3

[0058] Step 1, the composition of the molten iron is C: 3.7%, Si: 2.6%, Mn: ≤0.3%, S: ≤0.02%, P: ≤0.1%, Mg: 0.03%, Re: 0.04%, and the balance is Fe and inevitable impurities; wherein, the amount of the spheroidizing agent accounts for 1.0% of the total mass of the molten iron, the composition of the spheroidizing agent is Si: 47%, Mg: 6%, Ca: 2.8%, Re: 1.0%, and the balance is Fe and inevitable impurities; the amount of the inoculant accounts for 0.8% of the total mass of the molten iron, the composition of the inoculant is Si: 69%, Ba: 4.0%, Ca: 1.5%, and the balance is Fe and inevitable impurities. The particle size of the WC powder is 25-50μm, and its mass is 30% of the total mass of the WC powder and the molten iron.

[0059] According to the mass percentage, various raw materials are calculated, prepared and weighed: scrap steel, breaded iron, ferrosilicon, carburizer, inoculant, spheroidizer and WC powder; the weighed scrap steel, breaded iron, ferrosilicon and carburizer are placed in a medium frequency induction furnace, heated to 1620° C. and kept warm for 3 minutes to melt them into molten iron.

[0060] Step 2: Pour the molten iron obtained in step 1 into a ladle with a spheroidizing agent, an inoculant and iron filings at the bottom for spheroidization and inoculation treatment. After spheroidization and inoculation treatment, the temperature of the molten iron is controlled at 1560°C.

[0061] Step 3: Add the WC powder to the molten iron in step 2 through a sieve, stirring while adding to make it evenly dispersed. During the process, the temperature of the mixed melt of the WC ceramic particles and the molten iron is controlled at 1370°C.

[0062] Step 4, quickly pouring the mixed melt of WC and molten iron obtained in step 3 into a crystallizer with a water-cooled graphite inner sleeve;

[0063] Step 5: retain the mixed melt of WC and molten iron in the crystallizer for 2.5 minutes, then quickly pull out the crystallizer and continue solidification, and after complete solidification, obtain a WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material.

[0064] Example 4

[0065] Step 1, the composition of the molten iron is C: 3.6%, Si: 2.8%, Mn: ≤0.3%, S: ≤0.02%, P: ≤0.1%, Mg: 0.03%, Re: 0.03%, and the balance is Fe and inevitable impurities; wherein, the amount of the spheroidizing agent accounts for 1.0% of the total mass of the molten iron, the composition of the spheroidizing agent is Si: 45%, Mg: 6%, Ca: 2.5%, Re: 1.0%, and the balance is Fe and inevitable impurities; the amount of the inoculant accounts for 0.6% of the total mass of the molten iron, the composition of the inoculant is Si: 66%, Ba: 4.0%, Ca: 1.5%, and the balance is Fe and inevitable impurities. The particle size of the WC powder is 1-20 μm, and its mass is 40% of the total mass of the WC powder and the molten iron.

[0066] According to the mass percentage, various raw materials are calculated, prepared and weighed: scrap steel, breaded iron, ferrosilicon, carburizer, inoculant, spheroidizer and WC powder; the weighed scrap steel, breaded iron, ferrosilicon and carburizer are placed in a medium frequency induction furnace and heated to 1650° C. and kept warm for 3 minutes to melt them into molten iron.

[0067] Step 2: Pour the molten iron obtained in step 1 into a ladle with a spheroidizing agent, an inoculant and iron filings at the bottom for spheroidization and inoculation treatment. After spheroidization and inoculation treatment, the temperature of the molten iron is controlled at 1580°C.

[0068] Step 3: Add the WC powder to the molten iron in step 2 through a sieve, stirring while adding to make it evenly dispersed. During the process, the temperature of the mixed melt of the WC ceramic particles and the molten iron is controlled at 1350°C.

[0069] Step 4, quickly pouring the mixed melt of WC and molten iron obtained in step 3 into a crystallizer with a water-cooled graphite inner sleeve;

[0070] Step 5: retain the mixed melt of WC and molten iron in the crystallizer for 3 minutes, then quickly pull out the crystallizer and continue solidification, and after complete solidification, obtain a WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material.

[0071] The method of the present invention successfully introduces uniformly distributed spherical graphite self-lubricating phase and WC ceramic particle hard phase into the iron matrix through stirring casting and rapid solidification in large undercooling of liquid phase region with simple process and low production cost, and prepares WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material with uniform structure. The material has both self-lubricating and high wear-resistant properties, and can be used in harsh friction and wear service conditions to improve the working efficiency and life of parts.

