Amorphous aluminum-manganese alloy and aluminum compounded corrosion-resistant coating on magnesium alloy surface and preparation method of amorphous aluminum-manganese alloy and aluminum compounded corrosion-resistant coating

By first immersing the magnesium alloy surface in zinc and then preparing an amorphous aluminum-manganese alloy and aluminum composite coating, the problems of decreased corrosion resistance of the aluminum coating and copper introduction were solved, achieving high corrosion resistance and lightweight effect on the magnesium alloy surface.

CN118880407APending Publication Date: 2024-11-01SANLEI (NINGBO) NEW MATERIAL TECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411078753.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing aluminum coatings on magnesium alloy surfaces are prone to defects such as gaps and holes during ionic liquid aluminum plating, which leads to a significant decrease in corrosion resistance. Furthermore, the introduction of copper alloying elements increases weight and is not conducive to the lightweighting and recycling of magnesium alloys.

Method used

The magnesium alloy surface is first immersed in zinc, and then an amorphous aluminum-manganese alloy coating and an aluminum coating are prepared by ion liquid plating to form an amorphous aluminum-manganese alloy/aluminum composite coating. The amorphous aluminum-manganese alloy is used as a transition layer to improve the bonding strength and density, and to avoid the introduction of unfavorable alloying elements.

Benefits of technology

It significantly improves the corrosion resistance of magnesium alloy surfaces, ensures coating density and adhesion, maintains the advantage of lightweight design, and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880407A_ABST
    Figure CN118880407A_ABST
Patent Text Reader

Abstract

The invention discloses an amorphous aluminum-manganese alloy and aluminum compounded corrosion-resistant coating on the surface of a magnesium alloy and a preparation method of the amorphous aluminum-manganese alloy and aluminum compounded corrosion-resistant coating. The amorphous aluminum-manganese alloy plating layer is plated on the surface of the magnesium alloy subjected to zinc immersion treatment, and the aluminum plating layer is positioned on the surface of the amorphous aluminum-manganese alloy plating layer; the preparation method comprises the following steps: carrying out zinc immersion treatment on magnesium alloy to obtain a zinc immersion layer, plating the surface of the zinc immersion layer with an ionic liquid to prepare an amorphous aluminum-manganese alloy plating layer, carrying out ionic liquid aluminum plating to form an aluminum plating layer, and finally cleaning and drying to obtain the amorphous aluminum-manganese alloy coating. According to the method, the corrosion resistance of the ionic liquid aluminum coating on the magnesium alloy is remarkably improved, on the basis that alloy elements unfavorable for the magnesium alloy are not introduced, the metal coating with excellent corrosion resistance is obtained from various magnesium alloys, the total thickness of the coating is small, and the technical scheme is environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of magnesium alloy surface treatment, and particularly relates to a corrosion-resistant coating of amorphous aluminum-manganese alloy and aluminum composite on the surface of a magnesium alloy and a preparation method thereof. Background Art

[0002] Magnesium alloys have the advantages of light weight, high specific strength, good electrical and thermal conductivity, etc., and have broad application prospects in the fields of national defense, military industry, transportation, electronic communications, etc. Under the trend of lightweight development in various fields, the application of magnesium alloys has received more and more attention. However, magnesium alloys are very prone to corrosion in the use environment, and various surface treatment technologies must be used to form a protective layer on the surface of magnesium alloys.

[0003] According to the different materials of magnesium alloy surface protective layer, it can be divided into: polymer (such as fluorocarbon coating), inorganic compound (such as micro-arc oxidation film) and metal (such as copper / nickel composite layer, nickel phosphorus, aluminum, etc.). Among them, the metal protective layer has the advantages of high electrical and thermal conductivity, good high temperature resistance and anti-aging performance, and strong decorative effect. Aluminum has low density and high atmospheric corrosion resistance, and is an excellent surface protective layer material. At present, the methods for preparing aluminum protective layer on the surface of magnesium alloy include: thermal spraying, cold spraying, vacuum plating, electroplating, etc. Among them, the technology of ionic liquid aluminum electroplating has the advantages of low operating temperature, no restrictions on the shape of parts, and green environmental protection. It is the most promising aluminum coating preparation technology.

