High-strength steel and production process thereof

Through rare earth treatment and electromagnetic stirring technology, the high-strength steel composition design and continuous casting billet quality problems are solved, its impact toughness and strength are improved, and the high-end use requirements of construction machinery are met.

CN118880194AActive Publication Date: 2024-11-01HUNAN VALIN LIANYUAN IRON & STEEL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410975704.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

High-strength steels above 960MPa grade are prone to cracking and fatigue cracking during processing, mainly due to unscientific composition design and poor quality of continuous casting billets.

Method used

Rare earth treatment technology and electromagnetic stirring technology are adopted to control the microstructure and quality of the casting billet by adding rare earth alloys to refine inclusions during RH refining, and rolling electromagnetic stirring and dynamic light pressure technology during continuous casting.

Benefits of technology

It significantly improves the impact toughness and strength of high-strength steel, ensures high quality of the finished product, reduces the brittleness of the material, and meets the use requirements of construction machinery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880194A_ABST
    Figure CN118880194A_ABST
Patent Text Reader

Abstract

The invention discloses high-strength steel and a production process thereof, and relates to the technical field of high-strength steel production. The high-strength steel comprises the following chemical components in percentage by mass: 0.17%-0.19% of C, 0.40%-0.50% of Si, 1.60%-1.90% of Mn, less than or equal to 0.010% of P, less than or equal to 0.0010% of S, 0.10%-0.30% of Ni, 0.25%-0.40% of Mo, 0.05%-0.06% of Nb, 0.045%-0.055% of V, 0.020%-0.030% of Ti, 0.30%-0.60% of Cr, 0.003%-0.004% of B, 0.020%-0.050% of Alt, 0.002%-0.005% of RE and 0.0030%-0.0040% of N. The high-strength steel is good in toughness and high in strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-strength steel production, in particular to a high-strength steel and a production process thereof. Background Art

[0002] High-strength steels above 960MPa play an important role in the manufacture of large-scale engineering machinery due to their good formability, welding performance and excellent low-temperature impact toughness. These engineering machinery need to withstand large workloads in complex and changing service environments, so the performance requirements of the steel substrate used are very strict. Among them, strength and toughness are the most critical performance indicators. The composition design of high-strength steel and the quality control of continuous casting billets are key factors in determining the basic performance of the material.

[0003] At present, in actual use, high-strength steels above 960MPa may encounter quality problems such as processing cracking and fatigue cracking. The deep-seated causes of these problems are often related to unscientific composition design and poor internal quality of continuous casting billets. In order to solve these problems, this patent proposes a rare earth treatment technology for the production of high-strength steels above 960MPa. In addition, a production process using electromagnetic stirring technology to improve the quality of continuous casting billets has been developed. These innovations significantly improve the impact toughness of high-strength steel and effectively solve the cracking problem during use. Summary of the invention

[0004] The present invention overcomes the technical problems of the prior art that the steel inclusions are relatively large in size and the quality of the casting is poor, thereby providing high-strength steel and a production process thereof, wherein the inclusions in the high-strength steel are small in size and the high-strength steel finally produced has good toughness and high strength.

[0005] The present invention solves the above technical problems through the following technical solutions.

[0006] The following percentage contents of the present invention are all mass percentage contents.

[0007] The invention provides a high-strength steel, comprising the following chemical components in mass percentage: C: 0.17-0.19%, Si: 0.40-0.50%, Mn: 1.60-1.90%, P≤0.010%, S≤0.0010%, Ni: 0.10-0.30%, Mo: 0.25-0.40%, Nb: 0.05-0.06%, V: 0.045-0.055%, Ti: 0.020-0.030%, Cr: 0.30-0.60%, B: 0.003-0.004%, Alt: 0.020-0.050%, RE: 0.002-0.005%, N: 0.0030-0.0040%.

[0008] In the present invention, the high-strength steel has a -60° transverse impact energy of 95-96 J.

[0009] In the present invention, the yield strength of the high-strength steel is 1357-1362 MPa.

[0010] In the present invention, the type B inclusions in the high-strength steel are ≤ level 1.0, such as level 0.5 or level 1.0.

[0011] In the present invention, the content of RE in the high-strength steel is 0.0025-0.0045wt%.

[0012] RE refers to a rare earth element. In the present invention, RE is La and Ce.

