Cool polyester fiber and preparation method thereof

By using mannitol and lactitol and para-aminobenzoate esterification products as additives in polyester fibers, the problems of high pressure and insignificant cooling of traditional fiber equipment are solved, and better moisture absorption and cooling and ultraviolet absorption performance are achieved, which is significantly Improves the cool effect of the fiber.

CN118880486AActive Publication Date: 2024-11-01JIANGSU HENGKE ADVANCED MATERIALS CO LTD

Patent Information

Application Number
CN202411105976.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-01
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

During the spinning process, traditional cold polyester fibers have high equipment pressure, no obvious cool feeling, and poor dispersion of nano-level natural materials, which promotes photoaging by metal oxides.

Method used

The esterification products of mannitol and/or lactitol and para-aminobenzoic acid and its carboxylic acid derivatives are used as the cool-sensing additives, and melt blending, spinning, winding, drafting, and curling through a spiral extruder. Cooling polyester fiber, adjust the molar ratio of hydroxyl and carboxyl groups to 1:0.2-0.5, and improve the moisture absorption and ultraviolet absorption properties of the fiber.

Benefits of technology

It significantly improves the skin comfort and cooling performance of polyester fibers, improves nanoparticle agglomeration phenomenon, enhances the compatibility and dispersion of fibers, reduces equipment losses, and significantly improves the cooling performance of fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004990820520000071
    Figure BDA0004990820520000071
Patent Text Reader

Abstract

The invention discloses a cool-feeling polyester fiber which is characterized by comprising the following raw materials in parts by weight: 10-30 parts of a cool-feeling adjusting additive and 100-220 parts of polyester chips, wherein the cool sense adjusting additive is composed of mannitol and / or lactitol, and an esterification product of at least one of para aminobenzoic acid and carboxylic acid derivatives thereof, and salicylic acid and carboxylic acid derivatives thereof. By adjusting the ratio of mannitol and / or lactitol to at least one of p-aminobenzoic acid and carboxylic acid derivatives thereof, and salicylic acid and carboxylic acid derivatives thereof, the cool feeling adjusting additive capable of absorbing moisture, cooling and absorbing ultraviolet rays is obtained. The outward transfer rate of the polyester fibers to heat emitted by the human body can be effectively improved, and the skin-attaching cooling feeling of the fibers is obvious; meanwhile, the phenomenon of nanoparticle aggregation is avoided, and due to the similar dissolvability principle, the compatibility and dispersity in polyester fibers are excellent, and no bad loss is caused to spinning equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the textile industry, and in particular to a cool polyester fiber and a preparation method thereof. Background Art

[0002] Nowadays, with the continuous progress of science and technology and the continuous improvement of living standards, people have new demands on the performance of clothing. From the past emphasis on warmth and protection to the later emphasis on fashion, people have begun to pay attention to the functionality and environmental protection of fabrics. In recent years, humans have used a large amount of fossil fuels and cut down forests, causing a sharp increase in the concentration of gases such as carbon dioxide in the earth's atmosphere, resulting in a "greenhouse effect" and an increase in the global average temperature. Due to global warming, summers are hotter, and humans have increased the use of refrigeration equipment such as air conditioners, making the "greenhouse effect" more serious, creating a vicious cycle. In this context, people have put forward a demand for cool and comfortable clothing, and products with excellent cooling performance have been favored by people.

[0003] In recent years, the types of cooling fibers have become increasingly abundant, but based on the mechanism by which fibers produce a cooling sensation, cooling fibers can be divided into the following two types. One is to design a shaped fiber cross-section such as a flat, trilobal or cross-shaped fiber, and to improve the fiber's moisture absorption and air permeability through the microporous structure on the fiber surface. At the same time, the larger specific surface area of ​​the shaped fiber is used to enhance the capillary effect, promote the conduction of water on the fiber, and accelerate the evaporation of human sweat to release heat. The other is to add powders with high thermal conductivity to ordinary fibers, or to use the high thermal conductivity of the fiber matrix material itself to accelerate the rate at which heat is dissipated from the human body surface, thereby obtaining a cool feeling.