[0004] There are papers and patents reporting on ionic liquid aluminum plating of magnesium alloys. Before aluminum plating, the magnesium alloy is first anodized in the plating solution to remove the oxide film, or the surface of the magnesium alloy is treated by zinc immersion to enhance the bonding between the substrate and the coating. For example, US13240021 (Protective effect of ionic liquid aluminum plating on magnesium alloys) discloses a method of reverse current etching (anodic activation) of magnesium alloys in ionic liquids and then electroplating aluminum; CN108716011A (A method for improving the bonding between aluminum coating and magnesium alloy surface) discloses a method of ionic liquid aluminum plating after zinc immersion.

[0005] However, after anodic activation, magnesium alloy will undergo a rapid replacement reaction with ionic liquid, and the bonding force is difficult to control; and after zinc immersion, ionic liquid aluminum plating, the sample will have a bulging phenomenon in the process of atmospheric placement. The reason is that zinc immersion is a replacement reaction, and the obtained zinc layer is not dense enough. Therefore, when ionic liquid aluminum is plated, the aluminum coating is prone to defects such as gaps and holes, resulting in a significant decrease in the corrosion resistance of the coating. Some literature uses zinc immersion, first electroplating zinc thickening and then electroplating copper, and then ionic liquid aluminum zirconium alloy plating to form a three-layer structure of zinc / copper / aluminum zirconium alloy. Under the condition of a total coating thickness of 25μm, the salt spray test does not change color within 48h, and the substrate is not corroded within 144h. However, the introduction of copper not only increases the weight of the parts, weakens the advantages of magnesium alloy in lightweight, but also is not conducive to the recycling of magnesium alloy. Summary of the invention

[0006] In order to solve the problems existing in the background technology, the present invention provides a corrosion-resistant coating of amorphous aluminum-manganese alloy and aluminum composite on the surface of a magnesium alloy and a preparation method thereof, which solves the technical problem of significantly reduced corrosion resistance after aluminum plating, and also solves the defects and shortcomings brought about by the introduction of copper in the prior art.

[0007] The present invention adopts an ionic liquid aluminum plating method to improve the corrosion resistance of a metal plating layer on the surface of a magnesium alloy without introducing alloy elements such as copper.

[0008] The technical solution adopted by the present invention is:

[0009] 1. A corrosion-resistant coating of amorphous aluminum-manganese alloy and aluminum composite on the surface of a magnesium alloy:

[0010] It includes an amorphous aluminum-manganese alloy coating and an aluminum coating located on the surface of the amorphous aluminum-manganese alloy coating. Preferably, the magnesium alloy surface is sequentially provided with only a zinc immersion layer, an amorphous aluminum-manganese alloy coating, and an aluminum coating.

[0011] The amorphous aluminum-manganese alloy coating is plated on the surface of the magnesium alloy that has been subjected to zinc immersion treatment.

[0012] The thickness of the amorphous aluminum-manganese alloy coating is 2-6 μm; the thickness of the aluminum coating is 12-20 μm.

[0013] The manganese content of the amorphous aluminum-manganese alloy coating is 8 to 16 at. %.

[0014] 2. A method for preparing a corrosion-resistant coating of amorphous aluminum-manganese alloy and aluminum composite on the surface of the magnesium alloy:

[0015] After the magnesium alloy is zinc-impregnated to obtain a zinc-impregnated layer, an ionic liquid is used to plate on the surface of the zinc-impregnated layer to prepare an amorphous aluminum-manganese alloy coating, and then the ionic liquid is aluminum-plated to form an aluminum coating, and finally the coating is prepared after cleaning and drying.

[0016] The magnesium alloy may be AZ31B, AZ91D, AM60, LZ91 or the like.

[0017] The amorphous aluminum-manganese alloy is prepared by ionic liquid plating, specifically using an ionic liquid plating solution of manganese chloride-aluminum chloride-1-ethyl 3-methylimidazole chloride (MnCl2-AlCl3-EMIC) or manganese chloride-aluminum chloride-1-butyl 3-methylimidazole chloride (MnCl2-AlCl3-BMIC), at a temperature of 25°C to 60°C and a current density of 6 to 15 mA / cm 2 The coating preparation is carried out below.

[0018] In the ionic liquid plating solution of manganese chloride-aluminum chloride-1-ethyl 3-methylimidazole chloride (MnCl2-AlCl3-EMIC), the content of manganese chloride MnCl2 is 0.1-0.2 mol / L, and the molar ratio between aluminum chloride AlCl3 and 1-ethyl 3-methylimidazole chloride EMIC is (1.5-2.0):1; that is, MnCl2 is added to 1L of the solution, AlCl3-EMIC is a solution, the composition of AlCl3 and EMIC is 1.5:1-2:1, and the molar content of MnCl2 in the solution is 0.1-0.2 mol, which is the molar content of the AlCl3-EMIC solution.

