Method and device for preparing metachromatic linen-like fabric polyester fibers
By adding 2,5,6,6-tetramethyl-2,5-heptanediol to the polyester melt and using POY and DTY processes, the long-term cooling problem caused by high temperature of polyester fiber dyeing is solved, and the dyeing is improved Efficiency and fiber performance enable efficient preparation of heterodyed enameled fabric polyester fibers.
Patent Information
- Application Number
- CN202410926718.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-01
AI Technical Summary
The existing heterodyed enameled fabric polyester fibers require high temperatures when dyeing, which causes the fibers to take a long time to cool after dyeing, which increases the preparation time and reduces efficiency.
2,5,6,6-tetramethyl-2,5-heptanediol was added to the polyester melt and mixed by spiral stirring, followed by filtering and spinning into primary fibers, and the POY and DTY processes were used to add the elastic and dyeing, and finally styling is performed to reduce the dyeing temperature and time.
It significantly shortens the dyeing time, improves the dyeing rate and bulkiness of the fiber, simplifies the preparation process, reduces costs, and improves the dyeing performance and efficiency.
Smart Images

Figure CN118880484A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyester fiber preparation, and in particular relates to a method and a device for preparing heterodyned linen-like polyester fibers. Background Art
[0002] The fabric woven from heterodyned linen-like polyester fiber has rich surface color, full hand feel, strong three-dimensional sense, good moisture permeability and air permeability, which is very similar to natural linen fabric. It is less prone to wrinkles and has higher elasticity than natural fiber fabrics, and is quite popular among consumers.
[0003] At present, most manufacturers use fibers with circular cross-sections to achieve the bamboo-node effect during winding and drawing. In the early stage of fiber formation, due to its large specific surface area, large temperature gradient and velocity gradient, its tensile viscosity and rheological resistance increase rapidly, making the fiber highly oriented. In the post-drawing process, uneven thickness of hairy fibers and bamboo nodes will occur, resulting in uneven color.
[0004] The prior art CN110528104A discloses a method for preparing a heterodyned linen-like polyester fiber and polyester fiber, which makes the orientations of various parts of the fiber consistent and avoids the formation of a skin-core structure, thereby reducing the temperature difference between spindle positions, ensuring that the temperature of each bundle of yarn and each strand is consistent, the strength of the yarn bundle and the elongation CV value are small, the dyeing is uniform, and the yarn uniformity is good.
[0005] However, when the polyester fiber is dyed, the temperature required for dyeing is relatively high, so that the dyed polyester fiber needs to spend a long time to cool down, thereby increasing the preparation time of the polyester fiber and reducing the preparation efficiency of the polyester fiber. Summary of the invention
[0006] The purpose of the present invention is to provide a method and device for preparing heterodyned linen-like polyester fibers, aiming to solve the technical problem that when dyeing existing polyester fibers, the temperature required for dyeing is relatively high, so that the dyed polyester fibers need to spend a long time to cool, thereby increasing the preparation time of the polyester fibers and reducing the preparation efficiency of the polyester fibers.
[0007] In order to achieve the above technical objectives, the technical solution adopted by the present invention is as follows:
[0008] The present invention provides a method for preparing a meta-dyed linen-like polyester fiber, comprising the following steps:
[0009] Firstly, a polyester melt is prepared, and then 2,5,6,6-tetramethyl-2,5-heptanediol is added to the polyester melt, and the mixture is stirred and mixed to obtain a modified polyester melt mixed liquid;
[0010] The polyester melt mixture is filtered, and the filtered polyester melt mixture is extruded from the spinneret holes of a spinneret formed by a plurality of "H"-shaped combinations to obtain primary fibers;
[0011] Cooling the primary fibers, and after cooling, using a POY process to make the primary fibers into POY tows with uniform thickness;
[0012] The POY tow is subjected to a texturing treatment by using a DTY process, and after the texturing treatment, the POY tow is dyed to obtain a secondary fiber;
[0013] The secondary fibers are cooled, and after cooling, the secondary fibers are subjected to a shaping treatment to obtain the desired meta-dyed linen-like fabric polyester fibers.
