Cotton linter pulp chlorine-free bleaching agent and bleaching method
By using chlorine-free bleaching agents of persulfate, pyrophosphate and anionic surfactant, combined with suitable pH and temperature control, the problem of poor organic chloride production and bleaching effect in cotton short velvet pulp bleaching is solved. The efficient and environmentally friendly cotton velvet pulp bleaching effect is achieved, and refined cotton with high whiteness and high polymerization is obtained.
Patent Information
- Application Number
- CN202411153037.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-21
AI Technical Summary
In the prior art, cotton short velvet pulp bleaching is prone to produce organic chlorides or poor bleaching effect.
The chlorine-free bleaching agent composed of persulfate, pyrophosphate, polyphosphate and anionic surfactant is used to bleach the cotton short velvet pulp, and the activation ability of persulfate is enhanced by forming superoxide radicals and singlet oxygen. , improve bleaching efficiency and control reaction conditions by adjusting pH and temperature.
The production of refined cotton with high whiteness and high polymerization is achieved, which reduces the pollution load, and the COD content in the waste liquid after bleaching is low, which is green and environmentally friendly, and avoids the production of organic chlorides.
Smart Images

Figure CN118880646A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of bleaching, and in particular to a chlorine-free bleaching agent for cotton linter pulp and a bleaching method. Background Art
[0002] Cotton linter pulp is generally made by caustic soda pulping, and the refined cotton product obtained by bleaching the pulp can be used in the production of cellulose esters, nitrocellulose and cellulose acetate and other products, and is widely used. In order to strengthen environmental protection and promote green development, it is an inevitable trend for the bleaching industry to develop towards elemental chlorine-free (ECF) bleaching and total chlorine-free (TCF) bleaching. At present, the production of refined cotton in China is mainly to cook cotton linter with high temperature alkali method, and then bleach it with ECF or TCF.
[0003] In ECF, chlorine dioxide and sodium hypochlorite are commonly used bleaching agents. Patent CN202110932036.3 discloses a method for preparing a stable chlorine dioxide bleaching solution, in which chlorine gas and chlorine dioxide are directly introduced into a buffered absorption liquid to react with chlorine gas to generate hypochlorite with bleaching effect. While effectively treating chlorine gas, the bleaching effect of the stable chlorine dioxide bleaching solution is improved; chlorine dioxide can selectively oxidize lignin and colored substances, and the resulting refined cotton product has a relatively high whiteness and less damage to the fiber; but organic chlorides will still be produced in the bleaching waste liquid.
[0004] In TCF, hydrogen peroxide is a widely used bleaching agent. Patent CN201510453418.2 discloses a device and method for preparing refined cotton by bleaching cotton linters with high-concentration hydrogen peroxide. The cotton linters are bleached by mixing H2O2, an activator and an alkaline solution. Although H2O2 can effectively reduce or eliminate the colored groups of lignin under alkaline conditions and can break up lignin to dissolve it, hydrogen peroxide is not stable and is easy to decompose, especially in the presence of transition metal ions, which will accelerate the decomposition. Secondly, hydrogen peroxide itself is a weak oxidant, especially when treating lignin that has been in a passivated state after cooking, its effect is not ideal. Summary of the invention
[0005] The purpose of the present invention is to overcome the above technical deficiencies, provide a chlorine-free bleaching agent and a bleaching method for cotton linter pulp, and solve the technical problems in the prior art that bleaching of cotton linter pulp easily produces organic chlorides or the bleaching effect is poor.
[0006] In order to achieve the above technical purpose, the technical solution provided by the present invention is: In a first aspect, the present invention provides a chlorine-free bleaching agent for cotton linter pulp, which comprises, by weight, 1.4 to 7.9 parts of persulfate, 2.7 to 9.2 parts of pyrophosphate, 1.4 to 7.9 parts of polyphosphate, 1.4 to 7.9 parts of anionic surfactant, and 1000 parts of water.
