Preparation process of modified terylene extra-black profiled cotton-like filament fiber

Through the preparation process of modified polyester special black special-shaped cotton filament fibers, the problems of unstable blackness and small elongation of black fibers are solved, and high-quality, soft and fluffy fibers are prepared, suitable for high-end products and meet the market For high quality and personalized needs.

CN118880485APending Publication Date: 2024-11-01HUZHOU ZHONGYUE CHEM FIBER CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410933927.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the prior art, the blackness of black fibers is not stable enough and the elongation and elongation is small, resulting in more wool filaments in imitation cotton products, affecting quality and efficiency, and it is difficult to meet high quality and personalized needs.

Method used

Modified polyester special black special-shaped cotton filament fiber preparation technology is adopted to prepare modified semi-gloss white PET melt through copolymerization and blend polycondensation reaction, and mix it with black masterbatch, and extrude it by spinneret orifice assembly to obtain primary silk After multiple grid connection and drafting treatments, high-quality modified polyester extra-black special-shaped cotton filament fibers are formed.

Benefits of technology

It improves the blackness stability and elongation of the fiber, reduces the number of wool, and prepares a soft and fluffy fabric with high absorbency and high added value, suitable for high-end products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880485A_ABST
    Figure CN118880485A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation process of modified polyester extra-black profiled cotton-like filament fibers, and relates to the technical field of polyester black yarn cotton-like fiber production, the method comprises the following steps: preparing a modified semi-gloss raw white PET melt by using a copolymerization blending polycondensation reaction, filtering and pressurizing the modified semi-gloss raw white PET melt, and introducing the filtered and pressurized modified semi-gloss raw white PET melt into a dynamic mixer; preparing a modified extra-black polyester PET melt by combining the black master batch and the modified semi-gloss raw white PET melt, and extruding through a spinneret orifice plate assembly to obtain a first nascent filament and a second nascent filament; preparing a modified extra-black foreign fiber PET-POY (Polyester Pre-Oriented Yarn) product by utilizing the first nascent filaments, and preparing a modified extra-black foreign fiber PET-FOY product by utilizing the second nascent filaments; the modified terylene extra-black profiled cotton-like filament fiber is prepared based on the modified extra-black foreign fiber PET-POY product and the modified extra-black foreign fiber PET-FOY product. The invention prepares the modified terylene extra-black profiled cotton-like filament fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyester black silk cotton-like fiber production, in particular to a preparation process of modified polyester extra-black special-shaped cotton-like filament fibers. Background Art

[0002] In recent years, with the enhancement of environmental awareness and the popularization of the concept of sustainable development, colored fibers have received extensive attention due to their unique environmental advantages. There is no need for dyeing in the production process of colored fibers, which not only greatly reduces the wastewater discharge generated during the dyeing process, but also saves about 60% of carbon emissions compared with traditional dyed fabrics. This fiber effectively reduces working hours during the production process and improves the efficiency of the entire production process from fiber to fabric; taking black fiber as an example, as an important member of colored fibers, it has been widely used in the fields of home textiles, sports and outdoor products. At present, polyester spinning companies generally use online injection addition to add black masterbatch melt to semi-light ordinary melt at a ratio of 4% to 6% to produce black fibers. This method simplifies the production process, reduces production costs, and also meets the basic market demand for black fibers.

[0003] However, although the existing fiber production technology has met the market demand to a certain extent, it still has some obvious limitations: first, the ordinary black silk market has become saturated, the products are seriously homogenized, lack of innovation and differentiation, and it is difficult to meet consumers' demand for high-quality and personalized products; second, the blackness of ordinary black fibers is not enough, and the blackness of fiber fabrics is not strong, and they cannot provide a deep black visual effect, which to a certain extent limits the application scope and market competitiveness of the products; in addition, the products of mixed spinning of ordinary semi-gloss melt and ordinary black melt have a small elongation when producing fine denier imitation cotton products, and are prone to produce hairy fibers, which not only affects the quality of the product, but also reduces the weaving efficiency.

[0004] The existing technology has the problems of weak blackness, low elongation and much hair in the fine-denier cotton-like products. Therefore, there is an urgent need for a preparation process of modified polyester extra-black special-shaped cotton-like filament fibers. By innovating the fiber production technology, product differentiation can be improved, blackness stability can be enhanced, and the prepared product fabric can be soft and fluffy with a high dyeing rate to solve the shortcomings of the existing technology.

[0005] Currently, no effective solution has been proposed for the problems in the related technologies. Summary of the invention

[0006] In view of the problems in the related art, the present invention proposes a preparation process of modified polyester extra black special-shaped cotton-like filament fiber, which has the advantages of soft and fluffy product fabric, high dyeing rate and deep color absorption, thereby solving the problems of weak blackness, small elongation and much hair in the production of fine denier cotton-like products in the prior art.

[0007] To this end, the specific technical solution adopted by the present invention is as follows:

[0008] A preparation process of modified polyester extra black special-shaped cotton-like filament fibers, the preparation process of modified polyester extra black special-shaped cotton-like filament fibers comprising the following steps:

[0009] S1, preparing a modified semi-gloss white PET melt by copolymerization and blending polycondensation reaction, and filtering and pressurizing the modified semi-gloss white PET melt and then passing it into a dynamic mixer;

[0010] S2, combining the black masterbatch with the modified semi-gloss white PET melt to prepare a modified ultra-black polyester PET melt, and extruding it through a spinneret orifice assembly to obtain a first primary filament and a second primary filament;

[0011] S3, using the first primary filament to prepare a modified special black foreign fiber PET-POY product, and using the second primary filament to prepare a modified special black foreign fiber PET-FOY product;

[0012] S4. Based on the modified extra black foreign fiber PET-POY product and the modified extra black foreign fiber PET-FOY product, the modified polyester extra black special-shaped cotton-like filament fiber is prepared.

