Al acid etching solution for display panel, and preparation method and application of Al acid etching solution

Wet etching Mo/ is solved by using acidic components such as tartaric acid, egic acid and nitric acid as corrosion inhibitors in the wet etching solution. The problem of uneven etching rate in the Al metal process achieves uniform etching of substrates and avoids Mura, improving etching uniformity and cost-effectiveness.

CN118880334AInactive Publication Date: 2024-11-01ZHEJIANG AUFIRST MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410926512.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the wet etching process of Mo/Al metal, the etching liquid etches too fast on the metal molybdenum and the aluminum etching rate is too slow, resulting in problems such as metal delamination, Mura and poor etching uniformity.

Method used

Using a display panel Al acid etching solution, its composition includes organic acids such as tartaric acid and oxylic acid and inorganic acids such as nitric acid, through a specific mass ratio and additives 5-methoxy-N,N-dimethyltryptamine and Titanium oxide forms a synergistic corrosion inhibitor, adjusts the pH and viscosity of the etching liquid, slows down the etching rate of the Mo layer metal, and avoids the occurrence of Mura phenomenon.

Benefits of technology

The uniform etching of the Mo/Al substrate is achieved, the Mura phenomenon is avoided, the etching uniformity is ensured, the cost of the etching liquid is reduced, and the precision units on the substrate are protected through a gentle etching process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880334A_ABST
    Figure CN118880334A_ABST
Patent Text Reader

Abstract

The invention relates to a display panel Al acid etching solution and a preparation method and application thereof. The Al acid etching liquid for the display panel comprises the following components in parts by weight: 65-80 parts of organic acid; 5-10 parts of inorganic acid; 1-3 parts of nitrate; 0.5 to 2.5 parts of an additive; and 15-25 parts of ultrapure water. The etching process of the etching liquid is mild, and loss and damage to a precision unit on a substrate cannot be caused. The additive used in the etching solution can serve as a synergistic corrosion inhibitor to slow down Mo layer metal etching, and the Mura phenomenon is avoided. The etching liquid is good in uniformity, after the substrate is etched, parameter differences of the edge and all parts of the substrate are small, and no etching residue exists.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of display panel manufacturing technology, and in particular relates to an Al acid etching solution for a display panel, a preparation method thereof and a use thereof. Background Art

[0002] Etching technology is to transfer the photoresist pattern produced after development to the material under the photoresist to form a pattern defined by photolithography. It includes uniform removal of the entire surface of the material and selective removal of the pattern, which can be divided into two technologies: wet etching and dry etching.

[0003] Since 1970, component manufacturing has first begun to use plasma etching technology, also known as plasma etching technology, and people have a deeper understanding of plasma chemistry. In today's semiconductor integrated circuit or panel manufacturing process, it is required to accurately control the size of various materials to sub-micron size, and it must also have extremely high reproducibility. Plasma etching is the only technology in today's technology that can efficiently complete this work at a high yield. Therefore, plasma etching has become one of the main technologies for semiconductor manufacturing and thin film field effect transistor liquid crystal display TFT LCD (Thin Film Transistor Liquid Crystal Didsplay).

[0004] Compared with dry etching, wet etching has a good etching selectivity ratio between the material to be etched and the photoresist and the underlying material. However, in the process of wet etching of Mo / Al metal, the low-concentration diluted etching solution has a very fast etching rate for metal molybdenum, but a very slow etching rate for aluminum, which leads to metal stratification, excessive etching of the molybdenum metal layer, and more exposure of the underlying Al alloy layer, which causes problems such as color difference (Mura) and poor etching uniformity. Summary of the invention

[0005] The technical problem solved by the present invention is that in the process of wet etching Mo / Al metal, the etching liquid has a very fast etching rate for metal molybdenum, but a very slow etching rate for aluminum, which leads to metal stratification, excessive etching of the molybdenum metal layer, and more exposure of the underlying Al alloy layer, which causes Mura and poor etching uniformity.

[0006] In view of the technical problems existing in the prior art, the present invention designs an Al acid etching solution for display panels, a preparation method and use thereof, which mainly solves the Mura problem generated by Mo / Al substrates after etching and has good etching uniformity.

[0007] It should be noted that, in the present invention, unless otherwise specified, the specific meaning of "including" in relation to composition limitations and descriptions includes both open-ended "including", "comprising" and similar meanings, and closed-ended "consisting of..." and similar meanings.