[0007] In a second aspect, the present invention provides a method for bleaching cotton linter pulp, comprising the following steps: soaking the cotton linter pulp in a bleaching agent, mixing uniformly to obtain a mixture; adjusting the pH of the mixture to alkaline, performing a bleaching reaction, and washing and drying after the reaction to complete the bleaching of the cotton linter pulp.
[0008] Compared with the prior art, the beneficial effects of the present invention include: The invention uses persulfate as a main bleaching agent, and cooperates with pyrophosphate, polyphosphate and anionic surfactant to form a low-pollution chlorine-free bleaching agent to bleach cotton linter pulp. The pyrophosphate and polyphosphate constitute a polyphosphate system, and the activation ability of the persulfate is effectively enhanced by forming superoxide free radicals and singlet oxygen. The anionic surfactant has good surface activity and strong hydrophilicity, can effectively reduce the tension of the oil-water interface, improve the bleaching efficiency, and play a certain decontamination effect. The bleaching agent of the invention has a good bleaching effect, can effectively remove colored substances attached to cellulose, and has a small degree of damage to the cellulose. The bleaching method of the present invention has mild conditions, does not contain chlorine elements, does not require a bleaching terminator, reduces pollution load, and the COD content in the waste liquid after bleaching is below 280 mg / L, which is green and environmentally friendly. Bleaching cotton linter pulp can obtain refined cotton with high whiteness and high polymerization degree. The obtained refined cotton has a whiteness of more than 70 and a polymerization degree of more than 1000, and the degree of polymerization is 15% to 64% relative to unbleached cotton linter pulp. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 The effect of PA concentration on the bleaching effect of cotton linter pulp in the present invention; Figure 2 It is the effect of PB concentration on the bleaching effect of cotton linter pulp in the present invention; Figure 3 The effect of SDBS concentration on the bleaching effect of cotton linter pulp in the present invention; Figure 4 The effect of bleaching temperature on the bleaching effect of cotton linter pulp in the present invention; Figure 5 The effect of bleaching time on the bleaching effect of cotton linter pulp in the present invention; Figure 6 The effect of pH on the bleaching effect of cotton linter pulp in the present invention; Figure 7 The effect of PMS concentration on the bleaching effect of cotton linter pulp in the present invention; Figure 8 This is the FTIR diffraction pattern of cellulose cotton linter pulp before and after bleaching in Example 8 of the present invention; Fig. 9 The XRD patterns of cotton linter pulp and refined cotton in Example 8 of the present invention; Fig.10 The SEM images of cotton linter pulp and refined cotton in Example 8 of the present invention, wherein (a) is cotton linter pulp, magnified 200 times; (b) is cotton linter pulp, magnified 500 times; (c) is refined cotton, magnified 200 times; (d) is refined cotton, magnified 500 times; Fig.11 It is a diagram of the quenching experiment results in the present invention; Fig.12 It is the sulfate radical (SO4· - ) and EPR spectra of hydroxyl radical (·OH); Fig.13 The present invention is different reaction system under 1 EPR spectrum of O2; Fig.14 It is the EPR spectrum diagram of O2·- in different reaction systems in the present invention. DETAILED DESCRIPTION
[0010] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0011] In view of the defects that the existing elemental chlorine-free bleaching process is prone to produce pollutants, such as organic chlorides, and the bleaching efficiency is low in the total chlorine-free (TCF) bleaching process, the present invention provides a chlorine-free bleaching agent and a bleaching method for cotton linter pulp, using potassium persulfate as the main bleaching agent, sodium pyrophosphate, sodium tripolyphosphate, and sodium dodecylbenzene sulfonate to form a low-pollution bleaching agent, bleaching cotton linter pulp, and obtaining a refined cotton with high whiteness and high polymerization degree. The present invention can reduce the formation of pollutants from the source, is environmentally friendly, and has a high bleaching effect.