[0013] The present invention also provides a production process of high-strength steel, comprising the following steps:

[0014] S1. The molten iron is subjected to KR desulfurization, and then smelted in a converter and tapped to obtain molten steel;

[0015] S2. The molten steel is subjected to LF refining and RH refining, and the molten steel in the tundish is discharged;

[0016] Rare earth alloy is added during the RH refining process to make the rare earth content 20-50ppm, preferably 25-45ppm.

[0017] S3. The molten steel in the tundish is continuously cast to obtain ingots, which are then hot rolled to obtain high-strength steel.

[0018] In S1, the KR desulfurization makes the S content in the molten iron ≤ 0.001%.

[0019] In S1, the cleanliness of the desulfurized slag after KR desulfurization is ≥95%.

[0020] In S1, the temperature of the converter smelting is ≤1300°C.

[0021] In S1, the converter smelting adopts a double slag process or a slag pouring process before steel tapping.

[0022] In S1, the end point of the converter smelting is a P content ≤ 0.008%.

[0023] In S1, the end point of the converter smelting is an O content of 650-850 ppm.

[0024] In S1, after the steel is tapped, slag is first added to wash the steel, and then deoxidation and alloying are performed.

[0025] Further in S1, the slag washing material is lime; the amount of the slag washing material is 2.5-3.2 kg per ton of molten steel.

[0026] Further in S1, the alloy includes ferromanganese alloy, ferrosilicon alloy, ferrochrome alloy and aluminum block;

[0027] In S2, the LF refining includes the processes of adding aluminum for deoxidation, adding alloys for adjusting composition, making yellow-white slag for desulfurization and soft blowing.

[0028] Further in S2, the alloy includes ferromanganese alloy, ferrosilicon alloy, ferrochrome alloy, nickel alloy, ferromolybdenum alloy, ferroniobium alloy and ferrovanadium alloy.

[0029] Further in S2, lime and pre-melted slag are added to the yellow-white slag;

[0030] Among them, the amount of lime added to each ton of molten steel is 5-10kg;

[0031] The amount of pre-melted slag added per ton of molten steel is 0.5-2kg, preferably 0.7-1.3kg;

[0032] The components of the pre-melted slag include: CaO: 45-55%, Al2O3: 34-46%, SiO2≤5.0%, MgO≤6.0%, S≤0.15%, P≤0.05%, Fe2O3≤1.5%, H2O≤0.5%;

[0033] The particle size of the pre-melted slag is 5-40 mm.

[0034] Further in S2, the soft blowing time is 8-12 minutes.

[0035] In S2, the composition of the molten steel after LF refining is C: 0.17-0.19%, Si: 0.40-0.50%, Mn: 1.60-1.90%, P≤0.010%, S≤0.0010%, Ni: 0.10-0.30%, Mo: 0.25-0.40%, Nb: 0.05-0.06%, V: 0.045-0.055%, Cr: 0.30-0.60%, Alt: 0.020-0.050%, N: 0.0030-0.0060%, and the rest is iron and other inevitable impurities.

[0036] In S2, the tapping temperature after LF refining is 1605-1625°C.

[0037] In S2, the vacuum degree of the RH refining is ≤133Pa.

[0038] In S2, the cycle time of the RH refining is 20-25 minutes.

[0039] In S2, titanium-iron alloy and boron-iron alloy are added during the RH refining process, so that the molten steel in the RH refining process contains 0.020-0.030% Ti, 0.003-0.004% B and 0.0030-0.0040% N elements.

[0040] In S2, the rare earth alloy contains at least one of La and Ce; preferably, the rare earth alloy is a LaCe alloy; more preferably, the mass ratio of La to Ce in the rare earth alloy is 1:2;

[0041] The purity of the rare earth alloy is ≥99%.

[0042] The present invention adopts rare earth micro-treatment technology, that is, in the middle and late stages of RH (vacuum degassing) refining, a certain amount of rare earth alloy is added to the molten steel. This treatment method can effectively refine the inclusions in the steel, thereby significantly improving the microstructure of the steel, and effectively controlling the content and size of the inclusions. This lower inclusion rating is crucial to improving the impact toughness of the finished steel, because the refinement and uniform distribution of inclusions help reduce the brittleness of the material, thereby enhancing its mechanical properties.

[0043] In S2, the RH refining process before leaving the station also includes soft blowing and post-air breaking calming processes;

[0044] The soft blowing time is 6-15 minutes; the sedation time is 15-35 minutes.