[0013] Further, preparing a modified semi-gloss white PET melt by copolymerization and blending polycondensation reaction, and filtering and pressurizing the modified semi-gloss white PET melt and then passing it into a dynamic mixer comprises the following steps:

[0014] S11, using a slurry regulating valve to adjust the flow rate of pentaerythritol slurry, and passing the slurry into the slurry feeding tank under the action of gravity;

[0015] S12, the pentaerythritol slurry is mixed with the PTA and EG suspension in the slurry feeding tank to obtain a slurry mixture, and the slurry mixture is introduced into the esterification reactor by a slurry delivery pump to obtain an oligomer by a blending esterification reaction under preset temperature and preset pressure conditions;

[0016] S13, the oligomer is passed into a pre-polycondensation reaction kettle through an oligomer pipeline to carry out a pre-polycondensation reaction to obtain a prepolymer;

[0017] S14, the prepolymer is delivered to the final polymerization kettle through a delivery pump for copolymerization, blending and polycondensation reaction to obtain a modified semi-gloss white PET melt.

[0018] S15, using a melt pump to pass the modified semi-gloss white PET melt into a melt filter for filtering;

[0019] S16, using a spinning booster pump to pass the filtered modified semi-gloss white PET melt into a melt cooler for cooling, and then sending it into a dynamic mixer through a pipeline.

[0020] Further, combining the black masterbatch with the modified semi-gloss white PET melt to prepare a modified ultra-black polyester PET melt, and extruding it through a spinneret orifice assembly to obtain a first primary filament and a second primary filament includes the following steps:

[0021] S21, using a drying tower to remove moisture from the black masterbatch, and passing it into a screw extruder for extrusion to obtain a black melt;

[0022] S22, using a syringe pump to measure the black melt and passing it into a dynamic mixer, mixing it with the modified semi-gloss white PET melt to obtain a modified special black polyester PET melt;

[0023] S23, passing the modified special black polyester PET melt into the spinning manifold, and metering it by using the metering pump assembly 18;

[0024] S24. Based on the metering results, a modified extra black polyester PET melt is extruded through a spinneret orifice assembly, and passed through a ring blower for cooling to obtain a first primary filament and a second primary filament.

[0025] Further, preparing a modified special black foreign fiber PET-POY product using the first primary filament, and preparing a modified special black foreign fiber PET-FOY product using the second primary filament comprises the following steps:

[0026] S31, based on the first primary filament, using the guide disc assembly and the first network device to prepare a modified special black foreign fiber PET-POY product;

[0027] S32. Based on the second primary filament, a modified special black foreign fiber PET-FOY product is prepared by using a guide wire disc assembly and a main network device.

[0028] Further, based on the first primary filament, preparing the modified special black foreign fiber PET-POY product by using the godet assembly and the first network device includes the following steps:

[0029] S311, applying oil to the first primary filaments by using a first spinning oil nozzle, and homogenizing the oil of the first primary filaments by using a first spinning oil nozzle;

[0030] S312, adjusting the tension of the first primary filament by using the first guide wire disc A and the second guide wire disc A;

[0031] S313, using the first winding head to wind the adjusted first spun filament to obtain an ultra-black PET-POY product.

[0032] Further, based on the second primary filament, the modified special black foreign fiber PET-FOY product is prepared by using a godet assembly and a main network device, including the following steps:

[0033] S321, applying oil to the second primary filaments by using a second spinning oil nozzle, and homogenizing the oil of the second primary filaments by using a pre-spinning device;

[0034] S322, heating the second primary filament by using a heat pipe, and adjusting the tension by using the first guide wire disc B and the second guide wire disc B;

[0035] S323, using a second winding head to wind the adjusted second primary filament to obtain an ultra-black special-shaped PET-FOY product.

[0036] Furthermore, based on the modified special black foreign fiber PET-POY product and the modified special black foreign fiber PET-FOY product, the preparation of modified polyester special black special-shaped cotton-like filament fiber includes the following steps:

[0037] S41, passing the modified special black foreign fiber PET-POY product and the modified special black foreign fiber PET-FOY product into a zero roller for plying, and passing them into a second network device for grid connection;

[0038] S42, passing the product obtained by the network connection into a roller, an upper heat box, a cooling plate, a false twister and an intermediate roller for drawing and false twisting deformation, and using a lower heat box for stress elimination;

[0039] S43, using the winding laro winding stress-eliminated product to obtain modified polyester special black special-shaped cotton-like filament fibers.

[0040] Further, the addition ratio of pentaerythritol slurry is 110ppm-120ppm, the melt viscosity of the modified semi-gloss white PET is 0.615-0.620dL / g, the melting point of the modified semi-gloss white PET is 260±3°C, and the terminal shrinkage of the modified semi-gloss white PET is 45mol / t-50mol / t;

[0041] The black masterbatch contains carbon black in an effective concentration of 30%-35%. After the black masterbatch is extruded and melted by a screw extruder, it is injected into the dynamic mixer through an injection pump at an addition ratio of 10%-12%, and the rotation speed of the dynamic mixer is set to 35rpm-45rpm.

[0042] Further, the spinning box temperature is 275°C-280°C, the metering pump assembly includes two metering pumps and the speeds are independently controlled;

[0043] The spinning assembly includes a spinning assembly A and a spinning assembly B, and the number of the spinning assembly A and the number of the spinning assembly B are both 6;

[0044] The spinneret orifice plate assembly includes a spinneret orifice plate A and a spinneret orifice plate B. The number of spinneret orifice plates A and B are both 6. The number of holes of spinneret orifice plates A and spinneret orifice plate B is different. The cross section of the spinneret holes of spinneret orifice plate A is set to circular holes, and the cross section of the spinneret holes of spinneret orifice plate B is set to special-shaped holes. The spinneret holes of spinneret orifice plate A and spinneret orifice plate B are symmetrically distributed. The number of holes of spinneret orifice plate A is 72-144 holes, and the number of holes of spinneret orifice plate B is 48-96 holes. Spinneret orifice plate A and spinneret orifice plate B both extrude 12 bundles of filaments.

