Nickel oxide-based target material as well as preparation method and application thereof
By incorporating strontium oxide into nickel oxide targets, its sinterability and density are improved, solving the problem of high-quality preparation of nickel oxide targets and enhancing the performance of NiOx thin films, making them suitable for hole transport layers in perovskite solar cells.
Patent Information
- Application Number
- CN202410898224.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-05
AI Technical Summary
Existing technologies make it difficult to prepare high-density nickel oxide targets, leading to nodules and defects during magnetron sputtering. Furthermore, nickel oxide has low sintering activity, making it difficult to prepare high-quality NiOx films.
High-quality nickel oxide-based targets were prepared by using strontium oxide as a dopant and mixing it with nickel oxide powder, ball milling, spray granulation, molding, cold isostatic pressing, and sintering.
It improves the sinterability and density of nickel oxide targets, reduces the resistivity and roughness of thin films, and enhances the performance of NiOx thin films, making them suitable for hole transport layers in perovskite solar cells.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal target materials, and in particular to a nickel oxide-based target material and a preparation method and application thereof. Background Art
[0002] Magnetron sputtering is the main process for mass production of NiOx thin films, as it is easy to produce on an industrial scale and the deposited films have excellent and stable properties. As the raw material for magnetron sputtering, a good nickel oxide target needs to have high density and uniform fine grains to avoid nodules and defects generated during magnetron sputtering. However, nickel oxide itself has low sintering activity, which makes it difficult to sinter and prepare high-density nickel oxide targets.
[0003] Therefore, it is necessary to develop a nickel oxide-based target that can improve the sintering performance and target quality. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the first aspect of the present invention provides a nickel oxide-based target material, which can effectively improve the sintering property and target density of the nickel oxide target material and improve the performance of the nickel oxide-based film.
[0005] The second aspect of the present invention also provides a method for preparing a nickel oxide-based target material.
[0006] The third aspect of the present invention also provides an application of a nickel oxide-based target material.
[0007] The nickel oxide-based target material provided in the embodiment according to the first aspect of the present invention comprises nickel oxide and strontium oxide. The strontium oxide accounts for 0.1% to 20% of the total mass of the nickel oxide-based target material.
[0008] The nickel oxide-based target material according to the embodiment of the present invention has at least the following beneficial effects:
[0009] The present invention adopts strontium oxide as a dopant for the nickel oxide-based target material. The introduction of strontium oxide can not only improve the sintering property and target quality of the nickel oxide target material, but also improve the performance of the NiOx film, so that it can be applied to the hole transport layer of the perovskite battery.
[0010] This is because the strontium oxide of the present invention can produce a eutectic reaction with nickel oxide to improve its sintering activity and improve the quality of the target material. In addition, it can reduce the resistivity and roughness of the nickel oxide film, thereby improving the efficiency of the perovskite solar cell.
[0011] According to some embodiments of the present invention, the strontium oxide accounts for 1% to 20% of the total mass. It includes all values from 1% to 20% and sub-ranges thereof, such as 1%, 5%, 10%, 15%, 20% or a subset consisting of any two thereof. Thus, within the above range, the quality of the nickel oxide film prepared by the target material is better.
[0012] According to some embodiments of the present invention, the strontium oxide accounts for 3% to 5% of the total mass. Therefore, when the strontium oxide content is within the above range, the nickel oxide film prepared therefrom has lower resistivity and lower roughness.
[0013] According to a second aspect of the present invention, a method for preparing a nickel oxide-based target material is provided, comprising the following steps:
[0014] S1, mixing nickel oxide powder and strontium oxide powder, ball milling and spray granulation to obtain powder particles;
[0015] S2, molding the powder particles, and obtaining a green target material by cold isostatic pressing;
[0016] S3, sintering the green target material.
[0017] According to some embodiments of the present invention, the compression molding pressure is 0.1 MPa to 0.8 MPa.
[0018] According to some embodiments of the present invention, the cold isostatic pressing pressure is 200 MPa to 250 MPa.
[0019] According to some embodiments of the present invention, the sintering steps are as follows:
[0020] The temperature is raised to 500-750°C for insulation I, and then raised to 1400-1700°C for insulation II.
[0021] According to some embodiments of the present invention, the insulation time I is 20 hours to 30 hours.
[0022] According to some embodiments of the present invention, the insulation II time is 24 to 48 hours.
[0023] According to some embodiments of the present invention, the sintering is performed in an oxygen atmosphere.
[0024] The third aspect of the present invention provides an application of the nickel oxide-based target material in the preparation of optical semiconductor devices.