[0008] In order to solve the above-mentioned technical problems, the present invention adopts the following solutions:

[0009] A display panel Al acid etching solution, characterized in that it comprises the following components calculated by weight:

[0010]

[0011] Furthermore, the organic acid is one or more of tartaric acid, oxalic acid, acetic acid, citric acid, sebacic acid, lactic acid, glycine, and malic acid.

[0012] Furthermore, the organic acid is a mixture of tartaric acid and oxalic acid; the mass ratio of tartaric acid to oxalic acid in the organic acid is 3.5-5:1.

[0013] In the present invention, the mass ratio of tartaric acid to oxalic acid in the organic acid is preferably 4-4.5:1.

[0014] Furthermore, the organic acid is at least two of tartaric acid, oxalic acid, acetic acid, citric acid, sebacic acid, lactic acid, glycine, and malic acid.

[0015] Furthermore, the mass ratio of the two organic acids is 3.5-5:1.

[0016] Furthermore, the mass ratio of the two organic acids is preferably 4-4.5:1.

[0017] Furthermore, the inorganic acid is one or more of nitric acid, periodic acid, hydrobromic acid, and perchloric acid.

[0018] Furthermore, the nitrate is one or more of sodium nitrate, potassium nitrate, calcium nitrate and ammonium nitrate.

[0019] Furthermore, the additive is a mixture of 5-methoxy-N,N-dimethyltryptamine and titanium oxide.

[0020] Furthermore, the mass ratio of 5-methoxy-N,N-dimethyltryptamine to titanium oxide in the additive is 2-5:1.

[0021] The present invention also discloses a method for preparing an Al acid etching solution for a display panel, which is characterized by comprising the following steps:

[0022] Step 1: Weigh the respective amounts of each component;

[0023] Step 2: At 10-20° C., add all components except additives into a container, and finally slowly add the additives and stir until the solution is transparent and colorless with no particle precipitation, thereby obtaining the display panel Al acid etching solution.

[0024] It should be noted that in the preparation method, the temperature in step 1 is preferably 15° C., and the temperature is always kept below 20° C. to prevent excessive temperature and a large loss of oxalic acid.

[0025] The present invention also discloses an etching method of a display panel using an Al acid etching solution, which is characterized by comprising the following steps:

[0026] Step 1: In a sealed condition, the Al acid etching solution of the display panel is heated to 35-40° C. After the temperature is stabilized, the Mo / Al substrate is placed in the etching solution and the substrate is vibrated at the same time;

[0027] Step 2: Rinse the Mo / Al substrate after etching with ultrapure water at least twice to fully clean the residual etching solution, and finally blow dry with nitrogen to complete the etching.

[0028] In the present invention, the etching method can also be referred to as a one-step etching method for Mo / Al substrates, in which the etching time is different for substrates of different thicknesses, generally 20-30 OE. The cleaning time in step 2 is 1-2 min.

[0029] The invention also discloses a use of Al acid etching solution for a display panel in etching a metal substrate.

[0030] In the application of the present invention, the types of substrates to which the etching solution of the present invention can be applied include Mo / Al substrates, Mo / Al / Mo substrates, Mo / AlNd / Mo substrates, Mo / AlNd substrates, Ti / Al / Ti substrates, and the like.

[0031] In the present invention, in order to further optimize the etching effect, the display panel Al acid etching solution may further preferably include: 70-80 parts of organic acid; 5-8 parts of inorganic acid; 1-2 parts of nitrate; 1-2.5 parts of additives; and 15-20 parts of ultrapure water.

[0032] In the present invention, the inorganic acid is preferably nitric acid, which oxidizes metal Mo and Al into corresponding oxides to accelerate etching, and is also the main component for providing acidic conditions.

[0033] In the present invention, the nitrate is preferably potassium nitrate; the nitrate provides nitrate radicals to the etching solution, plays an auxiliary oxidation role, and reduces the viscosity of the etching solution.

[0034] In the present invention, the mass ratio of 5-methoxy-N,N-dimethyltryptamine to titanium oxide in the additive is most preferably 4:1; the additive can inhibit the corrosion of the Mo layer metal.

[0035] In the present invention, the combination of organic acids has a special effect:

[0036] First, tartaric acid can provide hydrogen ions, i.e., an acidic environment, to the etching solution, thus promoting the etching process of Mo and Al oxides. On the other hand, tartaric acid can chelate Mo and Al ions, thus preventing a large amount of metal ions from being adsorbed on the substrate.