[0004] The patent with publication number CN102031581B discloses a method for manufacturing a super cool health-care polyester fiber, in which flaky mica and aluminum oxide and zinc oxide with high phase change enthalpy and fast heat conduction speed are micronized, ground into 100-300 nanometer powders, and then blended with fiber-forming polymers to obtain a cool health-care polyester fiber. However, since mica, jade, etc. are all natural materials, it is difficult to crush them into nanometers, and they are prone to agglomeration, and their dispersibility in polyester melt is poor, and the pressure on the spinning equipment is also large, which is not conducive to the processing of polyester fibers. In addition, the presence of metal oxides such as aluminum oxide and zinc oxide will promote the light aging of polyester fibers. Summary of the invention

[0005] In order to solve the problems that traditional cooling polyester fibers put great pressure on equipment during the spinning process and have a lack of obvious cooling feeling, the present invention provides a cooling polyester fiber and a preparation method thereof. The cooling polyester fiber uses an esterification product of p-aminobenzoic acid and mannitol and / or lactitol as an additive, and there is no dispersion compatibility problem. At the same time, it can also better improve the skin comfort and cooling property of the polyester fiber.

[0006] A cooling polyester fiber comprises the following raw materials, measured by weight: 10-30 parts of a cooling temperature regulating additive and 100-220 parts of polyester chips; wherein the cooling temperature regulating additive is composed of an esterification product of mannitol and / or lactitol and at least one of p-aminobenzoic acid and its carboxylic acid derivatives, salicylic acid and its carboxylic acid derivatives.

[0007] In some embodiments of the present invention, the preparation method of the cooling temperature regulating additive comprises the following steps: dissolving mannitol and / or lactitol and at least one of p-aminobenzoic acid and its carboxylic acid derivatives, salicylic acid and its carboxylic acid derivatives in an organic solvent, adding a Lewis acid catalyst thereto, heating to 80-100°C for esterification reaction, and after the reaction is complete, cooling to room temperature, filtering, extracting with saturated sodium carbonate, and separating the liquids to obtain the cooling temperature regulating additive.

[0008] Furthermore, the p-aminobenzoic acid and its carboxylic acid derivatives are at least one of p-aminobenzoic acid, 5-carboxy-isoindoline (CAS: 15861-30-0), 4-piperazinyl-1-benzoic acid (CAS: 85474-75-5), 4-dimethylaminobenzoic acid, 4-(N,N-diethylamino)benzoic acid, 4-amino-2-methylbenzoic acid (CAS: 2486-75-1), 4-amino-3-methoxybenzoic acid (CAS: 2486-69-3), 4-amino-3-nitrobenzoic acid (CAS: 1588-83-6), p-acetamidobenzoic acid (CAS: 556-08-1), and 4-hydrazinobenzoic acid (CAS: 619-67-0).

[0009] Furthermore, the salicylic acid and its carboxylic acid derivatives are at least one of salicylic acid, sodium p-aminosalicylate dihydrate, 3-methylsalicylic acid, 3-methoxysalicylic acid, 4-methylsalicylic acid, 4-methoxysalicylic acid, 5-methylsalicylic acid, 5-methoxysalicylic acid, 6-methoxysalicylic acid, 2-hydroxy-3-naphthoic acid, 1,4-dihydroxy-2-naphthoic acid, 3,5-di-tert-butylsalicylic acid, 3,5-diisopropylsalicylic acid, 3-aminosalicylic acid, 5-aminosalicylic acid, gentisic acid, 3-nitrosalicylic acid, 4-nitrosalicylic acid, and 3,5-dinitrosalicylic acid.

[0010] Furthermore, the mannitol and / or lactitol and at least one of p-aminobenzoic acid and its carboxylic acid derivatives and / or salicylic acid and its carboxylic acid derivatives are added at a molar ratio of hydroxyl to carboxyl of 1:0.2-0.5.