[0045] In S3, the continuous casting casting machine controls the centering of the sector segments and the roll gap to be less than ±0.5 mm.

[0046] In S3, the superheat degree of the molten steel in the tundish during the continuous casting process is 25-45°C.

[0047] In S3, the continuous casting is operated at a constant casting speed.

[0048] In S3, the continuous casting speed is 1.0-1.2 m / min.

[0049] In S3, the continuous casting adopts three-stage dynamic soft reduction, and the total reduction is ≥6mm, preferably 6-8mm.

[0050] In the present invention, strict regulations are made on the state, superheat and pulling speed of the continuous casting machine, which are key factors to ensure high quality of low-multiple cast billets. In addition, the roller electromagnetic stirring and dynamic soft pressure reduction technology used in the continuous casting process further significantly improve the overall quality of the cast billets.

[0051] In S3, the continuous casting adopts roller electromagnetic stirring, and the current is controlled at 450-550A.

[0052] In S3, the central segregation of the ingot after continuous casting is ≤1.0 level.

[0053] In S3, the central porosity of the ingot after continuous casting is ≤ level 1.0.

[0054] In S3, the continuous casting billet has no intermediate cracks.

[0055] In S3, the hot rolling is performed through 5-7 rough rolling passes and 7 finish rolling passes.

[0056] In S3, the hot rolling speed is 10-14 m / min.

[0057] In S3, the hot rolling furnace temperature is 1250-1270°C.

[0058] In S3, the hot rolling finishing inlet temperature is 1100°C-1150°C.

[0059] In S3, the final rolling temperature of the hot rolling is 880-910°C.

[0060] In S3, the coiling temperature of the hot rolling is 550-580°C.

[0061] In the alloy used in the present invention, the Mn content in the ferromanganese alloy is ≥80%, the C content is ≤0.7%, and the rest is Fe and unavoidable impurities;

[0062] The Si content in the ferrosilicon alloy is 72%-80%, and the rest is Fe and inevitable impurities;

[0063] The ferrochrome alloy has a Cr content of 52%-60%, a C content of ≤0.2%, and the remainder being Fe and unavoidable impurities;

[0064] The iron-titanium alloy contains 68-72% Ti, and the rest is Fe and unavoidable impurities;

[0065] In the ferroboron alloy, B>19%, and the rest is Fe and unavoidable impurities;

[0066] The nickel alloy contains 45-50% Ni, ≤14% Si, and the rest is Fe and unavoidable impurities;

[0067] The molybdenum-iron alloy contains 60-65% Mo, ≤2% Si, and the rest is Fe and unavoidable impurities;

[0068] The ferroniobium alloy contains 63-65% Nb, ≤5% Si, and the rest Fe and unavoidable impurities;

[0069] The ferrovanadium alloy contains 50-55% Nb, ≤2.5% Si, ≤2.0% Al, and the rest is Fe and unavoidable impurities;

[0070] The Al content in the aluminum block is >99.4%, and the rest are inevitable impurities.

[0071] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0072] Compared with the prior art, the present invention has the following beneficial effects:

[0073] 1. The composition design of the high-strength steel of the present invention is a prerequisite for ensuring the strength and stability of the high-strength steel. RH refining completes the rare earth micro-treatment of the molten steel by adding a certain amount of rare earth alloy, refines the inclusions in the steel, and controls the Class B inclusions of the high-strength steel to below level 1.0, which helps to improve the impact toughness of the finished product.

[0074] 2. In the present invention, the state of the continuous casting machine, the degree of superheat and the casting speed are the key factors to ensure high quality of the ingot with low multiples. In addition, the roller electromagnetic stirring and dynamic soft pressure reduction technology used in the continuous casting process further significantly improve the overall quality of the ingot.

[0075] 3. The -60° transverse impact energy of the high-strength steel of the present invention is 95-96 J, and the yield strength of the high-strength steel is 1357-1362 MPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0076] Figure 1 This is the electron microscope energy spectrum of rare earth inclusions in the high-strength steel in Example 1.

[0077] Figure 2 This is the inclusion morphology of Comparative Example 1. DETAILED DESCRIPTION

[0078] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully in combination with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.

[0079] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0080] "Scope" disclosed in the present invention is defined in the form of lower limit and upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a particular range. The scope defined in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a particular parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3,4 and 5 are listed, the following scope can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present invention, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0081] If not otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form a new technical solution.