[0037] Secondly, oxalic acid provides hydrogen ions to the etching solution, and the acidification effect promotes etching. At high concentrations, it inhibits Mo metal etching. Oxalic acid is a weak acid and has a certain buffering effect.

[0038] Tartaric acid and oxalic acid work synergistically with each other. After being dissolved in the etching solution, the etching solution has low viscosity and good fluidity, which is conducive to uniform etching of the substrate during the etching process.

[0039] In the present invention, additives have unique advantages:

[0040] The corrosion inhibition principle of the additive of the present invention is as follows:

[0041] First, 5-methoxy-N,N-dimethyltryptamine and titanium oxide synergistically inhibit corrosion.

[0042] Titanium oxide is reduced to titanium element under the action of 5-methoxy-N,N-dimethyltryptamine.

[0043] Because Mo and Al metals undergo electrochemical reactions in the etching solution and generate current, the titanium element is selectively adsorbed in the area where the electrochemical reaction is most intense. Ultimately, most of it is deposited and adsorbed in the Mura area on the surface of the Mo / Al substrate, and forms a dense composite film with 5-methoxy-N,N-dimethyltryptamine, thereby achieving corrosion inhibition.

[0044] Secondly, 5-methoxy-N,N-dimethyltryptamine is a weakly alkaline substance, which can adjust the pH of the etching solution and reduce the etching degree of the Mo layer metal.

[0045] Third, 5-methoxy-N,N-dimethyltryptamine can act as a chelating agent to form stable complexes with Mo and Al ions, thereby reducing the possibility of metal ions participating in oxidation reactions.

[0046] The present invention provides an Al acid etching solution for a display panel, and its preparation method and use have the following beneficial effects:

[0047] 1. The additives 5-methoxy-N,N-dimethyltryptamine and titanium oxide are used in the etching solution of the present invention, which can act as synergistic corrosion inhibitors to slow down the metal etching of the Mo layer and avoid the generation of the Mura phenomenon.

[0048] 2. The etching process of the etching solution of the present invention is mild, and the organic acids used, such as tartaric acid and oxalic acid, are weak acids, which will not cause damage to the precision units on the substrate.

[0049] 3. The etching solution of the present invention has good uniformity. Since the etching solution of the present method has low viscosity and good fluidity, it can evenly etch all parts of the substrate. After the substrate is etched, the parameters of the edge and all parts of the substrate are relatively small, and there is no etching residue.

[0050] 4. The etching solution of the present invention has a simple preparation method, low cost, and small volatilization loss, and only pure water is needed for rinsing after etching. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 : This is a partial photo of an OLED made from a substrate etched with the etching solution of Comparative Example 2 after being powered on;

[0052] Figure 2 : This is a partial photo of the substrate after being etched using the etching solution of Example 1 to make an OLED after being powered on;

[0053] Figure 3 : An optical microscope picture of the substrate surface after etching using the etching solution of Comparative Example 2 at 50 OE magnified 1000 times;

[0054] Figure 4 : An optical microscope picture of the substrate surface after etching using the etching solution of Example 1 at 50 OE magnified 1000 times;

[0055] Figure 5 : This is a SEM picture of the substrate surface after etching with the etching solution of Comparative Example 2, magnified 40,000 times from a top-down angle;

[0056] Figure 6 : This is a SEM picture of the substrate surface after etching with the etching solution of Example 1, magnified 40,000 times from a top view angle. DETAILED DESCRIPTION

[0057] The present invention will be further described below in conjunction with specific embodiments and accompanying drawings:

[0058] The Al acid etching solutions for display panels involved in Examples 1-9 and Comparative Examples 1-3 of the present invention include components and mass ratios as shown in Table 1.

[0059] The preparation method of the display panel Al acid etching solution is as follows:

[0060] Step 1: Weigh the respective amounts of each component;

[0061] Step 2: At 15°C, add all components except additives into a container, and finally slowly add the additives and stir until the solution is transparent and colorless with no particle precipitation.

[0062] Table 1 Example 1-Example 9

[0063]

[0064] Table 2 Comparative Examples 1-3

[0065]

[0066] Regarding the etching method of the present invention:

[0067] Step 1: In a sealed condition, the Al acid etching solution of the display panel is heated to 40° C. After the temperature stabilizes, the Mo / Al substrate is placed in the etching solution and the substrate is vibrated at the same time;

[0068] Step 2: Rinse the Mo / Al substrate after etching with ultrapure water for 1 minute to fully clean the residual etching solution, and finally blow dry with nitrogen to complete the etching.