[0011] The reason why the molar ratio of hydroxyl to carboxyl in the system is limited to 1:0.2-0.5 is that the hygroscopic and exothermic properties of mannitol and / or lactitol are closely related to the hydroxyl structure they contain. If all the hydroxyl groups carried by them react with carboxylic acids to convert into ester groups, the cooling performance of the resulting esterified product will be greatly reduced. Although the salicylic acid structure and p-aminobenzoic acid ester structure have ultraviolet absorption, they still cannot achieve good tactile cooling. Therefore, after analyzing the test results, it is concluded that the molar ratio of hydroxyl to carboxyl in the system is preferably 1:0.2-0.5, and the resulting product is applied to polyester fibers to obtain better cooling performance.

[0012] Furthermore, the organic solvent is at least one of chloroform, dimethyl sulfoxide and toluene.

[0013] Furthermore, the Lewis acid is at least one of aluminum chloride, ferric chloride, boron trifluoride, and niobium pentachloride.

[0014] Furthermore, the added mass of the Lewis acid accounts for 2-5% of the total mass of the mannitol and / or lactitol and at least one of p-aminobenzoic acid and its carboxylic acid derivatives, salicylic acid and its carboxylic acid derivatives.

[0015] The preparation method of the above-mentioned cool polyester fiber comprises the following steps: melt-blending the cool temperature regulating additive and the polyester chips in a screw extruder, and then spinning, winding, drawing and curling to obtain the cool polyester fiber.

[0016] Furthermore, the spinning temperature is 270-290° C., the spinning speed is 1000-1200 m / min; and the drafting multiple is 3.8-4.2 times.

[0017] Furthermore, the cross-section of the cool polyester fiber of the present invention can be any cross-section of known melt spinning, such as circular, triangular, trilobal, hollow, flat, L-shaped, T-shaped, W-shaped, polygonal, dog-bone, etc., and its single fiber fineness is 0.8 denier to 10 denier.

[0018] Beneficial effects: Compared with the prior art, the cool polyester fiber provided by the present invention has the following advantages: by adjusting the ratio of mannitol and / or lactitol to at least one of p-aminobenzoic acid and its carboxylic acid derivatives, salicylic acid and its carboxylic acid derivatives, a cool regulating additive that can absorb moisture and reduce temperature and absorb ultraviolet rays is obtained, and when added to the polyester fiber, the rate of outward transfer of heat dissipated by the polyester fiber to the human body can be effectively increased, and the fiber has a significant cool feeling against the skin; at the same time, the phenomenon of nanoparticle agglomeration is also improved, and due to the principle of like dissolves like, the compatibility and dispersibility in the polyester fiber are excellent, and there is no adverse loss to the spinning equipment. DETAILED DESCRIPTION

[0019] The present invention is described in further detail below in conjunction with examples. It should be noted that the following embodiments and comparative examples are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various improvements within the concept of the present invention may be carried out without departing from the gist or scope of the present invention.

[0020] The preparation of the cooling agent used in the embodiment is exemplarily described below:

[0021] Cooling agent #1

[0022] 18.2 g (0.1 mol) of mannitol and 16.44 g (0.12 mol) of p-aminobenzoic acid were dissolved in 100 ml of chloroform, and 0.69 g of aluminum chloride was added thereto. The mixture was heated to 100° C. for esterification. After the reaction was complete, the mixture was cooled to room temperature, filtered, extracted with saturated sodium carbonate, and separated to obtain the cooling agent #1.

[0023] Cooling agent #2

[0024] 18.2 g (0.1 mol) of mannitol and 37.08 g (0.18 mol) of 4-piperazinyl-1-benzoic acid were dissolved in 100 ml of chloroform, and 1.66 g of aluminum chloride was added thereto. The mixture was heated to 90° C. for esterification reaction. After the reaction was complete, the mixture was cooled to room temperature, filtered, extracted with saturated sodium carbonate, and separated to obtain the cooling agent #2.

[0025] Cooling agent #3

[0026] 18.2 g (0.1 mol) of mannitol and 57.9 g (0.30 mol) of 4-(N,N-diethylamino)benzoic acid were dissolved in 100 ml of chloroform, and 3.81 g of aluminum chloride was added thereto. The mixture was heated to 100° C. for esterification reaction. After the reaction was complete, the mixture was cooled to room temperature, filtered, extracted with saturated sodium carbonate, and separated to obtain the cooling agent #3.