[0045] Furthermore, the oiling heights of the first spinning oil nozzle and the second spinning oil nozzle are independently adjustable, and the oiling height of the first spinning oil nozzle is 500mm-600mm;

[0046] The speeds of the first and second guide wire reels A are set to 3400m / min-3500m / min, the speed of the first winding head is set to 3400m / min-3500m / min, and the network pressure of the first network device is set to 0.5bar-0.7bar;

[0047] The oiling height of the second spinning nozzle is 800mm-1000mm, the heating temperature of the heat pipe is 150℃-170℃, the speed of the first godet B is set to 4000m / min-4200m / min, the speed of the second godet B is set to 4150m / min-4250m / min, the speed of the second winding head is set to 4200m / min-4300m / min, the pressure of the pre-network device is set to 0.8-1.0bar, and the pressure of the main network device is set to 2.5bar-3.0bar;

[0048] The grid-connected pressure of the second network device is set to 3bar~4bar, and the modified extra black foreign fiber PET-POY product and the modified extra black foreign fiber PET-FOY product are network-connected between the zero roller and the first roller at an overfeed rate of 100%-110%. The upper heat box temperature is set to 200℃~220℃, and the lower heat box temperature is set to 50℃~100℃.

[0049] The beneficial effects of the present invention are:

[0050] (1) The present invention adjusts the addition ratio and addition position of the three monomers pentaerythritol, changes the addition in the polymer pipeline to the addition in the slurry feeding tank, controls the addition ratio between 110ppm and 120ppm, and adopts the method of adding in the slurry feeding tank, so that the three monomers of pentaerythritol can participate in the reaction more fully. At the same time, by controlling the appropriate addition ratio, the floating fibers in the spinning process are reduced and the elongation of the polyester PET-POY / FOY product is improved. The obtained product fabric is soft and fluffy, has a high dyeing rate, and a deep color absorption degree.

[0051] (2) The present invention optimizes the terminal shrinkage content of the polyester melt, controls the terminal shrinkage content to be above 45 mol / t, adjusts the heating and insulation temperature during melt transportation to be maintained between 270°C and 272°C, and controls the viscosity drop of the melt to be less than 0.008 dg / L, thereby avoiding the large-scale accumulation of white powder on the spinning line and reducing the number of spinning filaments and hairy filaments caused by the addition of three monomers.

[0052] (3) The present invention optimizes the box temperature by selecting two metering pumps of different specifications and spinneret orifice plates with different hole cross-sections. Two different specifications of filaments are wound at different speeds to obtain two PET-POY and PET-FOY with two different molecular structures, thereby achieving the goal of obtaining two products of different specifications, different fiber cross-sections, and different molecular structures in the same spinning position.

[0053] (4) The present invention reduces the characteristic viscosity of the mixed melt of semi-gloss PET melt and black masterbatch by significantly increasing the addition ratio of black masterbatch, thereby improving the blackness of the melt; at the same time, by installing a double-channel network of a pre-network and a winding main network under the spinning nozzle, and adding a temperature-adjustable short heat pipe before the winding head to heat the filaments, the stress during the spinning process is reduced, the adhesion between the single filaments is increased, and the problem of fuzzy fibers in the high-speed spinning process of the modified ultra-black PET melt is solved.

[0054] (5) The present invention utilizes two kinds of special black PET-POY and special black special-shaped PET-FOY products with different orientation and crystal structure, which are connected and ply-coated on a texturing machine, and then go through heating, drawing and false twisting processes, and then enter a shaping hot box to eliminate internal stress, and then are wound and formed. The obtained product fabric has a special black luster visual sense, ultra-soft and delicate cotton feel and fluffiness, and the effect of rapid moisture absorption and quick drying.

[0055] (6) The modified polyester special black shaped imitation cotton fabric produced by the process of the present invention has high strength, wear resistance, light texture, soft skin-friendly, fluffy and warm cotton feeling and dazzling black color, and has the functions of moisture absorption and quick drying, and environmental protection and greenness. It can be used for high imitation fur, high-end plush toys, jacket lining, high-end sofa leather base, etc., and the product has high added value, broad market prospects and good economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0057] Figure 1It is a schematic diagram of a process for preparing a modified polyester special black shaped cotton-like filament fiber according to an embodiment of the present invention;

[0058] Figure 2 This is one of the specific implementation diagrams of a preparation process of a modified polyester special black shaped cotton-like filament fiber according to an embodiment of the present invention;

[0059] Figure 3 This is a second specific implementation diagram of a process for preparing a modified polyester special black shaped cotton-like filament fiber according to an embodiment of the present invention;

[0060] Figure 4 This is a process flow chart of modified polyester special black special-shaped cotton-like DTY according to an embodiment of the present invention;

[0061] Figure 5 Schematic diagram of the distribution of spinnerets on a spinneret plate B in a process for preparing a modified polyester special black shaped cotton-like filament fiber according to an embodiment of the present invention;

[0062] Figure 6 It is a cross-sectional view at another angle of the spinneret hole of the spinneret hole plate B in the preparation process of a modified polyester extra-black special-shaped cotton-like filament fiber according to an embodiment of the present invention.

[0063] In the figure:

[0064] 1. Pentaerythritol slurry; 2. Slurry feeding tank; 3. Slurry delivery pump; 4. Esterification reactor; 5. Pre-condensation reactor; 6. Delivery pump; 7. Final polymerization reactor; 8. PET modified melt; 9. Melt pump; 10. Melt filter; 11. Spinning booster pump; 12. Melt cooler; 13. Dynamic mixer; 14. Drying tower; 15. Screw extruder; 16. Injection pump; 17. Spinning box; 18. Metering pump assembly; 19. Spinning assembly; 20. Spinneret assembly; 21. Ring blowing cylinder; 22. Spinning nozzle assembly; 2 3. Heat pipe; 24. First guide wire reel A; 25. First network device; 26. Second guide wire reel A; 27; First winding head; 28. Pre-network device; 29. ​​First guide wire reel B; 30. Main network device; 31. Second guide wire reel B; 32. Winding head B; 33. Slurry regulating valve; 34. First primary filament; 35. Second primary filament; 36. Zero roller; 37. Second network device; 38. First roller; 39. Upper heat box; 40. Cooling plate; 41. False twister; 42. Second roller; 43. Lower heat box; 44. Winding roller. DETAILED DESCRIPTION

[0065] To further illustrate each embodiment, the present invention provides drawings, which are part of the disclosure of the present invention and are mainly used to illustrate the embodiments and can be used in conjunction with the relevant descriptions in the specification to explain the operating principles of the embodiments. With reference to these contents, ordinary technicians in the field should be able to understand other possible implementations and advantages of the present invention. The components in the figures are not drawn to scale, and similar component symbols are generally used to represent similar components.