[0014] Wherein, the specific method of preparing the polyester melt is:
[0015] Using purified terephthalic acid and ethylene glycol as raw materials, diethylene glycol as an additive, and ethylene glycol antimony as a catalyst, a slurry with a PTA content of (70±5)% is prepared, and then an esterification reaction is carried out;
[0016] After the esterification reaction, a catalyst is added to the slurry again, and the slurry is allowed to start a polycondensation reaction under negative pressure to prepare a polyester melt.
[0017] The stirring and mixing of the polyester melt and the 2,5,6,6-tetramethyl-2,5-heptanediol is achieved by using a propeller blade in a spiral stirring manner.
[0018] The stirring and mixing time of the polyester melt and the 2,5,6,6-tetramethyl-2,5-heptanediol is 30 minutes.
[0019] The polyester melt mixed liquid is filtered in a filter sand with high profile for filtering impurities in the polyester melt.
[0020] Among them, the leaf width of the "H"-shaped spinneret is 0.05mm, and the "H"-shaped spinneret includes two horizontal leaves and a vertical leaf perpendicular to the two horizontal leaves. The length of the vertical leaf is 0.45mm, the length of the two horizontal leaves is 0.15mm, and the hole depth is 0.35mm.
[0021] The present invention also provides a preparation device for heterodyne linen-like fabric polyester fiber, comprising a polyester melt preparation box, a stirring and mixing box, a filtering box, a first extruder, a second extruder, a DTY device, a dyeing machine and a setting machine, wherein the stirring and mixing box is provided with a propeller blade, the filtering box is provided with filtering sand, the first extruder is provided with a plurality of "H"-shaped spinnerets, and the polyester melt preparation box comprises an esterification reaction chamber and a polycondensation reaction chamber;
[0022] The esterification reaction chamber is used to perform an esterification reaction on the raw materials for preparing the polyester melt to obtain a slurry;
[0023] The polycondensation reaction chamber is used to perform polycondensation reaction on the slurry obtained after the esterification reaction to prepare a polyester melt;
[0024] The stirring and mixing box is used to stir and mix the polyester melt and 2,5,6,6-tetramethyl-2,5-heptanediol to obtain a modified polyester melt mixed liquid;
[0025] The filter box is used to filter the polyester melt mixture;
[0026] The first extruder is used to extrude the filtered polyester melt mixture from the spinneret holes of a spinneret formed by a plurality of "H"-shaped combinations to obtain primary fibers;
[0027] The second extruder is used to produce POY tows with uniform thickness from primary fibers using a POY process;
[0028] The DTY equipment is used to perform texturing treatment on POY tow using the DTY process;
[0029] The dyeing machine is used to dye the POY tow after the texturing treatment to obtain secondary fibers;
[0030] The shaping machine is used for shaping the secondary fibers.
[0031] The invention discloses a preparation method and device of a heterodyne type linen-like fabric polyester fiber. The invention adds 2,5,6,6-tetramethyl-2,5-heptanediol to a prepared polyester melt, thereby modifying the polyester melt, thereby reducing the dyeing temperature, shortening the dyeing time, increasing the dyeing rate of the fiber, and significantly improving the dyeing performance. After filtering the polyester melt mixed liquid, the filtered polyester melt mixed liquid is extruded from the spinneret holes of a spinneret formed by a plurality of "H"-shaped combinations, thereby making the prepared heterodyne type linen-like fabric polyester fiber have better bulkiness and a wider application range. By sequentially adopting a POY process, a DTY process and a shaping treatment to primary fibers, the preparation method of the prepared heterodyne type linen-like fabric polyester fiber is simple and easy to implement, and has low cost, thereby being easier to promote and apply. The invention solves the technical problem that when dyeing the existing polyester fiber, the temperature required for dyeing is high, so that the dyed polyester fiber needs to spend a long time to cool, thereby increasing the preparation time of the polyester fiber and reducing the preparation efficiency of the polyester fiber. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The present invention is further illustrated by means of the non-limiting examples given in the accompanying drawings.
[0033] Figure 1 It is a process step diagram of a method for preparing a meta-dyed linen-like fabric polyester fiber according to a first embodiment of the present invention.
[0034] Figure 2 The present invention is a flow chart of the preparation of polyester melt in the method for preparing the meta-dyed linen-like fabric polyester fiber according to the first embodiment of the present invention.
[0035] Figure 3 It is a preparation flow chart of a device for preparing meta-dyed linen-like fabric polyester fiber according to the second embodiment of the present invention.