[0027] Cooling agent #4

[0028] The process is the same as Cooling Additive #1, except that the p-aminobenzoic acid is replaced with an equal molar amount of salicylic acid.

[0029] Cooling agent #5

[0030] The process is the same as Cooling Additive #3, except that 4-(N,N-diethylamino)benzoic acid is replaced with an equal molar amount of 3,5-diisopropylsalicylic acid.

[0031] Cooling agent #6

[0032] 34.4 g (0.1 mol) of lactitol and 27.18 g (0.18 mol) of 4-amino-2-methylbenzoic acid were dissolved in 100 ml of dimethyl sulfoxide, and 1.85 g of ferric chloride was added thereto. The mixture was heated to 80° C. for esterification reaction. After the reaction was complete, the mixture was cooled to room temperature, filtered, extracted with saturated sodium carbonate, and separated to obtain the cooling sensation regulating additive #6.

[0033] Cooling agent #7

[0034] 34.4 g (0.1 mol) of lactitol and 64.44 g (0.36 mol) of acetylaminobenzoic acid were dissolved in 150 ml of dimethyl sulfoxide, and 4.94 g of ferric chloride was added thereto. The mixture was heated to 90° C. for esterification reaction. After the reaction was complete, the mixture was cooled to room temperature, filtered, extracted with saturated sodium carbonate, and separated to obtain the cooling additive #7.

[0035] Cooling agent #8

[0036] 34.4 g (0.1 mol) of lactitol and 45.36 g (0.27 mol) of 5-methoxysalicylic acid were dissolved in 200 ml of dimethyl sulfoxide, and 3.19 g of ferric chloride was added thereto. The mixture was heated to 100° C. for esterification reaction. After the reaction was complete, the mixture was cooled to room temperature, filtered, extracted with saturated sodium carbonate, and separated to obtain the cooling sensation regulating additive #8.

[0037] Cooling agent #9

[0038] 34.4 g (0.1 mol) of lactitol and 91.8 g (0.45 mol) of 1,4-dihydroxy-2-naphthoic acid were dissolved in 200 ml of toluene, and 6.3 g of boron trifluoride was added thereto. The mixture was heated to 100° C. for esterification. After the reaction was complete, the mixture was cooled to room temperature, filtered, extracted with saturated sodium carbonate, and separated to obtain the cooling additive #9.

[0039] Cooling agent #10

[0040] The process is the same as cooling feel modulating additive #9, except that the molar amount of 1,4-dihydroxy-2-naphthoic acid used is 0.54 mol.

[0041] Example 1

[0042] 30 parts of cooling agent #1 and 100 parts of polyester chips were melt-blended in a screw extruder, and then spun at 270°C (speed 1000 m / min), wound, drawn (3.8 times), and curled to obtain cooling polyester fibers.

[0043] Example 2

[0044] 25 parts of cooling agent #2 and 130 parts of polyester chips were melt blended in a screw extruder, and then spun at 270°C (speed 1000 m / min), wound, drawn (3.8 times), and curled to obtain cooling polyester fibers.

[0045] Example 3

[0046] 20 parts of cooling agent #3 and 150 parts of polyester chips were melt blended in a screw extruder, and then spun at 275°C (speed 1100 m / min), wound, drawn (4.0 times), and curled to obtain cooling polyester fibers.

[0047] Example 4

[0048] 15 parts of cooling agent #4 and 180 parts of polyester chips were melt blended in a screw extruder, and then spun at 275°C (speed 1100 m / min), wound, drawn (4.0 times), and curled to obtain cooling polyester fibers.

[0049] Example 5

[0050] 10 parts of cooling agent #5 and 220 parts of polyester chips were melt blended in a screw extruder, and then spun at 280°C (speed 1200 m / min), wound, drawn (4.2 times), and curled to obtain cooling polyester fibers.