[0025] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. DETAILED DESCRIPTION
[0026] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.
[0027] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0028] Nickel oxide and strontium oxide: Powder purity required is 4N, particle size is less than 100nm; commercially available.
[0029] Example 1
[0030] This example provides a nickel oxide-based target material, and its component dosage and preparation method are as follows:
[0031] Pure water was added to 5 parts of strontium oxide and 95 parts of nickel oxide powder, and then ball milled and mixed, and then spray granulated to obtain spherical particles. Then 0.5MPa compression molding was performed, and 230MPa cold isostatic pressing was performed to obtain a blank target. Finally, the temperature was raised from room temperature to 600℃ at a rate of 2℃ / min in an oxygen atmosphere for 24h, and then the temperature was raised to 1500℃ at a rate of 5℃ / min for 36h. Natural cooling to room temperature obtained a strontium-doped nickel oxide-based target.
[0032] Example 2
[0033] This example provides a nickel oxide-based target material, and its component dosage and preparation method are as follows:
[0034] Pure water was added to 5 parts of strontium oxide and 95 parts of nickel oxide powder, and then ball milled and spray granulated to obtain spherical particles. Then 0.1MPa compression molding was performed and 200MPa cold isostatic pressing was performed to obtain a green blank target. Finally, the temperature was raised from room temperature to 500℃ at a rate of 2℃ / min and kept for 24h in an oxygen atmosphere, and then the temperature was raised to 1500℃ at a rate of 5℃ / min and kept for 24h. Natural cooling to room temperature obtained a strontium-doped nickel oxide target.
[0035] Example 3
[0036] This example provides a nickel oxide-based target material, and its component dosage and preparation method are as follows:
[0037] Pure water was added to 5 parts of strontium oxide and 95 parts of nickel oxide powder, and then ball milled and mixed, and then spray granulated to obtain spherical particles. Then 0.8MPa compression molding was performed, and 250MPa cold isostatic pressing was performed to obtain a blank target. Finally, the temperature was raised from room temperature to 750℃ at a rate of 2℃ / min and kept for 30h in an oxygen atmosphere, and then the temperature was raised to 1700℃ at a rate of 5℃ / min and kept for 48h. Natural cooling to room temperature obtained a strontium-doped nickel oxide target.
[0038] Example 4
[0039] This example provides a nickel oxide-based target material, and its component dosage and preparation method are as follows:
[0040] Pure water was added to 1 part of strontium oxide and 99 parts of nickel oxide powder, and then ball milled and mixed, and then spray granulated to obtain spherical particles. Then 0.5MPa compression molding was performed, and 230MPa cold isostatic pressing was performed to obtain a blank target. Finally, the temperature was raised from room temperature to 600℃ at a rate of 2℃ / min in an oxygen atmosphere for 24h, and then the temperature was raised to 1500℃ at a rate of 5℃ / min for 36h. Natural cooling to room temperature obtained a strontium-doped nickel oxide target.
[0041] Example 5
[0042] This example provides a nickel oxide-based target material, and its component dosage and preparation method are as follows:
[0043] Pure water was added to 20 parts of strontium oxide and 80 parts of nickel oxide powder, and then ball milled and mixed, and then spray granulated to obtain spherical particles. Then 0.5MPa compression molding was performed, and 230MPa cold isostatic pressing was performed to obtain a blank target. Finally, the temperature was raised from room temperature to 600℃ at a rate of 2℃ / min in an oxygen atmosphere for 24h, and then the temperature was raised to 1500℃ at a rate of 5℃ / min for 36h. Natural cooling to room temperature obtained a strontium-doped nickel oxide target.
[0044] Example 6
[0045] This example provides a nickel oxide-based target material, and its preparation method is basically the same as that of Example 1, except that 10 parts of strontium oxide and 90 parts of nickel oxide are used.
[0046] Example 7
[0047] This example provides a nickel oxide-based target material, and its preparation method is basically the same as that of Example 1, except that 3 parts of strontium oxide and 97 parts of nickel oxide are used.
[0048] Comparative Example 1
[0049] This example provides a nickel oxide-based target material, and its component dosage and preparation method are as follows:
[0050] Pure water was added to 100 parts of nickel oxide powder, and then ball milled and spray granulated to obtain spherical particles. Then 0.5Mpa compression molding was performed, and 230MPa cold isostatic pressing was performed to obtain a green blank target. Finally, the temperature was raised from room temperature to 600℃ at a rate of 2℃ / min and kept for 24h in an oxygen atmosphere, and then the temperature was raised to 1500℃ at a rate of 5℃ / min and kept for 36h. The nickel oxide target was naturally cooled to room temperature to obtain the nickel oxide target.