[0066] According to an embodiment of the present invention, a process for preparing modified polyester extra black special-shaped cotton-like filament fibers is provided.

[0067] The present invention will now be further described with reference to the accompanying drawings and specific embodiments. Figure 1-Figure 6 As shown, Figure 2 The arrow ① in Figure 3 The arrow ① in the figure is connected. According to one embodiment of the present invention, a preparation process of modified polyester special black shaped cotton-like filament fiber is provided. The preparation process of modified polyester special black shaped cotton-like filament fiber comprises the following steps:

[0068] S1, preparing a modified semi-gloss white PET melt by copolymerization and blending polycondensation reaction, and filtering and pressurizing the modified semi-gloss white PET melt and then passing it into a dynamic mixer;

[0069] S2, combining the black masterbatch with the modified semi-gloss white PET melt to prepare a modified ultra-black polyester PET melt, and extruding it through a spinneret orifice assembly to obtain a first primary filament 34 and a second primary filament 35;

[0070] S3, using the first primary filament 34 to prepare a modified special black foreign fiber PET-POY product, and using the second primary filament 35 to prepare a modified special black foreign fiber PET-FOY product;

[0071] S4. Based on the modified extra black foreign fiber PET-POY product and the modified extra black foreign fiber PET-FOY product, the modified polyester extra black special-shaped cotton-like filament fiber is prepared.

[0072] Specifically, first, the prepared polypentatriol slurry is automatically controlled by a regulating valve to control the flow rate, flows into the slurry feeding tank through a pipeline under its own weight pressure, is evenly mixed with PTA and EG suspensions to form a blending system, and then is added to the esterification reactor through a slurry delivery pump for esterification reaction to form a polymer, and then is delivered to the pre-polycondensation reactor through a polymer pipeline for copolymerization, blending and polycondensation reaction. The prepolymer with a certain degree of polymerization coming out of the pre-polycondensation reactor is delivered to the final polymerization reactor through a delivery pump for full copolymerization reaction to form a modified semi-bright polyester melt with a specific viscosity and melting point; the modified semi-bright polyester melt passes through a melt pump, a melt filter and a spinning booster pump, a spinning melt cooler, and a spinning melt distribution pipeline in turn into an online injection dynamic mixer; a specific proportion of black masterbatch is dried in a drying tower, extruded and melted by a screw extruder, and then It is injected into the dynamic mixer through an injection pump, fully mixed with the modified semi-gloss polyester PET melt and then enters the spinning box. It is measured by two metering pumps of different specifications installed in the spinning box, and extruded into black melt streams from spinneret orifice plates with different components, different numbers of holes and different hole cross-sections. The black melt streams are cooled by an annular blower and oiled by an oil nozzle to form primary filaments with two different numbers of holes. The two filaments with different numbers of holes are respectively subjected to high-speed spinning, heat pipe heating and winding to form PET-POY and PET-FOY products with two different structures. The two PET-POY and PET-FOY products with two different structures are combined and fed into the net at the elastic zero roller, and successively pass through the first roller, the upper heating box, the cooling plate, the false twister, the second roller, the lower heating box, and finally winding to obtain the modified polyester special black special-shaped cotton-like filament fiber product.

[0073] In one embodiment, preparing a modified semi-gloss white PET melt by copolymerization and blending polycondensation reaction, and filtering and pressurizing the modified semi-gloss white PET melt and then passing it into a dynamic mixer comprises the following steps:

[0074] S11, using the slurry regulating valve 33 to adjust the flow rate of the pentaerythritol slurry 1, and passing it into the slurry feeding tank 2 under the action of gravity;

[0075] S12, the pentaerythritol slurry 1 is mixed with the PTA and EG suspension in the slurry feeding tank 2 to obtain a slurry mixture, and the slurry mixture is passed into the esterification reaction kettle 4 by a slurry delivery pump 3 to obtain an oligomer through a blending esterification reaction under a preset temperature and a preset pressure condition;

[0076] S13, the oligomer is passed through the oligomer pipeline into the pre-polycondensation reactor 5 for pre-polycondensation reaction to obtain a prepolymer;

[0077] S14, the prepolymer is delivered to the final polymerization kettle 7 through the delivery pump 6 for copolymerization, blending and polycondensation reaction to obtain a modified semi-gloss white PET melt 8.

[0078] S15, using a melt pump 9 to pass the modified semi-gloss white PET melt 8 into a melt filter 10 for filtering;

[0079] S16, using the spinning booster pump 11, the filtered modified semi-gloss white PET melt 8 is passed into the melt cooler 12 for cooling, and then sent into the dynamic mixer 13 through a pipeline.

[0080] Specifically, the preparation of the copolymerized and blended modified semi-gloss white PET melt is as follows: the pentaerythritol slurry 1 flows into the slurry feeding tank 2 by its own weight after the flow rate is automatically adjusted by the slurry regulating valve 33, and is mixed with the PTA and EG suspensions in the tank to form a slurry mixture, which is then sent to the esterification reactor 4 through the slurry delivery pump 3. Under certain temperature and pressure conditions, a blended esterification reaction occurs to form a polymer, and the polymer flows into the pre-condensation reactor 5 through the polymer pipeline for a pre-condensation reaction, and the prepolymer with a certain degree of polymerization is delivered to the final polymerization reactor 7 through the delivery pump 6 to further complete the copolymerization and blending condensation reaction, so as to form a modified semi-gloss white PET melt 8 with a certain characteristic viscosity, terminal condensation group and DEG content.