[0012] Among them, sodium pyrophosphate is used for bleaching paper and plant fibers, and sodium tripolyphosphate has the functions of chelation, suspension, dispersion, peptization, emulsification, pH buffering, etc., and can be used as a main auxiliary agent for synthetic detergents; the present invention forms a polyphosphate system by sodium pyrophosphate and sodium tripolyphosphate, which can synergistically promote the activation of potassium persulfate, effectively activate potassium persulfate to produce active substances, and significantly improve the oxidative degradation efficiency of potassium persulfate on organic matter, thereby improving the bleaching effect; sodium dodecylbenzene sulfonate is a common anionic surfactant with a wide source, low cost, good surface activity, and strong hydrophilicity. It can effectively reduce the tension of the oil-water interface and improve the bleaching efficiency. In addition, sodium dodecylbenzene sulfonate has a better decontamination effect on particulate dirt on natural fibers, and can also absorb nitrogen, phosphorus and certain metal ions in water.
[0013] In a first aspect, the present invention provides a chlorine-free bleaching agent for cotton linter pulp, which comprises, by weight, 1.4 to 7.9 parts of persulfate, 2.7 to 9.2 parts of pyrophosphate, 1.4 to 7.9 parts of polyphosphate, 1.4 to 7.9 parts of anionic surfactant, and 1000 parts of water; the pH value of the chlorine-free bleaching agent for cotton linter pulp is 8.5 to 11.0.
[0014] Preferably, the composition comprises, by weight, 2.7 to 7.9 parts of persulfate, 4 to 7.9 parts of pyrophosphate, 2.7 to 6.6 parts of polyphosphate, 1.4 to 6.6 parts of anionic surfactant, and 1000 parts of water; the pH value of the chlorine-free bleaching agent for cotton linter pulp is 9.0 to 10.5.
[0015] Preferably, the composition comprises, by weight, 4 to 6.6 parts of persulfate, 5.3 to 6.6 parts of pyrophosphate, 4 to 5.3 parts of polyphosphate, 2.7 to 6.6 parts of anionic surfactant, and 1000 parts of water; the pH value of the chlorine-free bleaching agent for cotton linter pulp is 9.0 to 10.0.
[0016] Preferably, the composition comprises, by weight, 5.3 parts of persulfate, 6.6 parts of pyrophosphate, 5.3 parts of polyphosphate, 6.6 parts of anionic surfactant and 1000 parts of water; and the pH value of the chlorine-free bleaching agent for cotton linter pulp is 9.5.
[0017] Preferably, the persulfate includes potassium persulfate, the pyrophosphate includes sodium pyrophosphate, the polyphosphate includes sodium tripolyphosphate, and the anionic surfactant includes sodium dodecylbenzene sulfonate.
[0018] In a second aspect, the present invention provides a method for bleaching cotton linter pulp, comprising the following steps: soaking cotton linter pulp in bleaching agent and mixing uniformly to obtain a mixture; The pH of the mixture is adjusted to alkaline, a bleaching reaction is carried out, and after the reaction is completed, the cotton linter pulp is directly washed and dried to complete the bleaching of the cotton linter pulp and obtain refined cotton.
[0019] Preferably, the bath ratio of cotton linter pulp and bleaching agent is 1:(10-60), wherein the bath ratio refers to the mass ratio of cotton linter pulp and bleaching agent.
[0020] In the bleaching reaction of the present invention, the product is directly cleaned and dried after the reaction is completed, and no bleaching terminator is required, thus saving costs.
[0021] Preferably, the pH of the mixture is adjusted to 8.5-11. Pyrophosphates (such as PA) and polyphosphates (such as PB) can effectively enhance the activation ability of persulfate by forming superoxide radicals and singlet oxygen under weak alkaline conditions; hydroxyl radicals (·OH) under alkaline conditions will promote the activation of persulfate, which is beneficial to the production of active substances. At the same time, cellulose will undergo hydrolysis under alkaline conditions, resulting in a decrease in the degree of polymerization; therefore, controlling the appropriate pH in the reaction system is a key factor in ensuring the acquisition of refined cotton with high whiteness and high degree of polymerization.