[0082] Unless otherwise specified, all technical features and optional technical features of the present invention can be combined with each other to form a new technical solution.

[0083] If not otherwise specified, all steps of the present invention may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0084] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0085] If not specifically stated, in the present invention, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0086] The alloys used in the following examples and comparative examples are as follows:

[0087] Ferromanganese alloy: Grade FeMn84C0.7, Mn content is 84%, C content is 0.7%, and the rest is Fe and unavoidable impurities;

[0088] Ferrosilicon alloy: grade FeSi75, Si content is 75%, the rest is Fe and unavoidable impurities);

[0089] Ferrochrome alloy: Grade FeCr55C2.0, Cr content 55%, C content ≤ 0.2%, the rest is Fe and unavoidable impurities

[0090] Titanium-iron alloy: grade 70TiFe, Ti content 68%-72%, the rest is Fe and unavoidable impurities);

[0091] Boron-iron alloy: Grade 19BFe, B content> 19%, the rest is Fe and unavoidable impurities;

[0092] The nickel alloy contains 45-50% Ni, ≤14% Si, and the rest is Fe and unavoidable impurities;

[0093] The molybdenum-iron alloy contains 60-65% Mo, ≤2% Si, and the rest is Fe and unavoidable impurities;

[0094] The ferroniobium alloy contains 63-65% Nb, ≤5% Si, and the rest is Fe and unavoidable impurities;

[0095] The ferrovanadium alloy contains 50-55% Nb, ≤2.5% Si, ≤2.0% Al, and the rest is Fe and unavoidable impurities;

[0096] Aluminum block: Al content is 99.6%, and the rest are inevitable impurities;

[0097] Rare earth alloy: LaCe alloy, the mass ratio of La to Ce is 1:2, and the purity is 99.5%.

[0098] The inclusion testing method of high-strength steel in the following examples and comparative examples refers to GB / T10561.

[0099] Example 1

[0100] 1. High-strength steel

[0101] High-strength steel is composed of the following chemical components in mass percentage: C: 0.18%, Si: 0.45%, Mn: 1.74%, P: 0.007%, S: 0.0008%, Ni: 0.20%, Mo: 0.32%, Nb: 0.054%, V: 0.049%, Cr: 0.44%, Alt: 0.031%, Ti: 0.028%, B: 0.0035%, N: 0.0035%, RE: 0.0039%, and the rest are iron and other inevitable impurities.

[0102] The transverse impact energy of high-strength steel at -60° is 95J.

[0103] The yield strength of high-strength steel is 1362MPa.

[0104] There are no slender MnS inclusions in high-strength steel, and the type B inclusions in high-strength steel are level 1.0.

[0105] The high-strength steel of this embodiment meets the use requirements of various types of engineering machinery.

[0106] 2. Production process of high-strength steel

[0107] The production process of high-strength steel includes the following steps:

[0108] S1. The molten iron is subjected to KR desulfurization, and then smelted in a converter and tapped to obtain molten steel;

[0109] S2. The molten steel is subjected to LF refining and RH refining, and the molten steel in the tundish is discharged;

[0110] S3. The molten steel in the tundish is continuously cast to obtain ingots, which are then hot rolled to obtain high-strength steel.

[0111] In the present embodiment S1, the KR desulfurization makes the S content in the molten iron to be 0.0008%.

[0112] In this embodiment S1, the degree of cleanliness of the desulfurized slag after KR desulfurization is 97%.

[0113] In this embodiment S1, the temperature of the converter smelting is 1274°C.

[0114] In the present embodiment S1, the converter smelting adopts a double slag process.

[0115] In the present embodiment S1, the endpoint P content of the converter smelting is 0.006%, and the O content is 721 ppm.

[0116] In this embodiment S1, the amount of steel produced is 205t.

[0117] In the present embodiment S1, after the steel is tapped, 600 kg of lime is first added to wash the slag, and then deoxidation and alloying are performed; the alloys used for deoxidation and alloying are ferromanganese alloy, ferrosilicon alloy, ferrochrome alloy and aluminum block.

[0118] In this embodiment S2, the LF refining includes the processes of making yellow-white slag, deep desulfurization and soft blowing;

[0119] Furthermore, 1400kg of lime and 300kg of pre-melted slag are required to make yellow and white slag; the components of the pre-melted slag include: CaO: 46%, Al2O3: 41%, SiO2: 3.2%, MgO: 5.3%, S: 0.08%, P: 0.02%, Fe2O3: 1.3%, H2O: 0.2%; the particle size of the pre-melted slag is 25mm.