[0081] Specifically, the pipeline transportation of the modified semi-gloss natural white PET melt is as follows: the modified semi-gloss PET melt 8 is transported by the melt pump 9 and filtered through the melt filter 10 to remove impurities, and then enters the melt cooler 12 for cooling under the pressure of the spinning booster pump 11. The cooled modified semi-gloss natural white melt enters the dynamic mixer 13 through the pipeline under a certain pressure.

[0082] In one embodiment, the black masterbatch and the modified semi-gloss white PET melt are combined to prepare a modified ultra-black polyester PET melt, and the melt is extruded through a spinneret orifice assembly to obtain a first primary filament 34 and a second primary filament 35, including the following steps:

[0083] S21, using a drying tower 14 to remove moisture from the black masterbatch, and passing it into a screw extruder 15 for extrusion to obtain a black melt;

[0084] S22, using the syringe pump 16 to measure the black melt and pass it into the dynamic mixer 13, and mix it with the modified semi-gloss white PET melt to obtain a modified ultra-black polyester PET melt;

[0085] S23, passing the modified special black polyester PET melt into the spinning manifold 17, and metering it by the metering pump assembly 18;

[0086] S24, based on the metering result, the modified extra black polyester PET melt is extruded by using the spinneret plate assembly 20, and passed into the annular blower 21 for cooling, so as to obtain the first primary filaments 34 and the second primary filaments 35.

[0087] Specifically, the preparation of the modified extra black polyester PET melt is as follows: the black masterbatch with a high concentration of carbon black content is dehumidified and water is removed in the drying tower 14, then enters the screw extruder 15 to be extruded and melted into a black melt, which is then metered by the injection pump 16 and injected into the dynamic mixer 13 to be fully mixed with the modified semi-gloss white PET melt to form the modified extra black polyester PET melt.

[0088] In one embodiment, the process of preparing a modified special black foreign fiber PET-POY product using the first primary filament 34 and preparing a modified special black foreign fiber PET-FOY product using the second primary filament 35 comprises the following steps:

[0089] S31, based on the first primary filament 34, using the godet assembly and the first network device 25 to prepare a modified special black foreign fiber PET-POY product;

[0090] Specifically, the wire guide disc assembly includes a first wire guide disc A, a second wire guide disc A, a first wire guide disc B and a second wire guide disc B.

[0091] Specifically, the wire guide disk is located between the spinning box, the cooling device, the oiling device and the winding head, forming a complete path for the filaments from spinning to winding. It can control the tension of the filaments passing through it by adjusting its speed, and guide the filaments to move along a specific path to prevent the filaments from deviating from the predetermined direction. The uniform distribution of the wire guide disks ensures that the filaments are evenly laid during winding.

[0092] Specifically, the network device is located after the filaments are cooled and oiled and before they are wound. In this embodiment, it is used in conjunction with the wire guide disk and the spinning nozzle assembly. It is a key component for improving the network structure and performance of the filaments in fiber production. It creates friction and entanglement between the filaments through mechanical action, thereby improving the cohesion and stability of the filaments, and helping to form a more uniform and stable filament structure. By enhancing the entanglement between the filaments, it can reduce the phenomenon of fuzzy and broken filaments in subsequent processing.

[0093] Specifically, in this embodiment, the wire guide disc is used in conjunction with a network device, the network device is used to increase the cohesion between the wire strips, and the wire guide disc is used to control the tension and path of the wire strips.

[0094] Specifically, the modified special black heterofilament PET-POY product is prepared as follows: the modified special black PET melt from the dynamic mixer 13 enters the spinning manifold 17, and is metered by two independent metering pumps A / B18 in the spinning manifold, and is extruded from different spinneret orifice plates A / B20 installed in the spinning assembly A / B19 into two different melt streams; the two different melt streams are simultaneously cooled in the annular blower 21 into primary filaments A34 and B35, and the primary filaments A is oiled by the spinning oil nozzle A22 to reduce the friction resistance of the filaments, and then the filament tension is adjusted by the wire guide disk GR1A24 and the wire guide disk GR2A26 at a certain speed, and enters the winding head A27 to be wound into a special black PET-POY product with high oriented crystallization. A network device A25 is installed between the wire guide disks GR1A and GR2A to homogenize the filaments with oil to increase the adhesion of the filaments. The spinnerets A / B are spinneret orifice plates with round holes and special-shaped holes respectively.

[0095] S32. Based on the second primary filament 35, a modified special black foreign fiber PET-FOY product is prepared by using a guide disc assembly and a main network device.

[0096] Specifically, the preparation of the modified special black hetero-fiber PET-FOY product is as follows: the primary filaments B35 coming out of the ring blower 21 are oiled through the spinning oil nozzle B22, and then the oil agent in the filaments is homogenized through the pre-network device B28 to improve the cohesion of the filaments. The filaments B are then heated to a certain temperature through the heat pipe 23 to improve the mobility of the fiber macromolecular chain, and the tension is adjusted through the guide wire discs GR1B29 and GR2B31 at a certain speed, and finally enter the high-speed winding head B32 to be wound into a special black hetero-shaped PET-FOY product with full orientation crystallization. The main network device B30 is installed between the guide wire discs GR1B and GR2B to network and interweave the filaments to reduce the hair of the product.

[0097] In one embodiment, based on the first primary filament 34, the modified special black foreign fiber PET-POY product is prepared by using the godet assembly and the first network device 25, including the following steps:

[0098] S311, using the first spinning oil nozzle 22 to apply oil to the first primary filaments 34, and using the first network device 25 to homogenize the oil of the first primary filaments 34;

[0099] S312, adjusting the tension of the first primary filament 34 by using the first guide wire disc A24 and the second guide wire disc A26;

[0100] S313, using the first winding head 27 to wind the adjusted first spun filament 34, to obtain an ultra-black PET-POY product.

[0101] Specifically, a first network device 25 is provided between the first wire guide disc A24 and the second wire guide disc A26 for homogenizing the oil agent of the first primary filaments 34, wherein the spinneret A / B are spinneret orifice plates with round holes and irregular holes, respectively.