[0022] Preferably, the bleaching reaction is carried out at 30-80° C. for 10-60 minutes. The bleaching temperature can affect the reaction rate of the bleaching system. The increase in bleaching time can allow the bleaching agent and cotton linter pulp to fully react and effectively remove colored substances, thereby affecting the whiteness and polymerization degree of refined cotton.
[0023] Preferably, during the bleaching reaction, stirring is performed every 3 to 8 minutes.
[0024] The present invention is further described in detail below through specific embodiments; to avoid redundancy, the main raw materials, instruments and related test standards / methods are described here: 1. Main raw materials: Cotton linter pulp: from Hubei Jinhanjiang Refined Cotton Co., Ltd., unbleached, whiteness 42-45, degree of polymerization 2600-2800; Potassium persulfate (PMS), sodium pyrophosphate (PA), sodium tripolyphosphate (PB), tert-butyl alcohol (TBA), histidine (L-his), and p-benzoquinone (BQ) were all purchased from Shanghai MacLean Biochemical Technology Co., Ltd.; sodium dodecylbenzenesulfonate (SDBS) was purchased from Tianjin Tianli Chemical Reagent Co., Ltd.; methanol (MeOH) and potassium dichromate were purchased from Sinopharm Group, and all of the above drugs were analytical grade.
[0025] 2. Main instruments: Fourier transform infrared spectrometer (FTIR), Fourier Transform, PE Company, USA; X-ray diffractometer (XRD), SmartLab, Rigaku Corporation, Japan; Scanning electron microscope (SEM), JSM-7500F, JEOL Ltd.; Electron paramagnetic resonance spectrometer (EPR), Bruker EMXplus, Bruker Corporation, USA.
[0026] 3. Test standard or method description (1) Determination of whiteness: According to GBT-9107-2023 "Whiteness Determination Method", a digital whiteness meter is used to measure the whiteness of refined cotton. Whiteness is one of the important physical indicators reflecting the quality of refined cotton.
[0027] (2) Determination of degree of polymerization (DP): According to GBT-9107-2023 "Determination of degree of polymerization", the time required for cellulose copper ammonia solution and blank copper ammonia solution to flow through the two scale lines of the viscometer is measured, and then the degree of polymerization of refined cotton degradation is calculated. A high degree of polymerization means that cellulose is more durable and has higher strength and toughness.
[0028] (3) Fourier transform infrared spectrometer (FTIR) test: Cotton linter pulp and refined cotton were selected and ground into thin slices. The samples were measured on an infrared spectrometer. The scanning range was 500~4000 cm -1 .
[0029] (4) X-ray diffraction (XRD) test The fiber crystal structure was detected by X-ray diffractometer, using a copper target to generate X-rays (0.154 nm) with a scanning range of 5-80°, and the crystallinity was calculated. The calculation formula for crystallinity (Xc) is: Xc=( Ι 200 - Ι am ) / Ι 200 ×100% In the above formula Ι 200 It represents the intensity of the 200-face diffraction peak, that is, the maximum diffraction intensity at 2θ=22.8°, and Ιam represents the intensity of the peak when 2θ=18°, that is, the diffraction intensity of the amorphous region.
[0030] (5) Scanning electron microscope (SEM) test A small piece of cotton linter pulp and refined cotton was selected for sample preparation. The sample was magnified and photographed using a scanning electron microscope to obtain an image of the surface morphology and structure of the cotton fiber. Before testing, the sample needs to be gold-sprayed. The scanning electron microscope test conditions are acceleration voltage: 0.1KV-20KV, beam intensity: 10 -13 ~2×10 -9 .
[0031] (6) Chemical oxygen demand (COD cr ) Determination COD cr(hereinafter referred to as COD) is chemical oxygen demand, also known as chemical oxygen consumption. It mainly uses potassium dichromate as an oxide to oxidize and decompose oxidizable substances in water (such as organic matter, nitrite, ferrous salt, sulfide, etc.), and then calculates the oxygen consumption based on the amount of oxidant consumed. The unit is expressed in mg / L.