[0120] Furthermore, the soft blowing time is 10 minutes.

[0121] In the present embodiment S2, the temperature of the molten steel discharged from the LF refining station is 1618°C.

[0122] In this embodiment S2, the composition of the LF refined molten steel is C: 0.181%, Si: 0.47%, Mn: 1.72%, P: 0.006%, S: 0.0008%, Ni: 0.19%, Mo: 0.29%, Nb: 0.055%, V: 0.051%, Cr: 0.40%, Alt: 0.038%, N: 0.0052%, and the rest is iron and other inevitable impurities.

[0123] In this embodiment S2, the vacuum degree of the RH refining is 10-100Pa.

[0124] In the present embodiment S2, titanium-iron alloy and boron-iron alloy are added during the RH refining process, so that the Ti content, B content and N content of the RH outgoing molten steel are 0.028%, 0.0035% and 0.0035%, respectively.

[0125] In the present embodiment S2, 25 kg of LaCe rare earth alloy is added during the RH refining process, so that the sum of the contents of La and Ce in the RH outlet molten steel is 39 ppm.

[0126] In this embodiment S2, the cycle time of the RH refining is 22 minutes.

[0127] In the present embodiment S2, the soft blowing time after RH refining is 8 minutes.

[0128] In the present embodiment S2, the sedation time after the RH refining and breaking air is 25 minutes.

[0129] In this embodiment S3, the continuous casting needs to check the casting machine status 3 days before use, and the continuous casting casting machine controls the centering of the sector and the roll gap to be less than ±0.5 mm.

[0130] In the present embodiment S3, the superheat degree of the molten steel in the tundish during the continuous casting process is 38°C.

[0131] In this embodiment S3, the continuous casting speed is 1.0-1.2 m / min.

[0132] In the present embodiment S3, the continuous casting adopts three-stage dynamic soft reduction, and the total reduction is 7 mm.

[0133] In the present embodiment S3, the continuous casting adopts roller electromagnetic stirring, and the current is controlled at 510A.

[0134] In the present embodiment S3, the stopper rod position of the continuous casting does not rise, and continuous casting of 15 furnaces in a single pouring can be achieved.

[0135] In this embodiment S3, the ingot after continuous casting has a center segregation of 0.5 level, a center porosity of 0.5 level, and no intermediate cracks.

[0136] In the present embodiment S3, the hot rolling is performed through 7 rough rolling passes and 7 finish rolling passes.

[0137] In this embodiment S3, the hot rolling speed is 10-14 m / min.

[0138] In this embodiment S3, the hot rolled slab has a furnace discharge temperature of 1260°C, a finishing rolling inlet temperature of 1130°C, a final rolling temperature of 895°C, and a coiling temperature of 570°C.

[0139] Example 2

[0140] The difference between this embodiment and embodiment 1 is that:

[0141] 1. High-strength steel

[0142] High-strength steel is composed of the following chemical components in mass percentage: C: 0.185%, Si: 0.48%, Mn: 1.83%, P: 0.008%, S: 0.0007%, Ni: 0.21%, Mo: 0.31%, Nb: 0.054%, V: 0.050%, Cr: 0.45%, Alt: 0.035%, Ti: 0.025%, B: 0.0034%, N: 0.0037%, RE: 0.0035%, and the rest are iron and other inevitable impurities.

[0143] The transverse impact energy of high-strength steel at -60° is 96J.

[0144] The yield strength of high-strength steel is 1357MPa.

[0145] There are no slender MnS inclusions in high-strength steel, and the type B inclusions in high-strength steel are level 0.5.

[0146] The high-strength steel of this embodiment meets the use requirements of various types of engineering machinery.

[0147] 2. Production process of high-strength steel

[0148] In the present embodiment S1, the KR desulfurization makes the S content in the molten iron to be 0.0005%.

[0149] In the present embodiment S1, the final P content of the converter smelting is 0.008%, and the O content is 685 ppm.

[0150] In this embodiment S1, the amount of steel produced is 204t.