[0102] In one embodiment, based on the second primary filament 35, the modified black foreign fiber PET-FOY product is prepared by using a godet assembly and a main network device, including the following steps:

[0103] S321, using the second spinning oil nozzle 22 to apply oil to the second primary filaments 35, and using the pre-spinning device 28 to homogenize the oil of the second primary filaments 35;

[0104] S322, heating the second primary filament 35 by using the heat pipe 23, and adjusting the tension by using the first guide wire disc B29 and the second guide wire disc B31;

[0105] S323, using the second winding head 32 to wind the adjusted second primary filament 35, to obtain a special black special-shaped PET-FOY product.

[0106] Specifically, a main network device 30 is installed between the wire guide discs GR1B and GR2B to network and interweave the wire strips to reduce the lint of the product.

[0107] In one embodiment, based on the modified special black foreign fiber PET-POY product and the modified special black foreign fiber PET-FOY product, preparing the modified polyester special black special shaped cotton-like filament fiber comprises the following steps:

[0108] S41, passing the modified special black foreign fiber PET-POY product and the modified special black foreign fiber PET-FOY product into the zero roller 34 for stranding, and passing them into the second network device 35 for grid connection;

[0109] S42, passing the product obtained by the network connection into a roller 36, an upper heat box 37, a cooling plate 38, a false twister 39 and an intermediate roller 40 for drawing and false twisting deformation, and using a lower heat box 41 for stress elimination;

[0110] S43, using the winding laro 42 to eliminate the product after the stress is eliminated, to obtain modified polyester special black special-shaped cotton-like filament fiber.

[0111] Specifically, the preparation of modified polyester extra black special-shaped cotton-like filament fiber is as follows: the extra black POY and the extra black special-shaped FOY enter the zero roller 34 for plying respectively, and then are connected to the network in the network device 35, and then pass through the first roller 36, the upper heat box 37, the cooling plate 38, the false twister 39, and the middle roller 40 to complete the drawing and false twisting deformation, and then enter the lower heat box 41 to complete the tensile deformation stress elimination, and finally enter the winding roller 42 to be wound into modified polyester extra black special-shaped cotton-like filament fiber.

[0112] In one embodiment, the addition ratio of pentaerythritol slurry 1 is 110ppm-120ppm, the viscosity of the modified semi-gloss white PET melt is 0.615-0.620dL / g, the melting point of the modified semi-gloss white PET melt is 260±3°C, and the terminal shrinkage group of the modified semi-gloss white PET melt is 45mol / t-50mol / t;

[0113] The effective concentration of carbon black contained in the black masterbatch is 30%-35%. After the black masterbatch is extruded and melted by the screw extruder 15, it is injected into the dynamic mixer 13 through the injection pump 16 at an addition ratio of 10%-12%, and the rotation speed of the dynamic mixer 13 is set to 35rpm-45rpm.

[0114] Specifically, pentaerythritol slurry 1 is added into the slurry feeding tank, the molar ratio of the esterification reaction is 1.5-1.6, pentaerythritol is a polyol, and has high reaction efficiency when participating in the esterification reaction, and at the same time makes the polyester macromolecular chain have a higher degree of branching, pentaerythritol three monomers participate in the copolymerization and blending reaction, and the obtained modified melt has low apparent viscosity, and the addition ratio of pentaerythritol three monomers is increased to more than 110ppm, which improves the elongation of the modified polyester melt spinning product and the permeability of the dye molecules, and at the same time controls the melt viscosity to be not less than 0.615dL / g and the terminal shrinkage group to be not less than 45mol / t, which can reduce the problems of many floating fibers in the spinning process and low strength of polyester PET products caused by excessive addition of three monomers.

[0115] Specifically, in the present embodiment, the number of melt filter elements is expanded from 40 to 80, the filtration area is increased by 100%, the filtration accuracy is increased from 20U to 15U, and the switching cycle of the modified copolymer blend melt filter is extended from 30 days to 90 days, which not only improves the quality of the melt, but also reduces the number of spinning filaments, extends the switching cycle, and reduces energy consumption; in the present embodiment, the melt temperature at the outlet of the melt cooler is set to 270°C-272°C, which can reduce the degradation of the melt during transportation and reduce the white powder aggregation phenomenon during the spinning process.

[0116] Specifically, in this embodiment, the two melts are ensured to be fully and evenly mixed to achieve the compatibility of two melts with different viscosities. At the same time, the high proportion of addition increases the blackness of the melt, which can achieve the effect of bright black modified PET melt.

[0117] In one embodiment, the temperature of the spinning manifold 17 is 275° C.-280° C., and the metering pump assembly includes two metering pumps and the speeds thereof are independently controlled;

[0118] The spinning assembly 19 includes a spinning assembly A and a spinning assembly B, and the number of the spinning assembly A and the number of the spinning assembly B are both 6;

[0119] The spinneret orifice plate assembly 20 includes a spinneret orifice plate A and a spinneret orifice plate B. The number of spinneret orifice plates A and B are both 6. The number of holes of spinneret orifice plates A and spinneret orifice plate B is different. The cross-section of the spinneret holes of spinneret orifice plate A is set to a circular hole, and the cross-section of the spinneret holes of spinneret orifice plate B is set to an irregular hole. The spinneret holes of spinneret orifice plate A and spinneret orifice plate B are symmetrically distributed. The number of holes of spinneret orifice plate A is 72-144 holes, and the number of holes of spinneret orifice plate B is 48-96 holes. Spinneret orifice plate A and spinneret orifice plate B both extrude 12 bundles of filaments.

[0120] Specifically, in this embodiment, low network pressure homogenizing oil is applied to the filaments to increase the cohesion of the filaments and reduce the amount of hair generated by the friction between the single filaments and the magnetic parts due to the accumulation of high amount of carbon black powder added in the special black product. The modified special black heterofiber PET-POY product has an elongation of 110%-120% and a strength of 2.7cN / dtex-3.0cN / dtex.