[0032] Example 1 The bleaching agent used in this embodiment has a PMS concentration of 6.6 g / L, a PA concentration of 6.6 g / L, a PB concentration of 5.3 g / L, and a SBDS concentration of 6.6 g / L, and is obtained by mixing PMS, PA, PB, and SBDS with water (without adjusting the pH value).
[0033] A method for bleaching cotton linter pulp comprises the following steps: weighing 5 g of cotton linter pulp, placing it in 150 g of the above-mentioned bleaching agent (bath ratio is 1:30), and mixing evenly. Then placing it in a controllable constant temperature water bath, bleaching it at 50°C for 30 minutes, stirring it every 5 minutes during the bleaching process to ensure uniform reaction. After the reaction is completed, rinsing it with tap water, and then drying it in an oven at 50°C to obtain refined cotton.
[0034] Example 2 The only difference from Example 1 is that the PA concentrations are adjusted to 2.7 g / L, 4 g / L, 5.3 g / L, 7.9 g / L, and 9.2 g / L, respectively, and the other steps and conditions are the same as those in Example 1.
[0035] The whiteness and degree of polymerization of the refined cotton obtained in Example 1 and Example 2 were tested to investigate the effect of different PA concentrations on the bleaching effect of cotton linter pulp. The results are as follows: Figure 1 shown.
[0036] Depend on Figure 1 It can be seen that when other conditions are fixed, the whiteness of the refined cotton decreases first, then increases, and then decreases with the increase of PA concentration. When the PA concentration increases to 6.6 g / L, the whiteness is as high as 85.1, which shows that the present invention uses potassium persulfate as the main bleaching agent to bleach the cotton pulp after cooking, and an appropriate amount of PA can activate PMS, so that the whiteness of the treated refined cotton is improved. When the PA concentration continues to increase, the whiteness remains basically unchanged, which may be because the active sites of the polyphosphate system have reached the highest level, so the bleaching effect of increasing the amount of PA is not obvious. The trend of the polymerization degree of refined cotton is to increase first and then slightly decrease. When PA is 6.6 g / L, the polymerization degree is 1552.
[0037] Example 3 The only difference from Example 1 is that the PB concentrations were adjusted to 1.4 g / L, 2.7 g / L, 4 g / L, 6.6 g / L, and 7.9 g / L, respectively, and the other steps and conditions were the same as those in Example 1.
[0038] The whiteness and degree of polymerization of the refined cotton obtained in Example 3 were tested to investigate the effect of different PB concentrations on the bleaching effect of cotton linter pulp. The results are as follows: Figure 2 shown.
[0039] Depend on Figure 2 It can be seen that the whiteness of refined cotton increases with the increase of PB concentration. When the PB concentration increases to 5.3 g / L, the whiteness is 85. When the PB concentration exceeds 5.3 g / L, the whiteness increases slowly and the degree of polymerization decreases slightly, indicating that continuing to increase the PB concentration will cause a certain degree of damage to the cellulose of refined cotton.
[0040] Example 4 The only difference from Example 1 is that the SDBS concentrations are adjusted to 1.4 g / L, 2.7 g / L, 4 g / L, 5.3 g / L, and 7.9 g / L, respectively, and the other steps and conditions are the same as those in Example 1.
[0041] The whiteness and polymerization degree of the refined cotton obtained in Example 4 were tested to investigate the effect of different SDBS concentrations on the bleaching effect of cotton linter pulp. The results are as follows: Figure 3 shown.
[0042] Depend on Figure 3 It can be seen that the whiteness of refined cotton increases with the increase of SDBS concentration. When the SDBS concentration is 6.6g / L, the whiteness is 85. When the SDBS concentration exceeds 6.6g / L, the whiteness increases slowly. With the increase of SDBS concentration, the degree of polymerization basically shows a downward trend. It may be because sodium dodecylbenzene sulfonate improves the wettability of cotton linter pulp, which is conducive to the diffusion of bleaching agent into the fiber, resulting in an increase in whiteness and a decrease in degree of polymerization. Taking all factors into consideration, it is preferred that the SDBS concentration be below 6.6g / L.