[0151] In this embodiment S2, the composition of the LF refined molten steel is C: 0.185%, Si: 0.48%, Mn: 1.83%, P: 0.008%, S: 0.0007%, Ni: 0.21%, Mo: 0.31%, Nb: 0.054%, V: 0.050%, Cr: 0.45%, Alt: 0.035%, N: 0.0056%, and the rest is iron and other inevitable impurities.

[0152] In the present embodiment S2, the temperature of the molten steel discharged from the LF refining station is 1615°C.

[0153] In the present embodiment S2, titanium-iron alloy and boron-iron alloy are added during the RH refining process, so that the Ti content, B content and N content of the RH outlet molten steel are 0.025%, 0.0034% and 0.0037%, respectively.

[0154] In the present embodiment S2, 25 kg of LaCe rare earth alloy is added during the RH refining process, so that the sum of the contents of La and Ce in the RH outlet molten steel is 35 ppm.

[0155] In the present embodiment S2, the sedation time after the RH refining and breaking air is 24 minutes.

[0156] In the present embodiment S3, the superheat degree of the molten steel in the tundish during the continuous casting process is 35°C.

[0157] Comparative Example 1

[0158] In this comparative example, no rare earth alloy was added during the RH refining process.

[0159] The difference between this comparative example and Example 1 is:

[0160] 1. High-strength steel

[0161] High-strength steel is composed of the following chemical components in mass percentage: C: 0.185%, Si: 0.48%, Mn: 1.83%, P: 0.014%, S: 0.0035%, Ni: 0.21%, Mo: 0.31%, Nb: 0.062%, V: 0.056%, Cr: 0.45%, Alt: 0.035%, Ti: 0.031%, B: 0.0028%, N: 0.0038%, and the rest are iron and other inevitable impurities.

[0162] The transverse impact energy of high-strength steel at -60° is 55J.

[0163] The yield strength of high-strength steel is 971MPa.

[0164] There are a small amount of slender MnS inclusions in high-strength steel. The Class B inclusions in high-strength steel are 1.5, and the inclusion morphology is as follows: Figure 2 shown.

[0165] The high-strength steel in this comparative example cannot meet the use requirements of high-end engineering machinery.

[0166] 2. Production process of high-strength steel

[0167] In this comparative example S1, the KR desulfurization makes the S content in the molten iron reach 0.0005%.

[0168] In this comparative example S1, the temperature of the converter smelting is 1264°C.

[0169] In this comparative example S1, the final P content of the converter smelting is 0.015%, and the O content is 685 ppm.

[0170] In this comparative example S1, the amount of steel produced is 204t.

[0171] In this comparative example S2, the composition of the LF refined molten steel is C: 0.185%, Si: 0.48%, Mn: 1.83%, P: 0.014%, S: 0.0035%, Ni: 0.21%, Mo: 0.31%, Nb: 0.062%, V: 0.056%, Cr: 0.45%, Alt: 0.035%, N: 0.0056%, and the rest is iron and other inevitable impurities.

[0172] In this comparative example S2, the temperature of the molten steel discharged from the LF refining station is 1615°C

[0173] In comparative example S2, titanium-iron alloy and boron-iron alloy are added during the RH refining process, so that the content of Ti, B and N in the RH outlet molten steel is 0.031%, 0.0028% and 0.0038%.

[0174] In this comparative example S2, no rare earth alloy is added during the RH refining process.

[0175] In this comparative example S2, the sedation time after the RH refining and breaking air is 24 minutes.

[0176] Comparative Example 2

[0177] The difference between this comparative example and Example 2 is that:

[0178] 1. High-strength steel

[0179] High-strength steel is composed of the following chemical components in mass percentage: C: 0.18%, Si: 0.45%, Mn: 1.74%, P: 0.007%, S: 0.0008%, Ni: 0.20%, Mo: 0.32%, Nb: 0.054%, V: 0.049%, Cr: 0.44%, Alt: 0.031%, Ti: 0.028%, B: 0.0035%, N: 0.0035%, RE: 0.0101%, and the rest are iron and other inevitable impurities.

[0180] The transverse impact energy of high-strength steel at -60° is 92J.

[0181] The yield strength of high-strength steel is 1128MPa.

[0182] There are no slender MnS inclusions in high-strength steel, and the type B inclusions in high-strength steel are level 0.5.

[0183] 2. Production process of high-strength steel

[0184] In this comparative example S2, 75 kg of LaCe rare earth alloy was added during the RH refining process, so that the sum of the contents of La and Ce in the RH outlet molten steel was 101 ppm.