[0036] In the figure: 101-polyester melt preparation box, 102-stirring mixing box, 103-filtering box, 104-first extruder, 105-second extruder, 106-DTY equipment, 107-dyeing machine, 108-setting machine, 109-esterification reaction chamber, 110-polycondensation reaction chamber. DETAILED DESCRIPTION
[0037] In order to enable those skilled in the art to better understand the present invention, the technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0038] First embodiment
[0039] See also Figure 1-2 , Figure 1 1 is a flow chart of the preparation method of the meta-dyed linen-like polyester fiber of the first embodiment of the present invention, Figure 2The present invention is a flow chart of the preparation of polyester melt in the method for preparing the meta-dyed linen-like fabric polyester fiber according to the first embodiment of the present invention.
[0040] The present invention provides a method for preparing a meta-dyed linen-like polyester fiber, comprising the following steps:
[0041] S101, first preparing a polyester melt, then adding 2,5,6,6-tetramethyl-2,5-heptanediol to the polyester melt, and stirring and mixing to obtain a modified polyester melt mixed solution;
[0042] S102, filtering the polyester melt mixture, and extruding the filtered polyester melt mixture from spinneret holes formed by a plurality of "H"-shaped spinnerets to obtain primary fibers;
[0043] S103, cooling the primary fibers, and after cooling, using a POY process to make the primary fibers into POY tows with uniform thickness;
[0044] S104, texturizing the POY tow using a DTY process, and dyeing the POY tow after the texturizing process to obtain secondary fibers;
[0045] S105, cooling the secondary fibers, and after cooling, performing a shaping treatment on the secondary fibers to obtain the desired meta-dyed linen-like fabric polyester fibers.
[0046] In this embodiment, the present invention adds 2,5,6,6-tetramethyl-2,5-heptanediol to the prepared polyester melt, thereby modifying the polyester melt, thereby reducing the dyeing temperature, shortening the dyeing time, increasing the dyeing rate of the fiber, and significantly improving the dyeing performance. After filtering the polyester melt mixture, the filtered polyester melt mixture is extruded from the spinneret holes of a spinneret composed of a plurality of "H"-shaped combinations, so that the prepared heterodyne type linen-like fabric polyester fiber has better bulkiness and a wider range of applications. By sequentially adopting the POY process, the DTY process and the shaping treatment for the primary fiber, the preparation method of the prepared heterodyne type linen-like fabric polyester fiber is simple and easy, and has low cost, and is easier to promote and apply, thereby solving the technical problem that when the existing polyester fiber is dyed, the temperature required for dyeing is high, so that the dyed polyester fiber needs to spend a long time to cool, thereby increasing the preparation time of the polyester fiber and reducing the preparation efficiency of the polyester fiber.
[0047] Wherein, the specific method of preparing the polyester melt is:
[0048] S106, using purified terephthalic acid and ethylene glycol as raw materials, diethylene glycol as an additive, and ethylene glycol antimony as a catalyst, preparing a slurry with a PTA content of (70±5)%, and then performing an esterification reaction;
[0049] S107. After the esterification reaction, a catalyst is added to the slurry again, and the slurry is allowed to start a polycondensation reaction under negative pressure to prepare a polyester melt.
[0050] Secondly, the stirring and mixing of the polyester melt and the 2,5,6,6-tetramethyl-2,5-heptanediol is achieved by using a propeller blade to stir in a spiral manner, and the stirring and mixing time of the polyester melt and the 2,5,6,6-tetramethyl-2,5-heptanediol is 30 minutes.
[0051] Thirdly, the polyester melt mixture is filtered in a filter sand containing high profile filter sand for filtering impurities in the polyester melt.
[0052] Meanwhile, the leaf width of the "H"-shaped spinneret is 0.05 mm, and the "H"-shaped spinneret includes two transverse leaves and a vertical leaf perpendicular to the two transverse leaves, the vertical leaf is 0.45 mm long, the two transverse leaves are both 0.15 mm long, and the hole depth is 0.35 mm.
[0053] In addition, the process parameters of the POY process are: cooling temperature 23-28° C., cooling wind speed 1.55-1.95 m / s, spinning temperature 280-320° C., and winding speed 3000-3500 m / min.