[0043] Example 5 The only difference from Example 1 is that the bleaching temperatures are adjusted to 30° C., 40° C., 60° C., 70° C., and 80° C., respectively, and the other steps and conditions are the same as those in Example 1.
[0044] The whiteness and polymerization degree of the refined cotton obtained in Example 5 were tested to investigate the effect of different bleaching temperatures on the bleaching effect of cotton linter pulp. The results are as follows: Figure 4 shown.
[0045] like Figure 4As shown in the figure, the whiteness of refined cotton increases with the increase of bleaching temperature. The increase of bleaching temperature will accelerate the reaction rate of PMS, and the reaction is more intense, which will increase the whiteness of refined cotton, but it will also cause fiber damage and the degree of polymerization will show a downward trend. Taking all factors into consideration, the preferred bleaching temperature is 30-50 ℃.
[0046] Example 6 The only difference from Example 1 is that the bleaching time is adjusted to 10 min, 20 min, 40 min, 50 min and 60 min respectively, and the other steps and conditions are the same as those in Example 1.
[0047] The whiteness and polymerization degree of the refined cotton obtained in Example 6 were tested to investigate the effect of different bleaching times on the bleaching effect of cotton linter pulp. The results are as follows: Figure 5 shown.
[0048] Depend on Figure 5 It can be seen that with the increase of bleaching time, the whiteness of refined cotton is gradually improved. In the first 30 minutes, the whiteness increases rapidly, and the increase trend slows down after 30 minutes. In the first 10 minutes, the active substances in the bleaching agent oxidize and degrade the colored substances attached to cellulose in large quantities; as time goes on, these colored substances gradually decrease. As time goes on, while improving the whiteness, the active substances in the bleaching agent react with cellulose, causing cellulose damage and a decrease in the degree of polymerization. Taking all factors into consideration, the optimal bleaching time is 10 to 30 minutes.
[0049] Example 7 The only difference from Example 1 is that the pH values of the bleaching agent are adjusted to 8.5, 9.0, 9.5, 10.0, 10.5 and 11 respectively with sodium hydroxide solution and sulfuric acid, and the other steps and conditions are the same as those of Example 4.
[0050] The whiteness and polymerization degree of the refined cotton obtained in Example 7 were tested to investigate the effect of different pH values on the bleaching effect of cotton linter pulp. The results are as follows: Figure 6 shown.
[0051] Depend on Figure 6 It can be seen that when the pH is less than 9.5, the whiteness of refined cotton increases with the increase of pH. When the pH exceeds 9.5, both the whiteness and the degree of polymerization show a downward trend. When the pH exceeds 9.5, the activation ability of PMS weakens, and under over-alkaline conditions, PMS may be induced to transform into sulfate radicals, while sulfate radicals play a smaller role in the bleaching process. Therefore, under over-alkaline conditions, the whiteness of refined cotton will decrease, and cellulose will also undergo hydrolysis reaction, resulting in a decrease in the degree of polymerization. Taking all factors into consideration, the preferred pH is 9.0-10.0.
[0052] Example 8 The only difference from Example 1 is that the bleaching agent is different, specifically: In the bleaching agent of this embodiment, the concentration of PMS is 5.3 g / L, the concentration of PA is 6.6 g / L, the concentration of PB is 5.3 g / L, the concentration of SBDS is 6.6 g / L, and the pH is 9.5; the specific conditions of the bleaching method for cotton linter pulp are the same as those in Example 1.
[0053] After testing, the whiteness of the refined cotton obtained was 83.6 and the degree of polymerization was 2210.