Claims

1. WC ceramic particles reinforced iron-based self-lubricating wear-resistant block material, characterized in that: The material is formed by adding WC powder into molten iron, and the tissue composition of the material is that WC ceramic particles and spheroidal graphite are evenly distributed in the iron matrix; wherein the raw materials of the molten iron include scrap steel, primary iron, ferrosilicon, carburizer, inoculant and spheroidizer, and the molten iron is composed of the following raw material components in terms of mass percentage: C: 3.4% to 3.7%, Si: 2.4% to 2.8%, Mn: ≤0.6%, S: ≤0.02%, P: ≤0.1%, Mg: 0.02% to 0.04%, Re: 0.02% to 0.04%, and the remainder is Fe and unavoidable impurities; the mass of the WC powder is 10% to 40% of the total mass of the WC powder and the molten iron.

2. A method for preparing a WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material, characterized in that: Follow the steps below to implement it: Step 1, weighing molten iron raw materials and WC powder, the molten iron raw materials include: scrap steel, raw iron, ferrosilicon, recarburizer, inoculant and spheroidizer, and then heating and melting the weighed scrap steel, raw iron, ferrosilicon and recarburizer into molten iron; Step 2, pouring the molten iron into a ladle with a spheroidizing agent, an inoculant and iron filings on the bottom for spheroidizing and inoculating treatment; Step 3, dispersing the cast WC powder through a sieve and adding it into the molten iron in step 2; Step 4, quickly pouring the mixed melt of WC and molten iron obtained in step 3 into a crystallizer with a water-cooled graphite inner sleeve; Step 5: retain the mixed melt in the crystallizer for 1 to 3 minutes, then quickly pull out the crystallizer and continue solidification, and after complete solidification, obtain a WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material.

3. The method for preparing the WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material according to claim 2, characterized in that: The mass percentage of each element in the molten iron raw material in step 1 is: C: 3.4% to 3.7%, Si: 2.4% to 2.8%, Mn: ≤0.6%, S: ≤0.02%, P: ≤0.1%, Mg: 0.02% to 0.04%, Re: 0.02% to 0.04%, the remainder being Fe and unavoidable impurities; and the mass of the WC powder is 10% to 40% of the total mass of the WC powder and the molten iron raw material.

4. The method for preparing the WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material according to claim 2, characterized in that: In step 1, the raw iron is breaded iron.

5. The method for preparing the WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material according to claim 2, characterized in that: The heating and melting temperature in step 1 is 1570-1650° C., and the holding time is 2-4 minutes.

6. The method for preparing the WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material according to claim 2, characterized in that: In step 1, the spheroidizing agent is Si-Mg-Ca-Re, which is composed of the following raw material components in mass percentage: Si: 43-47%, Mg: 5.7-6.1%, Ca: 2.5-2.8%, Re: 0.9-1.1%, and the balance is Fe and unavoidable impurities; the amount of the spheroidizing agent accounts for 1.0-1.2% of the total mass of the molten iron raw material.

7. The method for preparing the WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material according to claim 2, characterized in that: In step 1, the inoculant is Si-Ba-Ca, which is composed of the following raw material components in terms of mass percentage: Si: 66-69%, Ba: 3.9-4.0%, Ca: 1.3-1.7%, and the remainder is Fe and unavoidable impurities; the amount of the inoculant accounts for 0.6-0.8% of the total mass of the molten iron raw material.

8. The method for preparing the WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material according to claim 2, characterized in that: In step 2, the spheroidizer is laid at the bottom of the ladle, and the inoculant and iron chips are covered on it in turn.

9. The method for preparing the WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material according to claim 2, characterized in that: In step 2, the temperature of the molten iron after spheroidizing and inoculating treatment is controlled at 1520-1580°C.

10. The WC ceramic particle reinforced iron-based self-lubricating wear-resistant block material according to claim 2 The preparation method is characterized in that Step 3: Stir continuously while adding WC powder to the molten iron. The temperature of the mixed melt of WC ceramic particles and molten iron is controlled at 1350-1400°C.

Citation Information

Patent Citations

  • Tungsten carbide ceramic particle / high-chromium cast iron composite wear-resistant lining plate and manufacturing method thereof

    CN104674108A

  • Ceramic particle reinforced iron-based composite material and preparing method and application thereof

    CN107904511A

  • Thermal-shock-fatigue-resistant glass mold iron profile and preparation method thereof

    CN113416886A

  • Preparation method of iron-based continuous casting profile based on graphite nodule ultra-fining

    CN113500171A

  • Steel / graphite composite profile and preparation method thereof

    CN115522132A