[0121] In one embodiment, the oiling heights of the first spinning oil nozzle 22 and the second spinning oil nozzle 22 are independently adjustable, and the oiling height of the first spinning oil nozzle 22 is 500mm-600mm;

[0122] The speed of the first wire guide disc A24 and the second wire guide disc A26 is set to 3400m / min-3500m / min, the speed of the first winding head 27 is set to 3400m / min-3500m / min, and the network pressure of the first network device 25 is set to 0.5bar-0.7bar;

[0123] The oiling height of the second spinning nozzle 22 is 800mm-1000mm, the heating temperature of the heat pipe 23 is 150℃-170℃, the speed of the first godet B29 is set to 4000m / min-4200m / min, the speed of the second godet B31 is set to 4150m / min-4250m / min, the speed of the second winding head 32 is set to 4200m / min-4300m / min, the pressure of the pre-network 28 is set to 0.8-1.0bar, and the pressure of the main network 30 is set to 2.5bar-3.0bar;

[0124] The grid-connected pressure of the second network device 35 is set to 3bar~4bar, the modified special black foreign fiber PET-POY product and the modified special black foreign fiber PET-FOY product are network-connected between the zero roller 34 and the first roller 36 at an overfeed rate of 100%-110%, the temperature of the upper heat box 39 is set to 200℃~220℃, and the temperature of the lower heat box 43 is set to 50℃~100℃.

[0125] Specifically, in the present embodiment, after the filaments are heated by the heat pipe, the heat transport function of the macromolecular chain is increased, the spinning and stretching resistance is reduced, the orientation and crystallization are improved during the high-speed spinning and stretching process, and the produced ultra-black PET-FOY has good physical properties of high strength and long elongation; and the above embodiment adopts a pre-network plus main network double-channel network method, which reduces the friction resistance between the ultra-black PET-FOY filaments and the equipment, and avoids the problem of single filament breakage.

[0126] Specifically, this embodiment completes the stretching deformation and shaping effect in a low multiple drafting, a higher upper heat box temperature and a lower lower heat box temperature, thereby producing a modified polyester special black special-shaped cotton-like filament fiber.

[0127] In order to facilitate the understanding of the above technical solution of the present invention, the following is a comparison of the performance of a general black round hole cotton-like filament fiber product produced by a traditional production process as a reference and a modified polyester special black special-shaped cotton-like filament fiber product produced by the present method as follows:

[0128]

[0129] As shown in the table above, the modified polyester extra black special-shaped cotton-like DTY produced by the preparation process of the modified polyester extra black special-shaped cotton-like filament fiber proposed in the present invention has the characteristics of high strength and elongation, low yarn breakage rate, low fuzziness rate and high special-shaped degree. The fiber fabric is wear-resistant, light, soft and skin-friendly; it has a fluffy and warm cotton feel and a cool black visual sense, and has moisture absorption, quick drying, and environmental protection and green effects. It can be widely used in high imitation fur, high-end plush toys, jacket linings, high-end sofa leather bases, etc., and has the characteristics of high efficiency, high technology and high added value.

[0130] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A process for preparing modified polyester special black shaped cotton-like filament fibers, characterized in that: The preparation process of the modified polyester special black special-shaped cotton-like filament fiber comprises the following steps: S1, preparing a modified semi-gloss white PET melt by copolymerization and blending polycondensation reaction, and filtering and pressurizing the modified semi-gloss white PET melt and then passing it into a dynamic mixer; S2, combining the black masterbatch with the modified semi-gloss white PET melt to prepare a modified ultra-black polyester PET melt, and extruding it through a spinneret orifice assembly to obtain a first primary filament (34) and a second primary filament (35); S3, using the first primary filament (34) to prepare a modified special black foreign fiber PET-POY product, and using the second primary filament (35) to prepare a modified special black foreign fiber PET-FOY product; S4. Based on the modified extra black foreign fiber PET-POY product and the modified extra black foreign fiber PET-FOY product, the modified polyester extra black special-shaped cotton-like filament fiber is prepared.

2. The process for preparing modified polyester special black shaped cotton-like filament fiber according to claim 1, characterized in that: The method of preparing the modified semi-gloss white PET melt by copolymerization, blending and polycondensation reaction, and filtering and pressurizing the modified semi-gloss white PET melt and then passing it into a dynamic mixer comprises the following steps: S11, using the slurry regulating valve (33) to adjust the flow rate of the pentaerythritol slurry (1), and passing the slurry into the slurry feeding tank (2) under the action of gravity; S12, the pentaerythritol slurry (1) is mixed with the PTA and EG suspension in the slurry feeding tank (2) to obtain a slurry mixture, and the slurry mixture is introduced into the esterification reaction kettle (4) by a slurry delivery pump (3), and a polymer is obtained by a blending esterification reaction under a preset temperature and a preset pressure condition; S13, the oligomer is introduced into a pre-polycondensation reaction kettle (5) through an oligomer pipeline to carry out a pre-polycondensation reaction to obtain a prepolymer; S14, the prepolymer is delivered to the final polymerization kettle (7) through the delivery pump (6) for copolymerization, blending and polycondensation reaction to obtain a modified semi-gloss white PET melt (8). S15, using a melt pump (9) to pass the modified semi-gloss white PET melt (8) into a melt filter (10) for filtering; S16, using a spinning booster pump (11), the filtered modified semi-gloss white PET melt (8) is passed into a melt cooler (12) for cooling, and then sent to a dynamic mixer (13) through a pipeline.

3. The process for preparing modified polyester special black shaped cotton-like filament fiber according to claim 2, characterized in that: The method of combining the black masterbatch with the modified semi-gloss white PET melt to prepare the modified extra-black polyester PET melt, and extruding it through a spinneret orifice assembly to obtain the first primary filament (34) and the second primary filament (35) comprises the following steps: S21, using a drying tower (14) to remove moisture from the black masterbatch, and passing the masterbatch into a screw extruder (15) for extrusion to obtain a black melt; S22, using a syringe pump (16) to measure the black melt and pass it into a dynamic mixer (13), and mix it with the modified semi-gloss white PET melt to obtain a modified ultra-black polyester PET melt; S23, passing the modified extra black polyester PET melt into the spinning manifold (17), and metering it using a metering pump assembly (18); S24. Based on the metering results, the modified extra black polyester PET melt is extruded using a spinneret orifice assembly (20), and passed through a ring blower (21) for cooling to obtain a first primary filament (34) and a second primary filament (35).