[0054] Example 9 The only difference from Example 8 is that the PMS concentrations were adjusted to 1.4 g / L, 2.7 g / L, 4 g / L, 6.6 g / L, and 7.9 g / L, respectively, and the pH was 9.5. The other steps and conditions were the same as those in Example 8.
[0055] The whiteness and polymerization degree of the refined cotton obtained in Example 8 and Example 9 were tested to investigate the effect of different PMS concentrations on the bleaching effect of cotton linter pulp. The results are as follows: Figure 7 shown.
[0056] Depend on Figure 7 It can be seen that the whiteness of refined cotton increases with the increase of PMS concentration. When the PMS concentration increases to 5.3 g / L, the whiteness increases slowly. The increase in PMS dosage increases the active substances in the bleaching agent, enhances the oxidizing ability, and increases the whiteness, but also causes the degradation of cellulose and decreases the degree of polymerization. Taking all factors into consideration, the preferred PMS is 2.7-5.3 g / L.
[0057] The cotton linter pulp used and the refined cotton obtained in Example 8 are characterized and analyzed below.
[0058] 1. FTIR analysis The changes in the cellulose structure of cotton linter pulp before and after bleaching were understood by analyzing the characteristic absorption peaks of various functional groups in the infrared spectrum. Figure 8 shown.
[0059] Depend on Figure 8 It can be seen that 3400~3200cm -1 A broad and medium-strong absorption peak appears, which belongs to the OH stretching vibration peak. At this time, the hydrogen atoms are easy to attract each other with the lone electrons in the oxygen atom with greater electronegativity on other bonds to form hydrogen bonds. 2988~2890cm -1 The absorption peak is attributed to the CH stretching vibration peak, which is the characteristic absorption peak of cellulose. The wave number is 1400 cm -1 The left and right are C-H2 bending vibration and CH bending vibration. The wave number is 1100 cm -1The left and right are the cellulose COC stretching vibration and OH association absorption bands. -1 It is attributed to the stretching vibration peak of anomeric carbon (C1) and glycosidic vibration. After bleaching, the absorption intensity of OH stretching vibration does not change significantly, and the absorption intensity of COC stretching vibration of cellulose is slightly enhanced. This may be because PMS has a certain oxidizing ability and increases the oxygen-containing groups in cotton linter pulp; the absorption peak intensity of glycosidic vibration and anomeric carbon (C1) stretching vibration peak is enhanced. The reason may be that during the bleaching process, a small amount of cellulose is degraded, exposing more glycosidic bonds and anomeric carbon, which also shows that bleaching will slightly damage the cellulose structure, resulting in a decrease in the degree of polymerization of cellulose.
[0060] Through infrared spectrum analysis, it was found that there was no absorption peak of benzene ring functional group, which means that the unbleached cotton linter pulp basically does not contain lignin. The whiteness of unbleached cotton linter pulp is relatively low, which is probably due to the colored impurities remaining in the cooking process attached to the cellulose. In addition, the characteristic absorption peaks of cotton linter cellulose before and after bleaching have no significant changes in position and intensity, and no new absorption peaks appear. This also shows that the bleaching method of the present invention only removes the colored substances on the cellulose during the bleaching process, and the damage to the fiber is relatively small. This is consistent with the results of high whiteness and high polymerization degree of refined cotton measured in the present invention, indicating that the bleaching method of the present invention is an effective and feasible bleaching process.
[0061] 2. XRD analysis Cellulose crystallinity refers to the percentage of crystalline regions in cellulose to the whole cellulose. It is an important parameter to describe the crystal structure of cellulose. It is closely related to lignin, cellulose and hemicellulose. X-ray diffraction was used to analyze the changes in cellulose crystallinity in unbleached cotton linter pulp and refined cotton. The results are as follows Fig. 9 And as shown in Table 1.