[0185] In the comparative example S3, the stopper rod position of the continuous casting was raised by 18 mm, and the production was interrupted after continuous casting of 2 furnaces.

[0186] Comparative Example 3

[0187] The difference between this comparative example and Example 1 is:

[0188] 1. High-strength steel

[0189] High-strength steel is composed of the following chemical components in mass percentage: C: 0.185%, Si: 0.48%, Mn: 1.83%, P: 0.008%, S: 0.0007%, Ni: 0.21%, Mo: 0.31%, Nb: 0.054%, V: 0.050%, Cr: 0.45%, Alt: 0.035%, Ti: 0.025%, B: 0.0034%, N: 0.0037%, RE: 0.0039%, and the rest are iron and other inevitable impurities.

[0190] The transverse impact energy of high-strength steel at -60° is 84J.

[0191] The yield strength of high-strength steel is 965MPa.

[0192] There are no slender MnS inclusions in high-strength steel, and the type B inclusions in high-strength steel are level 1.0.

[0193] 2. Production process of high-strength steel

[0194] In this comparative example S3, the superheat degree of the molten steel in the tundish is 38°C.

[0195] In this comparative example S3, the continuous casting speed is 1.3 m / min.

[0196] In this comparative example S3, the casting machine controls the centering of the sector and the roll gap to be within ±1.0 mm.

[0197] In this comparative example S3, the continuous casting adopts a three-stage dynamic soft reduction, with a total reduction of 4 mm.

[0198] In comparative example S3, the continuous casting adopts roller electromagnetic stirring, and the current is controlled at 500A.

[0199] In the comparative example S3, the ingot after continuous casting has a center segregation of 1.5, a center porosity of 1.0, and a small amount of middle cracks.

[0200] In the above-mentioned embodiments and comparative examples, Examples 1 and 2 both use rare earth micro-processing to refine the inclusions in the steel, so that the Class B inclusions of the high-strength steel are controlled at level 0.5 and level 1.0. In Comparative Example 1, no rare earth alloy is added, resulting in Class B inclusions in the high-strength steel being level 1.5, and the presence of a small amount of slender MnS inclusions. In Comparative Example 2, the rare earth content is high, but the castability of the molten steel is poor, and the production is interrupted after two continuous castings. The continuous casting process puts forward specific requirements on the casting machine state, superheat and pulling speed, which lays the basic guarantee conditions for the low-multiple quality of the ingot after continuous casting. Therefore, the quality of the ingot obtained in Comparative Example 3 is poor.

[0201] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods. The specific embodiments described above further describe the purpose, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A high-strength steel, characterized in that: Contains the following chemical components in mass percentage: C: 0.17-0.19%, Si: 0.40-0.50%, Mn: 1.60-1.90%, P≤0.010%, S≤0.0010%, Ni: 0.10-0.30%, Mo: 0.25-0.40%, Nb: 0.05-0.06%, V: 0.045-0.055%, Ti: 0.020-0.030%, Cr: 0.30-0.60%, B: 0.003-0.004%, Alt: 0.020-0.050%, RE: 0.002-0.005%, N: 0.0030-0.0040%.

2. The high-strength steel according to claim 1, characterized in that: Satisfy at least one of the following conditions (1)-(3): (1) The transverse impact energy of the high-strength steel at -60° is 95-96 J; (2) The yield strength of the high-strength steel is 1357-1362 MPa; (3) The Class B inclusions in the high-strength steel are ≤ Grade 1.

0.

3. The production process of high-strength steel according to claim 1 or 2, characterized in that: The following steps are involved: S1. The molten iron is subjected to KR desulfurization, and then smelted in a converter and tapped to obtain molten steel; S2. The molten steel is subjected to LF refining and RH refining, and the molten steel in the tundish is discharged; Rare earth alloy is added during the RH refining process to make the rare earth content 20-50ppm; S3. The molten steel in the tundish is continuously cast to obtain ingots, which are then hot rolled to obtain high-strength steel.

4. The production process of high-strength steel according to claim 3, characterized in that: The S1 satisfies at least one of the following conditions (1)-(5): (1) the KR desulfurization makes the sulfur content in the molten iron ≤ 0.001%; (2) The temperature of the converter smelting is ≤1300°C; (3) The end point of the converter smelting is a P content of ≤0.008%; (4) The end point of the converter smelting is an O content of 650-850 ppm; (5) After the steel is tapped, slag is first added to wash the steel, and then deoxidation and alloying are performed; wherein the alloy includes ferromanganese alloy, ferrosilicon alloy, ferrochrome alloy and aluminum block.