[0019] The Mn content in the coating obtained from the ionic liquid plating solution is 8 to 16 at%.

[0020] The ionic liquid aluminum plating method specifically uses aluminum chloride-1-ethyl 3-methyl imidazole chloride (AlCl3-EMIC), aluminum chloride-trimethyl aniline chloride or aluminum chloride-trimethyl benzyl ammonium chloride as the plating solution, at a temperature of 25°C to 80°C and a current density of 10 to 80 mA / cm 2 The coating preparation is carried out below.

[0021] In the aluminum chloride-1-ethyl 3-methyl imidazole chloride (AlCl3-EMIC) plating solution, the molar ratio of aluminum chloride AlCl3 to 1-ethyl 3-methyl imidazole chloride EMIC is (1.5-2.0): 1. In addition, additives such as nicotinamide, o-phenanthroline, 4-cyanopyridine, cetylpyridinium chloride, and cetyltrimethylammonium bromide can be added to improve the density and thickness uniformity of the coating.

[0022] The amorphous aluminum-manganese alloy coating and the aluminum coating prepared in the present invention form a metallurgical bond, which diffuses between atoms and interlocks with each other. This can significantly improve the corrosion resistance of the ionic liquid aluminum coating on the magnesium alloy without introducing adverse alloy conditions. At the same time, the total thickness is thin, which is environmentally friendly, and achieves multiple effects and advantages in many aspects.

[0023] 3. A magnesium alloy surface having a corrosion-resistant coating of the amorphous aluminum-manganese alloy and aluminum composite.

[0024] A zinc coating, an amorphous aluminum-manganese alloy coating and an aluminum coating are sequentially prepared on the surface of the magnesium alloy outward, and the amorphous aluminum-manganese alloy coating and the aluminum coating constitute a corrosion-resistant coating composited with an amorphous aluminum-manganese alloy and aluminum.

[0025] The technical idea of ​​the present invention is: on the basis of the pre-treatment of magnesium alloy zinc immersion, an amorphous aluminum alloy is used as a transition layer to construct an amorphous aluminum alloy / aluminum composite coating, which significantly improves the corrosion resistance of the ionic liquid aluminum coating on the magnesium alloy. That is, for the magnesium alloy treated with zinc immersion, an amorphous aluminum-manganese alloy coating is prepared on the surface of the zinc immersion layer by using ionic liquid plating technology, and then aluminum is plated with ionic liquid. The amorphous aluminum-manganese alloy coating acts as an over-coating, and a dense coating is obtained on the surface of the zinc immersion layer, providing a good base for ionic liquid aluminum plating; while the aluminum coating plays a role in corrosion resistance, and can also protect the amorphous coating with greater brittleness.

[0026] In addition, the corrosion potential of amorphous aluminum-manganese alloy is between that of magnesium alloy and pure aluminum, and the corrosion rate of amorphous aluminum-manganese alloy is much lower than that of pure aluminum. Therefore, using amorphous aluminum-manganese alloy as a transition layer can also slow down the galvanic corrosion rate between aluminum and magnesium alloy.

[0027] The beneficial effects of the present invention are:

[0028] The present invention uses amorphous aluminum alloy as a transition layer on the basis of pre-treatment of magnesium alloy zinc immersion to construct an amorphous aluminum alloy / aluminum composite coating, thereby significantly improving the corrosion resistance of the ionic liquid aluminum coating on the magnesium alloy.

[0029] Through the present invention, a variety of magnesium alloys can obtain metal coatings with excellent corrosion resistance without introducing alloy elements that are unfavorable to magnesium alloys, and the total thickness of the coating is thin, and the technical solution is environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 Schematic diagram of amorphous aluminum-manganese alloy composite coating on magnesium alloy surface;

[0031] Figure 2 This is the SEM image of the surface of AZ31B alloy after zinc immersion (5000 times);

[0032] Figure 3 This is the SEM morphology of the surface of AZ31B composite coating (5000 times);

[0033] Figure 4 This is the cross-sectional EDS image of the composite coating on AZ31B;

[0034] Figure 5 This is the SEM image (500 times) of 20um aluminum plated with ionic liquid after zinc immersion;