[0069] About performance testing and description:

[0070] Performance 1 The test method for mildness of etching process is:

[0071] Step 1: Heat the etching solution to 40°C. After the temperature stabilizes, place the substrate Place in the etching solution, oscillate the substrate, and etch for 50 OE.

[0072] Step 2: Rinse the etched Mo / Al substrate with ultrapure water for 1 minute to fully clean the etching solution residue, and finally dry it with nitrogen to obtain the etched substrate.

[0073] Performance 2Mura test method is:

[0074] Use substrates with the same thickness specifications Conduct experiments.

[0075] A substrate is divided into 5 points, and the temperature of the etching solution is raised to 40°C. After the temperature stabilizes, the substrates are placed in different etching solutions for etching, and the etching time is 30OE.

[0076] The substrate is taken out, cleaned and blown dry. After removing the photoresist, the substrate is split and the sample is prepared for SEM inspection.

[0077] The average CD-loss (μm) of the Mo layer metal at 5 points was calculated. The calculation results are shown in Table 3.

[0078] It should be noted that in the display panel industry, Mura refers to the phenomenon of uneven brightness of liquid crystal displays, that is, dark or inconsistent areas appear on the screen.

[0079] Observe the situation after the etching substrate is made into OLED and powered on. Figure 1-Figure 2 ; Place the etched substrate under an optical microscope to observe the surface precision units. Figure 3-Figure 4 ; Observe the surface effect after etching the middle point on the substrate Figure 5-Figure 6 .

[0080] Table 3 Test results

[0081]

[0082] Further analysis of the test results:

[0083] It can be seen from Table 3 that, by comparing the CD-loss data, the uniformity of the etching solution of the embodiment of the present invention is better than that of the etching solution of the comparative example, that is, the difference in etching parameters at different positions of the etching solution of the present invention is much smaller than that of the etching solution of the comparative example.

[0084] Judging from the CD-loss data alone, the CD-loss of the comparative etching solution is higher than that of the embodiment etching solution as a whole. The larger the CD-loss, the faster the etching. The etching rate of the embodiment etching solution of the present invention to the Mo layer metal is slower, while the etching rate of the comparative etching solution to the Mo layer metal is faster.

[0085] Therefore, from another aspect, it is reflected that the etching process of the etching solution of the embodiment is milder than that of the etching process of the etching solution of the comparative example.

[0086] Compared with Example 1, Comparative Example 1 only adds 5-methoxy-N,N-dimethyltryptamine. The CD-loss at different positions is quite different. The precision unit on the substrate is destroyed, the metal of the top Mo layer shrinks severely, and severe Mura phenomenon occurs.

[0087] Compared with Example 1, Comparative Example 2 only adds titanium oxide, and there is a large difference in CD-loss at different positions. The precision units on the substrate are destroyed, the metal of the top Mo layer shrinks severely, and severe Mura phenomenon occurs.

[0088] Comparative Example 3 uses an etching solution of phosphoric acid, nitric acid, and acetic acid system with a relatively large proportion of nitric acid. After etching, the CD-loss at different positions of the substrate varies greatly, the precision units on the substrate are destroyed, the top Mo layer metal shrinks, and a slight Mura phenomenon occurs.

[0089] Further comparison is made through the attached drawings in the specification:

[0090] Figure 1 This is a partial photo of an OLED made from a substrate etched using the etching solution of Comparative Example 2 after being powered on; Figure 2 This is a partial photograph of the substrate after being etched using the etching solution of Example 1 to make an OLED after being powered on.

[0091] from Figure 1 It can be seen that after the substrate etched with the etching solution of Comparative Example 2 was made into an OLED, the scanning electron microscope showed that obvious black and white spots Mura appeared on the surface.

[0092] from Figure 2 It can be seen that after the substrate is etched using the etching solution of Example 1 and made into an OLED, the scanning electron microscope shows that there is no Mura and the surface is clean and smooth.

[0093] Figure 3 This is an optical microscope picture of the substrate surface magnified 1000 times after etching using the etching solution of Comparative Example 2 and etching time of 50 OE; Figure 4 This is an optical microscope picture of the substrate surface magnified 1000 times after etching using the etching solution of Example 1 and a time of 50 OE.