[0051] Comparative Example 2
[0052] This example provides a nickel oxide-based target material, and its preparation method is basically the same as that of Example 1, except that, based on the total mass of the nickel oxide-based target material, strontium oxide accounts for 0.05% of the total mass. 0.05 parts of strontium oxide and 99.95 parts of nickel oxide.
[0053] Comparative Example 3
[0054] This example provides a nickel oxide-based target material, and its preparation method is basically the same as that of Example 1, except that, based on the total mass of the nickel oxide-based target material, strontium oxide accounts for 25% of the total mass. 25 parts of strontium oxide and 75 parts of nickel oxide.
[0055] Performance Testing
[0056] The nickel oxide-based targets prepared in Examples 1 to 7 of the present invention and the comparative example were tested for relative density, and the data are shown in Table 1.
[0057] The nickel oxide-based targets prepared in Examples 1 to 7 of the present invention and the comparative example were subjected to radio frequency magnetron sputtering (sputtering power 1 KW, chamber vacuum 6.5×10 -4 The resistivity and RMS roughness of the prepared films were tested. The data are shown in Table 1.
[0058] Relative density: measured using the Archimedes displacement method;
[0059] Resistivity: measured using a four-probe DC resistance meter;
[0060] Film root mean square roughness: measured using atomic force microscopy.
[0061] Table 1 Examples 1 to 7 and Comparative Examples 1 to 3
[0062] Relative density (%) Resistivity (Ω·cm) RMS roughness(nm) Example 1 98.5 <![CDATA[3.8×10 4 ]]> 5.99 Example 2 96.4 <![CDATA[4.8×10 5 ]]> 6.04 Example 3 97.8 <![CDATA[4.5×10 5 ]]> 6.03 Example 4 94.6 <![CDATA[7.7×10 6 ]]> 7.64 Example 5 95.7 <![CDATA[3.6×10 6 ]]> 6.98 Example 6 96.3 <![CDATA[2.4×10 6 ]]> 7.32 Example 7 97.2 <![CDATA[6.2×10 5 ]]> 6.24 Comparative Example 1 90.3 <![CDATA[8.4×10 6 ]]> 8.01 Comparative Example 2 90.5 <![CDATA[8.4×10 6 ]]> 7.96 Comparative Example 3 86.8 <![CDATA[7.3×10 6 ]]> 8.60
[0063] From the data in Table 1, it can be seen that the present invention can increase the relative density of the target material by introducing strontium oxide doping into the nickel oxide target material, and can reduce the resistivity and roughness of the film made from the target material by magnetron sputtering.
[0064] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.
Claims
1. A nickel oxide-based target material, characterized in that: The target comprises nickel oxide and strontium oxide. The strontium oxide accounts for 0.1% to 20% of the total mass of the nickel oxide-based target.
2. The nickel oxide-based target material according to claim 1, characterized in that: The strontium oxide accounts for 1% to 20% of the total mass.
3. The nickel oxide-based target material according to claim 1, characterized in that: The strontium oxide accounts for 3% to 5% of the total mass.
4. The method for preparing a nickel oxide-based target according to any one of claims 1 to 3, characterized in that: The steps include: S1, mixing nickel oxide powder and strontium oxide powder, ball milling and spray granulation to obtain powder particles; S2, molding the powder particles, and obtaining a green target material by cold isostatic pressing; S3, sintering the green target material.
5. The preparation method according to claim 4, characterized in that: The compression molding pressure is 0.1 MPa to 0.8 MPa.
6. The preparation method according to claim 4, characterized in that: The cold isostatic pressing pressure is 200 MPa to 250 MPa.
7. The preparation method according to claim 4, characterized in that: The sintering steps are as follows: The temperature is raised to 500-750°C for insulation I, and then raised to 1400-1700°C for insulation II.
8. The preparation method according to claim 7, characterized in that: The insulation time I is 20h to 30h.
9. The preparation method according to claim 7, characterized in that: The time of the insulation II is 24 to 48 hours.
10. Use of the nickel oxide-based target material according to any one of claims 1 to 3 in the preparation of optical semiconductor devices.
Citation Information
Patent Citations
Oxide sintered compact, sputtering target, and oxide semiconductor thin film obtained using same
CN106458759A
NMO oxide semiconductor material and preparation method and application thereof
CN116332623A
Hole transport layer, preparation method thereof and perovskite solar cell
CN117794268A
High-density nickel oxide-based rotating target material and preparation method thereof
CN118206360A
Electric Water Pump Using Axial Gap Type Electric Motor