[0054] Finally, the process parameters of the DTY process are: spinning speed 400-650 m / min, shaping overfeed rate 1.5-3.8%, winding overfeed rate 1.5-2.5%, and stretching multiple 1.5-1.8.
[0055] When using the method for preparing a heterodyned linen-like fabric polyester fiber of the present embodiment, purified terephthalic acid and ethylene glycol are used as raw materials, diethylene glycol is used as an additive, and ethylene glycol antimony is used as a catalyst. After preparing a slurry with a PTA content of (70±5)%, an esterification reaction is carried out. After the esterification reaction, the catalyst is added to the slurry again, and the slurry is allowed to start a condensation reaction under negative pressure conditions to prepare a polyester melt.
[0056] After preparing the polyester melt, 2,5,6,6-tetramethyl-2,5-heptanediol is added to the polyester melt, and the polyester melt and 2,5,6,6-tetramethyl-2,5-heptanediol are stirred and mixed by a propeller blade in a spiral stirring manner for 30 minutes to obtain a modified polyester melt mixture. Thereafter, the polyester melt mixture is filtered in a filter sand with a high degree of special shape for filtering impurities in the polyester melt, and the filtered polyester melt mixture is extruded from the spinneret holes of a spinneret composed of a plurality of "H" shapes to obtain primary fibers, wherein the leaf width of the "H"-shaped spinneret is 0.05 mm, and the "H"-shaped spinneret includes two horizontal leaves and a vertical leaf perpendicular to the two horizontal leaves, the vertical leaf is 0.45 mm long, the two horizontal leaves are both 0.15 mm long, and the hole depth is 0.35 mm.
[0057] Then, the primary fiber is cooled, and after cooling, the primary fiber is made into a POY tow with uniform thickness by using a POY process, and the process parameters of the POY process are: cooling temperature 23-28°C, cooling wind speed 1.55-1.95m / s, spinning temperature 280-320°C, winding speed 3000-3500m / min, and then the POY tow is subjected to a DTY process for elastic treatment, and after the elastic treatment, the POY tow is dyed to obtain a secondary fiber, and the process parameters of the DTY process are: spinning speed 400-650m / min, shaping overfeed rate 1.5-3.8%, winding overfeed rate 1.5-2.5%, and stretching multiple 1.5-1.8. Finally, the secondary fiber is cooled, and after cooling, the secondary fiber is subjected to a shaping treatment to obtain the desired heterodyned linen-like fabric polyester fiber.
[0058] In summary, the present invention adds 2,5,6,6-tetramethyl-2,5-heptanediol to the prepared polyester melt, thereby modifying the polyester melt, thereby reducing the dyeing temperature, shortening the dyeing time, increasing the dyeing rate of the fiber, and significantly improving the dyeing performance. After filtering the polyester melt mixture, the filtered polyester melt mixture is extruded from the spinneret holes of a spinneret formed by a plurality of "H"-shaped combinations, thereby making the prepared heterodyne type linen-like fabric polyester fiber have better bulkiness and a wider application range. By sequentially adopting the POY process, the DTY process and the shaping treatment to the primary fiber, the preparation method of the prepared heterodyne type linen-like fabric polyester fiber is simple and easy, and has low cost, and is easier to promote and apply, and solves the technical problem that when the existing polyester fiber is dyed, the temperature required for dyeing is high, so that the dyed polyester fiber needs to spend a long time to cool, thereby increasing the preparation time of the polyester fiber and reducing the preparation efficiency of the polyester fiber.
[0059] Second embodiment
[0060] See also Figure 3 , Figure 3 The present invention is a preparation flow chart of a preparation device for a metachromatic linen-like fabric polyester fiber according to a second embodiment of the present invention. Based on the first embodiment, the present invention further provides a preparation device for a metachromatic linen-like fabric polyester fiber, comprising a polyester melt preparation box 101, a stirring and mixing box 102, a filtering box 103, a first extruder 104, a second extruder 105, a DTY device 106, a dyeing machine 107 and a setting machine 108, wherein the polyester melt preparation box 101 comprises an esterification reaction chamber 109 and a polycondensation reaction chamber 110.