5. The production process of high-strength steel according to claim 3, characterized in that: The LF refining satisfies at least one of the following conditions (1)-(3): (1) The LF refining includes the processes of adding aluminum for deoxidation, adding alloy for adjusting composition, making yellow-white slag for desulfurization and soft blowing; (2) The composition of the molten steel after LF refining is C: 0.17-0.19%, Si: 0.40-0.50%, Mn: 1.60-1.90%, P≤0.010%, S≤0.0010%, Ni: 0.10-0.30%, Mo: 0.25-0.40%, Nb: 0.05-0.06%, V: 0.045-0.055%, Cr: 0.30-0.60%, Alt: 0.020-0.050%, N: 0.0030-0.0060%, and the rest is iron and other inevitable impurities; (3) The tapping temperature after LF refining is 1605-1625°C.

6. The production process of high-strength steel according to claim 5, characterized in that: The LF refining satisfies at least one of the following conditions (1)-(3): (1) The alloys include ferromanganese alloys, ferrosilicon alloys, ferrochrome alloys, nickel alloys, ferromolybdenum alloys, ferroniobium alloys and ferrovanadium alloys; (2) The yellow-white slag needs to be added with lime and pre-melted slag; Among them, the amount of pre-melted slag added to each ton of molten steel is 0.5-2kg; The components of the pre-melted slag include: CaO: 45-55%, Al2O3: 34-46%, SiO2≤5.0%, MgO≤6.0%, S≤0.15%, P≤0.05%, Fe2O3≤1.5%, H2O≤0.5%; (3) The soft blowing time is 8-12 minutes.

7. The production process of high-strength steel according to claim 3, characterized in that: The RH refining satisfies at least one of the following conditions (1)-(5): (1) The vacuum degree of the RH refining is ≤133Pa; (2) The RH refining cycle time is 20-25 min; (3) titanium-iron alloy and boron-iron alloy are added during the RH refining process, so that the molten steel in the RH refining process contains 0.020-0.030% Ti, 0.003-0.004% B and 0.0030-0.0040% N elements; (4) RH refining also includes soft blowing and post-air sedation processes before leaving the station (5) The rare earth alloy contains at least one of La and Ce.

8. The production process of high-strength steel according to claim 7, characterized in that: The RH refining satisfies at least one of the following conditions (1)-(3): (1) The rare earth alloy is LaCe alloy; (2) The soft blowing time is 6-15 minutes; (3) The sedation time is 15-35 minutes.

9. The production process of high-strength steel according to claim 3, characterized in that: The continuous casting satisfies at least one of the following conditions (1)-(7): (1) The continuous casting casting machine controls the centering of the sector and the roll gap to be less than ±0.5 mm; (2) The superheat of the molten steel in the tundish during the continuous casting process is 25-45° C.; (3) The continuous casting speed is 1.0-1.2 m / min; (4) The continuous casting adopts three-stage dynamic soft reduction, and the total reduction is ≥6mm; (5) The continuous casting adopts roller electromagnetic stirring, and the current is controlled at 450-550A; (6) The center segregation of the ingot after continuous casting is ≤1.0 level; (7) The central porosity of the ingot after continuous casting is ≤1.0 level.

10. The production process of high-strength steel according to claim 3, characterized in that: The hot rolling satisfies at least one of the following conditions (1)-(6): (1) The hot rolling is performed through 5-7 rough rolling passes and 7 finish rolling passes; (2) The hot rolling speed is 10-14 m / min; (3) The hot rolling furnace temperature is 1250-1270°C; (4) the hot rolling finishing inlet temperature is 1100° C.-1150° C.; (5) The final rolling temperature of the hot rolling is 880-910°C; (6) The coiling temperature of the hot rolling is 550-580°C.

Citation Information

Patent Citations

  • REOMT method for improving impact toughness of steel for S355ML flange

    CN112143955A

  • Small-compression-bit thick quenched and tempered steel plate and production method thereof

    CN117926105A

  • Gpa-grade bainite steel having ultra-high yield ratio and manufacturing method for gpa-grade bainite steel

    US20230357882A1

  • High-strength steel sheet and method for producing same

    WO2011142356A1