[0094] When testing the mild etching effect, the etching time should exceed the etching time required by the process, under the condition of 50OE. Figure 3 and Figure 4 It can be seen that the etching process of the etching solution of comparative example 3 is relatively strong, which will cause serious damage to the precision units on the surface of the substrate; while the etching process of the etching solution of embodiment 1 is gentle, and even under long-term etching conditions, there is almost no damage to the precision units on the surface of the substrate.

[0095] Figure 5 This is a SEM image of the substrate surface after etching with the etching solution of Comparative Example 2, magnified 40,000 times from a top view angle; Figure 6 This is a SEM image of the substrate surface after etching with the etching solution of Example 1, magnified 40,000 times from a top view angle.

[0096] from Figure 5 It can be seen that the red framed area is the area where the top Mo layer metal is severely retracted, that is, serious Mura phenomenon occurs. Figure 6 There is no severe shrinkage area of ​​the Mo layer metal, that is, there is no Mura phenomenon.

[0097] Because the etching rates of Mo and Al metals on the substrate in traditional etching solutions are quite different (Mo etching rate is too fast), a large Mo shrinkage phenomenon (step phenomenon) occurs, resulting in the subsequent Mura phenomenon.

[0098] The use of the etching solution of the present invention can effectively reduce the etching rate of the Mo layer metal, thereby avoiding the occurrence of step phenomenon and ensuring that the Mura phenomenon will not occur later due to a poor etching process.

[0099] The etching process of the etching solution of the present invention is mild, and tartaric acid and oxalic acid are both weak acids, and the nitric acid component accounts for a small proportion, so the etching process is mild and will not cause damage to the precision units on the substrate. The additive used in the etching solution of the present invention can be used as a synergistic corrosion inhibitor to slow down the metal etching of the Mo layer and avoid the generation of the Mura phenomenon. The etching solution of the present invention has good uniformity. After the substrate is etched, the parameters after etching at the edge and various parts of the substrate are relatively small, and there is no etching residue.

[0100] The present invention is described exemplarily above in conjunction with the embodiments and drawings. It is obvious that the implementation of the present invention is not limited to the above-mentioned methods. As long as various improvements are made using the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.

Claims

1. A display panel Al acid etching solution, characterized in that: Calculated by weight, it includes the following components: 65-80 parts of organic acid; 5-10 parts of inorganic acid; 1-3 parts of nitrate; Additives 0.5-2.5 parts; 15-25 parts of ultrapure water.

2. The Al acid etching solution for display panel according to claim 1, characterized in that: The organic acid is one or more of tartaric acid, oxalic acid, acetic acid, citric acid, sebacic acid, lactic acid, glycine and malic acid.

3. The Al acid etching solution for display panel according to claim 2, characterized in that: The organic acid is a mixture of tartaric acid and oxalic acid; the mass ratio of the tartaric acid to oxalic acid is 3.5-5:

1.

4. The Al acid etching solution for display panel according to claim 1, characterized in that: The inorganic acid is one or more of nitric acid, periodic acid, hydrobromic acid and perchloric acid.

5. The Al acid etching solution for display panel according to claim 1, characterized in that: The nitrate is one or more of sodium nitrate, potassium nitrate, calcium nitrate and ammonium nitrate.

6. The Al acid etching solution for display panel according to claim 1, characterized in that: The additive is a mixture of 5-methoxy-N,N-dimethyltryptamine and titanium oxide.

7. The Al acid etching solution for display panel according to claim 6, characterized in that: The mass ratio of 5-methoxy-N,N-dimethyltryptamine to titanium oxide in the additive is 2-5:

1.

8. A method for preparing the Al acid etching solution for a display panel according to any one of claims 1 to 7, characterized in that The following steps are involved: Step 1: Weigh each component in its respective amount; Step 2: At 10-20° C., add all components except additives into a container, and finally slowly add the additives and stir until the solution is transparent and colorless with no particle precipitation, thereby obtaining the display panel Al acid etching solution.

9. An etching method for a display panel using an Al acid etching solution according to any one of claims 1 to 7, characterized in that The following steps are involved: Step 1: In a sealed condition, the Al acid etching solution of the display panel is heated to 35-40° C. After the temperature is stabilized, the Mo / Al substrate is placed in the etching solution and the substrate is vibrated at the same time; Step 2: Rinse the Mo / Al substrate after etching with ultrapure water at least twice to fully clean the residual etching solution, and finally blow dry with nitrogen to complete the etching.

10. Use of the display panel Al acid etching solution according to any one of claims 1 to 7 in etching a metal substrate.