[0061] In this embodiment, the polyester melt preparation box 101, the stirring and mixing box 102, the filtering box 103, the first extruder 104, the second extruder 105, the DTY equipment 106, the dyeing machine 107 and the setting machine 108 are used in coordination, so that the desired heterodyned linen-like fabric polyester fiber can be prepared, and the dyeing temperature is reduced, the dyeing time is shortened, the dyeing rate of the fiber is increased, and the dyeing performance is significantly improved.
[0062] The stirring and mixing box 102 is provided with a propeller blade, the filtering box 103 is provided with filtering sand, and the first extruder 104 is provided with a plurality of "H"-shaped spinnerets;
[0063] The esterification reaction chamber 109 is used to perform an esterification reaction on the raw materials for preparing the polyester melt to obtain a slurry;
[0064] The polycondensation reaction chamber 110 is used to perform polycondensation reaction on the slurry obtained after the esterification reaction to prepare a polyester melt;
[0065] The stirring and mixing box 102 is used to stir and mix the polyester melt and 2,5,6,6-tetramethyl-2,5-heptanediol to obtain a modified polyester melt mixed liquid;
[0066] The filter box 103 is used to filter the polyester melt mixture;
[0067] The first extruder 104 is used to extrude the filtered polyester melt mixture from the spinneret holes of a spinneret formed by a plurality of "H"-shaped combinations to obtain primary fibers;
[0068] The second extruder 105 is used to use the POY process to make the primary fibers into POY tows with uniform thickness;
[0069] The DTY device 106 is used to perform texturing on the POY tow using the DTY process;
[0070] The dyeing machine 107 is used to dye the POY tow after the texturing treatment to obtain secondary fibers;
[0071] The shaping machine 108 is used to shape the secondary fibers.
[0072] When using the device for preparing the heterodyned linen-like fabric polyester fiber of the present embodiment, purified terephthalic acid and ethylene glycol are used as raw materials, diethylene glycol is used as an additive, and ethylene glycol antimony is used as a catalyst. After preparing a slurry with a PTA content of (70±5)%, the slurry is poured into the esterification reaction chamber 109 for esterification reaction. After the esterification reaction, the slurry after the reaction is poured into the polycondensation reaction chamber 110, and the catalyst is added to the slurry again. Under negative pressure conditions, the slurry is allowed to start a polycondensation reaction to prepare a polyester melt.
[0073] After the polyester melt is prepared, the polyester melt is poured into the stirring and mixing box 102, 2,5,6,6-tetramethyl-2,5-heptanediol is added to the polyester melt, and the polyester melt and 2,5,6,6-tetramethyl-2,5-heptanediol are stirred and mixed by a propeller blade in a spiral stirring manner for 30 minutes to obtain a modified polyester melt mixed liquid, and then the polyester melt mixed liquid is poured into the filter box 103, and the filter box 103 is equipped with a high-profile filter for filtering impurities in the polyester melt. The polyester melt mixture is filtered in the filter sand of the first extruder 104, and the filtered polyester melt mixture is transmitted to the first extruder 104, so that the polyester melt is extruded from the spinneret holes of the spinneret composed of multiple "H" shapes in the first extruder 104 to obtain primary fibers, wherein the leaf width of the "H"-shaped spinneret is 0.05mm, and the "H"-shaped spinneret includes two horizontal leaves and a vertical leaf perpendicular to the two horizontal leaves, the vertical leaf is 0.45mm long, the two horizontal leaves are 0.15mm long, and the hole depth is 0.35mm.
[0074] Then, the primary fiber is cooled, and after cooling, the primary fiber is transferred to the second extruder 105, and the primary fiber is made into a POY tow with uniform thickness by using the POY process in the second extruder 105. The process parameters of the POY process are: cooling temperature 23-28°C, cooling wind speed 1.55-1.95m / s, spinning temperature 280-320°C, winding speed 3000-3500m / min, and then the prepared POY tow is transferred to the DTY device 106, and the DTY device 106 is used. The TY process is used to perform texturing on the POY tow, and after the texturing treatment, the POY tow is dyed by the dyeing machine 107 to obtain secondary fibers. The process parameters of the DTY process are: spinning speed 400-650 m / min, shaping overfeed rate 1.5-3.8%, winding overfeed rate 1.5-2.5%, stretching multiple 1.5-1.8. Finally, the secondary fibers are cooled, and after cooling, the secondary fibers are shaped by the shaping machine 108 to obtain the desired heterodyned linen-like polyester fibers.