[0035] Figure 6 The morphology comparison diagram of the 4um amorphous aluminum-manganese alloy coating and the pure aluminum coating on the zinc immersion layer (2000 times), where (a) represents the amorphous aluminum-manganese alloy coating and (b) represents the pure aluminum coating. DETAILED DESCRIPTION

[0036] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0037] The coating structure of the present invention is as follows Figure 1 As shown, the specific technical solution is as follows:

[0038] 1. Composite coating thickness: (1) Amorphous aluminum-manganese alloy layer thickness: 2-6um. A thin coating is not conducive to the formation of a dense amorphous alloy layer, and a thick coating is more brittle; (2) Aluminum coating thickness: 12-20um. A thin coating has insufficient corrosion resistance, and a thick coating is prone to dendrites. The manganese content in the amorphous aluminum-manganese alloy is 8-16at.%Mn.

[0039] 2. Process flow: magnesium alloy after zinc immersion → ionic liquid plating of amorphous aluminum-manganese alloy → ionic liquid aluminum plating → cleaning → drying. The magnesium alloy can be AZ31B, AZ91D, AM60, LZ91, etc.;

[0040] 3. Ionic liquid plating of amorphous aluminum-manganese alloy. (1) Plating solution: manganese chloride-aluminum chloride-1-ethyl 3-methylimidazole chloride (MnCl2-AlCl3-EMIC). It can also be other ionic liquid plating solutions, such as aluminum chloride-aluminum chloride-1-butyl 3-methylimidazole chloride (MnCl2-AlCl3-BMIC), etc.; (2) Plating solution composition: the molar ratio of AlCl3 to EMIC is (1.5-2.0):1, and the MnCl2 content is 0.1-0.2 mol / L; (3) Process parameters: 25℃-60℃, current density 6-15mA / cm 2 , the time is determined according to the thickness.

[0041] 4. Ionic liquid aluminum plating. (1) Plating solution: AlCl3-EMIC. It can also be aluminum chloride-trimethylanilinium chloride, aluminum chloride-trimethylbenzylammonium chloride, etc.; (2) Plating solution composition: the molar ratio of AlCl3 to EMIC is (1.5-2.0):1, and it can contain additives such as 4-cyanopyridine, nicotinamide, cetylpyridinium chloride, cetyltrimethylammonium bromide, etc. to improve the density and thickness uniformity of the coating; (3) Process parameters: 25℃~80℃, current density 10~80mA / cm 2 , the time is determined according to the thickness.

[0042] 5. Clean with alcohol and blow dry with hot air.

[0043] Embodiments of the present invention are as follows:

[0044] Embodiment 1:

[0045] (1) Ionic liquid plating of amorphous aluminum-manganese alloy

[0046] AZ31B magnesium alloy was selected for zinc immersion treatment: commercial zinc immersion solution was used for zinc immersion treatment. Figure 2 As shown, there are many gaps between the zinc particles (the black areas in the picture).

[0047] The amorphous aluminum-manganese alloy plating solution is MnCl2-AlCl3-EMIC, wherein the molar ratio of AlCl3-EMIC is 1.5:1, the MnCl2 content is 0.20 mol / L, and the temperature is 25°C;

[0048] High-purity aluminum wire was used as the anode and zinc-impregnated AZ31B was used as the cathode. They were connected to the positive and negative electrodes of a DC power supply at 6 mA / cm 2 The plating was carried out for 30 min at a current density of .

[0049] (2) Ionic liquid aluminum plating

[0050] The plating solution is AlCl3-EMIC, where the molar ratio of AlCl3-EMIC is 1.5:1, and the temperature is 25°C; a high-purity aluminum wire is used as the anode, and AZ31B plated with amorphous aluminum-manganese alloy is used as the cathode, which are connected to the positive and negative electrodes of a DC power supply at 10 mA / cm 2 The current density was 0.04 and the plated samples were plated for 60 min. After plating, the samples were cleaned with alcohol, washed with water and then dried.

[0051] Electron microscope photos of aluminum coating Figure 3 As shown, it can be seen that the aluminum coating is uniform, flat and dense.

[0052] (3) Coating thickness and corrosion resistance test

[0053] The cross-sectional SEM of AZ31B after amorphous aluminum alloy / aluminum composite plating is shown in Figure 2. Figure 4 It can be seen that the top is the magnesium alloy substrate; the white thin layer is the zinc immersion layer, with a thickness of about 0.6μm; the grayish white is the amorphous aluminum-manganese alloy coating, with a thickness of 4μm, in which the manganese content is 15.6at%; the aluminum coating is 12μm thick, and the total thickness is 16μm.