[0051] Example 6

[0052] Same as Example 5, except that the cooling sensation regulating additive #5 replaces the cooling sensation regulating additive #6.

[0053] Example 7

[0054] Same as Example 5, except that the cooling sensation regulating additive #5 is replaced by the cooling sensation regulating additive #7.

[0055] Example 8

[0056] Same as Example 5, except that the cooling sensation regulating additive #5 is replaced by the cooling sensation regulating additive #8.

[0057] Example 9

[0058] Same as Example 5, except that the cooling sensation regulating additive #5 is replaced by the cooling sensation regulating additive #9.

[0059] Example 10

[0060] Same as Example 5, except that the cooling sensation regulating additive #5 is replaced by the cooling sensation regulating additive #10.

[0061] Comparative Example 1

[0062] Same as Example 5, except that the cooling sensation regulating additive #5 is replaced with an equal amount of mannitol.

[0063] Comparative Example 2

[0064] Same as Example 5, except that the cooling sensation regulating additive #5 is replaced with an equal amount of 3,5-diisopropyl salicylic acid.

[0065] Comparative Example 3

[0066] Same as Example 6, except that the cooling sensation adjusting additive #6 is replaced with an equal amount of lactitol.

[0067] Comparative Example 4

[0068] Same as Example 6, except that the cooling agent #6 is replaced with an equal amount of 4-amino-2-methylbenzoic acid.

[0069] Comparative Example 5

[0070] Same as Example 6, except that no cooling sensation adjusting additive #6 is added.

[0071] Performance Testing

[0072] Hygroscopicity: According to the standard GB / T9995-1997 "Oven drying method for moisture content and regain of textile materials", the moisture regain of the fiber is measured, the fabric sample is exposed to the environment with a temperature fluctuation range of ±2℃, and the constant temperature oven temperature is set to (105±2)℃, and the drying time is 60min;

[0073] Moisture permeability: refer to the standard GB / T 12704.1-2009 "Test method for moisture permeability of textile fabrics Part 1: Moisture absorption method", control the circulating air flow speed to 0.3-0.5m / s, and the relative humidity control accuracy is ±2%;

[0074] Contact coolness performance: Tested using KES-QM coolness performance tester, with reference to standard GB / T35263-2017. For each piece of fabric, prepare three 10cm×10cm samples with the same surface density and place them in standard atmosphere for more than 24 hours for equilibrium. The test results are averaged. The test index is the coolness coefficient Q max , that is, the peak value of heat release in 0.2 seconds, Q max The larger the value, the cooler the human body feels when in contact with the fabric, and vice versa.

[0075] The test results are detailed in Table 1:

[0076] Table 1 Performance test results of the fibers obtained in Examples 1-10 and Comparative Examples 1-5

[0077]

[0078] It can be seen from the data in Table 1 that the cool feeling polyester fiber provided by the present invention has excellent hygroscopicity and moisture permeability, thereby achieving a relatively ideal contact cool feeling. The results of Example 10 can be compared with the results of Examples 1-9. It can be found that when the hydroxyl groups of the lactitol used are reacted more, the prepared cool feeling regulating additive is added to the polyester fiber, and the moisture permeability and cool feeling coefficient are both reduced. It can be seen that the amount of hydroxyl groups contained in the cool feeling regulating additive has a greater impact on the contact cool feeling of the cool feeling polyester fiber. The results of Comparative Examples 1-4 show that the contact cool feeling of the obtained polyester fiber is not as good as the contact cool feeling of the polyester fiber obtained in Examples 1-10 when mannitol or lactitol or salicylic acid derivatives or para-aminobenzoic acid derivatives are used alone. It can be inferred that the product of mannitol and / or lactitol and at least one compound of para-aminobenzoic acid and its carboxylic acid derivatives, salicylic acid and its carboxylic acid derivatives has a much greater improvement in the cool feeling of the polyester fiber than the improvement of the single component.