[0075] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by those with ordinary knowledge in the technical field without departing from the spirit and technical ideas disclosed by the present invention should still be covered by the claims of the present invention.
Claims
1. A method for preparing a metachromatic linen-like fabric polyester fiber, characterized in that: The following steps are involved: Firstly, a polyester melt is prepared, and then 2,5,6,6-tetramethyl-2,5-heptanediol is added to the polyester melt, and the mixture is stirred and mixed to obtain a modified polyester melt mixed liquid; The polyester melt mixture is filtered, and the filtered polyester melt mixture is extruded from the spinneret holes of a spinneret formed by a plurality of "H"-shaped combinations to obtain primary fibers; Cooling the primary fibers, and after cooling, using a POY process to make the primary fibers into POY tows with uniform thickness; The POY tow is subjected to a texturing treatment by using a DTY process, and after the texturing treatment, the POY tow is dyed to obtain a secondary fiber; The secondary fibers are cooled, and after cooling, the secondary fibers are subjected to a shaping treatment to obtain the desired meta-dyed linen-like fabric polyester fibers.
2. The method for preparing the metachromatic linen-like fabric polyester fiber according to claim 1, characterized in that: The specific method for preparing the polyester melt is: Using purified terephthalic acid and ethylene glycol as raw materials, diethylene glycol as an additive, and ethylene glycol antimony as a catalyst, a slurry with a PTA content of (70±5)% is prepared, and then an esterification reaction is carried out; After the esterification reaction, a catalyst is added to the slurry again, and the slurry is allowed to start a polycondensation reaction under negative pressure to prepare a polyester melt.
3. The method for preparing the metachromatic linen-like fabric polyester fiber according to claim 1, characterized in that: The stirring and mixing of the polyester melt and the 2,5,6,6-tetramethyl-2,5-heptanediol is achieved by using a propeller blade in a spiral stirring manner.
4. The method for preparing the metachromatic linen-like fabric polyester fiber according to claim 3, characterized in that: The stirring mixing time of the polyester melt and the 2,5,6,6-tetramethyl-2,5-heptanediol is 30 minutes.
5. The method for preparing the metachromatic linen-like fabric polyester fiber according to claim 1, characterized in that: The polyester melt mixed liquid is filtered in a filter sand filled with high profile filter sand for filtering impurities in the polyester melt.
6. The method for preparing the metachromatic linen-like polyester fiber according to claim 1, characterized in that: The leaf width of the "H"-shaped spinneret is 0.05mm, and the "H"-shaped spinneret includes two transverse leaves and a vertical leaf perpendicular to the two transverse leaves, the vertical leaf is 0.45mm long, the two transverse leaves are both 0.15mm long, and the hole depth is 0.35mm.
7. A device for preparing metachromatic linen-like polyester fibers, applied to the method for preparing metachromatic linen-like polyester fibers according to any one of claims 1 to 6, characterized in that: It includes a polyester melt preparation box, a stirring and mixing box, a filtering box, a first extruder, a second extruder, a DTY device, a dyeing machine and a setting machine. The stirring and mixing box is provided with a propeller blade, the filtering box is provided with filtering sand, the first extruder is provided with a plurality of "H"-shaped spinnerets, and the polyester melt preparation box includes an esterification reaction chamber and a polycondensation reaction chamber; The esterification reaction chamber is used to perform an esterification reaction on the raw materials for preparing the polyester melt to obtain a slurry; The polycondensation reaction chamber is used to perform polycondensation reaction on the slurry obtained after the esterification reaction to prepare a polyester melt; The stirring and mixing box is used to stir and mix the polyester melt and 2,5,6,6-tetramethyl-2,5-heptanediol to obtain a modified polyester melt mixed liquid; The filter box is used to filter the polyester melt mixture; The first extruder is used to extrude the filtered polyester melt mixture from the spinneret holes of a spinneret formed by a plurality of "H"-shaped combinations to obtain primary fibers; The second extruder is used to produce POY tows with uniform thickness from primary fibers using a POY process; The DTY equipment is used to perform texturing treatment on POY tow using the DTY process; The dyeing machine is used to dye the POY tow after the texturing treatment to obtain secondary fibers; The shaping machine is used for shaping the secondary fibers.