[0054] The product of this embodiment was subjected to a neutral salt spray test according to GB / T 10125-2012. The results are shown in Table 1. There was no change on the inner surface at 360 hours, and several small black spot corrosion appeared at 384 hours.

[0055] Embodiment 2:

[0056] The plating solution of AZ91D magnesium alloy after zinc immersion and amorphous aluminum-manganese alloy is MnCl2-AlCl3-EMIC, where the molar ratio of AlCl3 / EMIC is 2:1, the MnCl2 content is 0.1 mol / L, the temperature is 60 °C, and the flow rate is 15 mA / cm 2The aluminum plating solution is AlCl3-EMIC with a molar ratio of 2:1, a temperature of 80°C, and contains 10 mmol / L of cetylpyridinium chloride. The current density is 80 mA / cm 2 The plating was carried out for 8 min at a current density of .

[0057] The test results are shown in Table 1. The thickness of the amorphous aluminum-manganese alloy coating is 6μm, of which the manganese content is 8.5at%; the thickness of the aluminum coating is 12μm, and the total thickness is 18μm. In the salt spray test, there was no change on the inner surface for 192h, and several small black spots of corrosion appeared at 216h.

[0058] Embodiment 3:

[0059] The plating solution of AZ31B magnesium alloy after zinc immersion and amorphous aluminum-manganese alloy is MnCl2-AlCl3-EMIC, where the molar ratio of AlCl3 / EMIC is 1.8:1, the MnCl2 content is 0.15 mol / L, the temperature is 40°C, and the flow rate is 10 mA / cm 2 The aluminum plating solution is AlCl3-EMIC with a molar ratio of 1.6:1, containing 2mmol / L of 4-cyanopyridine, at a temperature of 40°C and a current density of 30mA / cm 2 The plating was carried out for 24 min at a current density of .

[0060] The test results are shown in Table 1. The thickness of the amorphous aluminum-manganese alloy coating is 2μm, of which the manganese content is 12.0at%; the thickness of the aluminum coating is 15μm, and the total thickness is 17μm. In the salt spray test, there is no change on the inner surface for 96h, and several small black spots of corrosion appear at 120h.

[0061] Comparative Example 1:

[0062] As a comparison, the surface morphology of the zinc-impregnated AZ31B magnesium alloy was directly aluminum-plated with AlCl3-EMIC ionic liquid with a molar ratio of 2:1. The coating thickness was 20 μm. Figure 5 It can be seen that the aluminum in the coating is in granular form, about 10 μm in size, with a small amount of large particles of 40 to 50 μm, and there are obvious gaps between the particles.

[0063] The sample of this comparative example was placed in the atmosphere and bulged, indicating poor bonding. After 24 hours of salt spray test, rust spots appeared at the bulge.

[0064] The product test results of this comparative example compared with Examples 1-3 are shown in Table 1:

[0065] Table 1 Coating thickness and neutral salt spray test results

[0066]

[0067] From the comparison in the above table, it can be seen that the present invention can significantly improve the compactness and salt spray results, that is, significantly improve the corrosion resistance, by plating a layer of amorphous aluminum-manganese alloy with a suitable thickness.

[0068] Embodiment 4:

[0069] The AZ31B magnesium alloy after zinc immersion was plated with amorphous aluminum-manganese alloy with a thickness of 4 μm according to the same treatment process and process parameters as in Example 1, then taken out, cleaned, dried, and observed by SEM. The results are as follows: Figure 6 As shown. Figure 6 As can be seen from (a), the amorphous Al-Mn alloy coating presents a typical cauliflower-like amorphous morphology and the coating is very dense.

[0070] Comparative Example 2:

[0071] As a comparison, the zinc-immersed AZ31B magnesium alloy was subjected to the same preparation process and process parameters as in Example 1, but without the amorphous aluminum-manganese alloy plating treatment in step (1). The alloy was then aluminum-plated to a thickness of 4 μm, taken out, cleaned, dried, and observed by SEM. The results are as follows: Figure 6 As shown. Figure 6 From (b), we can see that the pure aluminum coating is granular, about 3um in size, with obvious gaps between the particles, and the density of the coating is poor.