[0079] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A cool polyester fiber, It is characterized in that The invention comprises the following raw materials in parts by weight: 10-30 parts of a cooling sensation regulating additive and 100-220 parts of polyester chips; wherein the cooling sensation regulating additive is composed of an esterification product of mannitol and / or lactitol and at least one of p-aminobenzoic acid and its carboxylic acid derivatives, salicylic acid and its carboxylic acid derivatives.

2. The cool polyester fiber according to claim 1, It is characterized in that The preparation method of the cooling temperature regulating additive comprises the following steps: dissolving mannitol and / or lactitol and at least one of p-aminobenzoic acid and its carboxylic acid derivatives, salicylic acid and its carboxylic acid derivatives in an organic solvent, adding a Lewis acid catalyst thereto, heating to 80-100° C. for esterification reaction, and cooling to room temperature after the reaction is complete, filtering, extracting with saturated sodium carbonate, and separating the liquids to obtain the cooling temperature regulating additive.

3. The cool polyester fiber according to claim 2, It is characterized in that The p-aminobenzoic acid and its carboxylic acid derivatives are at least one of p-aminobenzoic acid, 5-carboxy-isoindoline, 4-piperazine-1-benzoic acid, 4-dimethylaminobenzoic acid, 4-(N,N-diethylamino)benzoic acid, 4-amino-2-methylbenzoic acid, 4-amino-3-methoxybenzoic acid, 4-amino-3-nitrobenzoic acid, p-acetylaminobenzoic acid, and 4-hydrazinobenzoic acid.

4. The cool polyester fiber according to claim 2, It is characterized in that The salicylic acid and its carboxylic acid derivatives are at least one of salicylic acid, sodium p-aminosalicylate dihydrate, 3-methylsalicylic acid, 3-methoxysalicylic acid, 4-methylsalicylic acid, 4-methoxysalicylic acid, 5-methylsalicylic acid, 5-methoxysalicylic acid, 6-methoxysalicylic acid, 2-hydroxy-3-naphthoic acid, 1,4-dihydroxy-2-naphthoic acid, 3,5-di-tert-butylsalicylic acid, 3,5-diisopropylsalicylic acid, 3-aminosalicylic acid, 5-aminosalicylic acid, gentisic acid, 3-nitrosalicylic acid, 4-nitrosalicylic acid, and 3,5-dinitrosalicylic acid.

5. The cool polyester fiber according to claim 2, It is characterized in that The mannitol and / or lactitol and at least one of p-aminobenzoic acid and its carboxylic acid derivatives and / or salicylic acid and its carboxylic acid derivatives are added according to a molar ratio of hydroxyl to carboxyl of 1:0.2-0.

5.

6. The cool polyester fiber according to claim 2, It is characterized in that The organic solvent is at least one of chloroform, dimethyl sulfoxide and toluene.

7. The cool polyester fiber according to claim 2, It is characterized in that The Lewis acid is at least one of aluminum chloride, ferric chloride, boron trifluoride and niobium pentachloride.

8. The cool polyester fiber according to claim 7, It is characterized in that The added mass of the Lewis acid accounts for 2-5% of the total mass of the mannitol and / or lactitol and at least one of p-aminobenzoic acid and its carboxylic acid derivatives, salicylic acid and its carboxylic acid derivatives.

9. The method for preparing the cool polyester fiber according to any one of claims 1 to 8, It is characterized in that The method comprises the following steps: melt-blending a cooling feeling regulating additive and polyester chips in a screw extruder, and then spinning, winding, drawing and curling to obtain cooling feeling polyester fibers.

10. The method for preparing the cool polyester fiber according to claim 9, It is characterized in that The spinning temperature is 270-290° C., the spinning speed is 1000-1200 m / min; and the drafting multiple is 3.8-4.2 times.

Citation Information

Patent Citations

  • Methylmenthol derivative and cool-sensation imparter composition containing same

    CN110168038A

  • Cool-sensation imparter composition containing 2,2,6-trimethylcyclohexanecarboxylic acid derivative

    US20200297607A1

Cited By

  • Cool polyester fiber and preparation method thereof

    CN122543185A

  • Cool polyester fiber and method for producing the same

    CN122543185B