4. The process for preparing modified polyester special black shaped cotton-like filament fiber according to claim 3, characterized in that: The method of preparing a modified special black foreign fiber PET-POY product by using the first primary filament (34) and preparing a modified special black foreign fiber PET-FOY product by using the second primary filament (35) comprises the following steps: S31, based on the first primary filament (34), using the guide disc assembly and the first network device (25) to prepare a modified special black foreign fiber PET-POY product; S32. Based on the second primary filament (35), a modified special black foreign fiber PET-FOY product is prepared by using a guide wire disc assembly and a main network device.

5. The process for preparing modified polyester special black shaped cotton-like filament fiber according to claim 4, characterized in that: The method of preparing a modified special black foreign fiber PET-POY product based on the first primary filament (34) by using a godet assembly and a first network device (25) comprises the following steps: S311, applying oil to the first primary filaments (34) using the first spinning oil nozzle (22), and homogenizing the oil of the first primary filaments (34) using the first spinning oil nozzle (22); S312, using the first guide wire disc A (24) and the second guide wire disc A (26) to adjust the tension of the first primary filament (34); S313, using the first winding head (27) to wind the adjusted first spun filament (34) to obtain an ultra-black PET-POY product.

6. The process for preparing modified polyester special black shaped cotton-like filament fiber according to claim 5, characterized in that: The method of preparing the modified special black foreign fiber PET-FOY product based on the second primary filament (35) by using a godet assembly and a main network device comprises the following steps: S321, applying oil to the second primary filaments (35) using a second spinning oil nozzle (22), and homogenizing the oil of the second primary filaments (35) using a pre-spinning device (28); S322, using the heat pipe (23) to heat the second primary filament (35), and using the first guide wire disc B (29) and the second guide wire disc B (31) to adjust the tension; S323, using the second winding head (32) to wind the adjusted second primary filament (35) to obtain a special black special-shaped PET-FOY product.

7. The process for preparing modified polyester special black shaped cotton-like filament fiber according to claim 6, characterized in that: The method for preparing modified polyester special black special-shaped cotton-like filament fibers based on modified special black foreign fiber PET-POY products and modified special black foreign fiber PET-FOY products comprises the following steps: S41, passing the modified special black foreign fiber PET-POY product and the modified special black foreign fiber PET-FOY product into a zero roller (34) for stranding, and passing them into a second network device (35) for grid connection; S42, passing the product obtained by the network connection into a roller (36), an upper heat box (37), a cooling plate (38), a false twister (39) and an intermediate roller (40) for drawing and false twisting, and using a lower heat box (41) for stress relief; S43, using the winding laro (42) to wind the product after stress elimination, to obtain modified polyester special black special-shaped cotton-like filament fibers.

8. The process for preparing modified polyester special black shaped cotton-like filament fiber according to claim 7, characterized in that: The pentaerythritol slurry (1) is added in an amount of 110 ppm to 120 ppm, the modified semi-gloss white PET melt viscosity is 0.615 to 0.620 dL / g, the modified semi-gloss white PET melt melting point is 260±3° C., and the terminal condensation group of the modified semi-gloss white PET melt is 45 mol / t to 50 mol / t; The black masterbatch contains carbon black in an effective concentration of 30%-35%. After the black masterbatch is extruded and melted by a screw extruder (15), it is injected into a dynamic mixer (13) through an injection pump (16) at an addition ratio of 10%-12%, and the rotation speed of the dynamic mixer (13) is set to 35rpm-45rpm.

9. The process for preparing modified polyester special black shaped cotton-like filament fiber according to claim 8, characterized in that: The temperature of the spinning manifold (17) is 275°C-280°C, and the metering pump assembly (18) includes two metering pumps whose rotation speeds are independently controlled; The spinning assembly (19) comprises a spinning assembly A and a spinning assembly B, and the number of the spinning assembly A and the number of the spinning assembly B are both 6; The spinneret orifice plate assembly (20) comprises a spinneret orifice plate A and a spinneret orifice plate B. The number of the spinneret orifice plates A and B are both 6. The number of holes of the spinneret orifice plates A and B is different. The cross section of the spinneret holes of the spinneret orifice plate A is set as a circular hole, and the cross section of the spinneret holes of the spinneret orifice plate B is set as a special-shaped hole. The spinneret holes of the spinneret orifice plate A and the spinneret orifice plate B are symmetrically distributed. The number of holes of the spinneret orifice plate A is 72-144 holes, and the number of holes of the spinneret orifice plate B is 48-96 holes. The spinneret orifice plate A and the spinneret orifice plate B both extrude 12 bundles of filaments.

10. The process for preparing modified polyester special black shaped cotton-like filament fiber according to claim 9, characterized in that: The oiling heights of the first spinning oil nozzle (22) and the second spinning oil nozzle (22) are both independently adjustable, and the oiling height of the first spinning oil nozzle (22) is 500 mm-600 mm; The speeds of the first guide wire disc A (24) and the second guide wire disc A (26) are set to 3400m / min-3500m / min, the speed of the first winding head (27) is set to 3400m / min-3500m / min, and the network pressure of the first network device (25) is set to 0.5bar-0.7bar; The oiling height of the second spinning nozzle (22) is 800 mm-1000 mm, the heating temperature of the heat pipe (23) is 150° C.-170° C., the speed of the first godet B (29) is set to 4000 m / min-4200 m / min, the speed of the second godet B (31) is set to 4150 m / min-4250 m / min, the speed of the second winding head (32) is set to 4200 m / min-4300 m / min, the pressure of the pre-network device (28) is set to 0.8-1.0 bar, and the pressure of the main network device (30) is set to 2.5 bar-3.0 bar; The grid-connected pressure of the second network device (35) is set to 3 bar to 4 bar, the modified special black foreign fiber PET-POY product and the modified special black foreign fiber PET-FOY product are grid-connected between the zero roller (34) and the first roller (36) at an overfeed rate of 100% to 110%, the temperature of the upper heat box (39) is set to 200°C to 220°C, and the temperature of the lower heat box (43) is set to 50°C to 100°C.