[0072] Comparison between the above-mentioned Example 4 and Comparative Example 2 can illustrate that the present invention can achieve significantly good results in the amorphous aluminum-manganese alloy plating scheme in which the amorphous layer is used as a transition layer.

[0073] Therefore, it can be seen from the above comparative experiments that the present invention solves the problem of the loose zinc coating by using the amorphous aluminum-manganese alloy as the over-plating layer, and plays a decisive role in improving the corrosion resistance of the ionic liquid aluminum coating on the magnesium alloy.

[0074] The above specific implementation modes are used to explain the present invention rather than to limit the present invention. Any modification and change made to the present invention within the spirit of the present invention and the protection scope of the claims shall fall within the protection scope of the present invention.

[0075] The above description is only a preferred embodiment of the present invention, so all equivalent changes or modifications made according to the structure, characteristics and principles described in the scope of the patent application of the present invention are included in the scope of the patent application of the present invention.

Claims

1. A corrosion-resistant coating of amorphous aluminum-manganese alloy and aluminum composite on the surface of a magnesium alloy, characterized in that: The invention comprises an amorphous aluminum-manganese alloy coating and an aluminum coating located on the surface of the amorphous aluminum-manganese alloy coating.

2. The corrosion-resistant coating of amorphous aluminum-manganese alloy and aluminum composite on the surface of magnesium alloy according to claim 1, characterized in that: The amorphous aluminum-manganese alloy coating is plated on the surface of the magnesium alloy that has been subjected to zinc immersion treatment.

3. The corrosion-resistant coating of amorphous aluminum-manganese alloy and aluminum composite on the surface of magnesium alloy according to claim 1, characterized in that: The thickness of the amorphous aluminum-manganese alloy coating is 2-6 μm; the thickness of the aluminum coating is 12-20 μm.

4. The preparation method according to claim 1, characterized in that: The manganese content of the amorphous aluminum-manganese alloy coating is 8 to 16 at. %.

5. A method for preparing a corrosion-resistant coating of amorphous aluminum-manganese alloy and aluminum composite applied to the surface of the magnesium alloy according to any one of claims 1 to 4, characterized in that: After the magnesium alloy is zinc-impregnated to obtain a zinc-impregnated layer, an ionic liquid is used to plate on the surface of the zinc-impregnated layer to prepare an amorphous aluminum-manganese alloy coating, and then the ionic liquid is aluminum-plated to form an aluminum coating, and finally the coating is prepared after cleaning and drying.

6. The preparation method according to claim 5, characterized in that: The ionic liquid plating method for preparing the amorphous aluminum-manganese alloy is to use an ionic liquid plating solution of manganese chloride-aluminum chloride-1-ethyl 3-methyl imidazole chloride or manganese chloride-aluminum chloride-1-butyl 3-methyl imidazole chloride at a temperature of 25°C to 60°C and a current density of 6 to 15 mA / cm 2 The coating preparation is carried out below.

7. The preparation method according to claim 6, characterized in that: In the ionic liquid plating solution of manganese chloride-aluminum chloride-1-ethyl 3-methyl imidazole chloride, the content of manganese chloride MnCl2 is 0.1-0.2 mol / L, and the molar ratio between aluminum chloride AlCl3 and 1-ethyl 3-methyl imidazole chloride EMIC is (1.5-2.0):

1.

8. The preparation method according to claim 6, characterized in that: The ionic liquid aluminum plating is specifically using aluminum chloride-1-ethyl 3-methyl imidazole chloride, aluminum chloride-trimethyl aniline chloride or aluminum chloride-trimethyl benzyl ammonium chloride as the plating solution, at a temperature of 25°C to 80°C and a current density of 10 to 80 mA / cm 2 The coating is prepared under the following conditions; In the aluminum chloride-1-ethyl 3-methyl imidazole chloride plating solution, the molar ratio of aluminum chloride AlCl3 to 1-ethyl 3-methyl imidazole chloride EMIC is (1.5-2.0):

1.

9. A magnesium alloy surface, characterized in that: A corrosion-resistant coating comprising the amorphous aluminum-manganese alloy and aluminum composite as claimed in any one of claims 1 to 3.

10. A magnesium alloy surface according to claim 9, characterized in that: A zinc coating, an amorphous aluminum-manganese alloy coating and an aluminum coating are sequentially prepared on the surface of the magnesium alloy outward.

Citation Information

Patent Citations

  • Method for improving surface binding force of aluminum plating layer and magnesium alloy