[0062] Table 1 Effect of the bleaching method of the present invention on the crystallinity of cotton linter pulp
[0063] Depend on Fig. 9 It can be seen that the main component of unbleached cotton linter pulp is cellulose, and diffraction peaks appear at 2θ=14.98°, 22.8° and 34.49°. The above three characteristic peaks also appear in the refined cotton after bleaching. The cellulose crystal form is consistent before and after bleaching, with no obvious difference. This is because the PMS bleaching method only removes the colored substances attached to the surface of cotton linter pulp fibers, and does not change the crystal structure of cellulose. It can be seen from Table 1 that the crystallinity of cellulose does not change much before and after bleaching, which also shows that the bleaching method of the present invention can selectively oxidize and remove colored substances, and has little effect on the crystal structure of cellulose. This is consistent with the analysis results of infrared spectroscopy.
[0064] 3. Scanning electron microscope (SEM) analysis In order to further explore the effect of PMS bleaching method on cellulose surface morphology and damage degree, the surface morphology of unbleached cotton linter pulp and refined cotton was observed by scanning electron microscopy. Fig.10 shown.
[0065] Depend on Fig.10 It can be seen that the morphological structure of the cotton fibers in the unbleached cotton linter pulp shown in Figures (a) and (b) is complete, but the surface contains some fine fibers and a few fragments. After being treated by the bleaching method of the present invention, the surface of the fibers shown in Figures (c) and (d) becomes smooth and flat, and the fragments on the fiber surface are also removed. The fibers do not show surface disorder and cracks, and the surface etching is small, so the integrity of the fibers is not destroyed, which is consistent with the result that the degree of polymerization has not dropped sharply. This shows that the bleaching method of the present invention has a relatively small effect on the morphological structure of cellulose and is an excellent process for obtaining high-whiteness, high-polymerization refined cotton.
[0066] 4. COD analysis In the traditional refined cotton bleaching production process, chlorine-containing bleaching agents are used, and the bleaching waste liquid mainly contains organic chlorides such as chloroform and chlorophenols and toxic, teratogenic, and mutagenic organic substances such as dioxins and furans. If directly discharged, it will have a huge impact on environmental pollution, and wastewater treatment is also very difficult. However, the present invention uses PMS as the main bleaching agent, does not produce toxic byproducts such as chlorine-containing compounds, can reduce the formation of industrial pollutants from the source, and the wastewater COD produced by the system is very low, so the subsequent wastewater treatment cost is reduced. The COD of the bleaching wastewater produced after bleaching in Example 8 was tested three times, and the results are shown in Table 2. The average content of the average COD of the bleaching wastewater is 270.9 mg / L, which is much lower than the traditional chlorine-containing bleaching process, indicating that the bleaching method of the present invention is a green bleaching technology with safe and reliable characteristics, and effectively eliminates the generation of organic chlorides.
[0067] Table 2 COD content in wastewater from bleaching process of the present invention
[0068] 5. Mechanism of the bleaching method of the present invention Generally speaking, sulfate radicals (SO4· - ), hydroxyl radical (·OH), superoxide radical (O2· - ) and other free radicals and singlet oxygen ( 1O2) non-radical active substances. These active substances play an important role in removing colored substances attached to the surface of cellulose. In order to explore the active substances that play a major role in the bleaching system of the present invention, in this experiment, different quenchers were added to identify the free radicals that play a major role in the PMS bleaching system. Specifically, methanol (MeOH) [k(SO4· - ) = 2.5 × 10 7 M -1 s -1 , k(·OH) = 1.0× 10 9 M -1 s -1 ] to sulfate radical (SO4· - ) and hydroxyl radicals (·OH) have a high quenching effect. Tert-butyl alcohol (TBA) [ k(SO4· - )=(4.0-9.1)×10 5 M -1 s -1 , k(·OH)= (3.8-7.6)×10 9 M -1 s -1 ] to sulfate radical (SO4· - ) has a weak quenching effect, but has a good quenching effect on hydroxyl radicals (·OH) and is very stable. L-histidine (L-his) [ k( 1 O2) = 3.2 × 107 M -1 s -1 ] can effectively quench singlet oxygen ( 1 O2), p-benzoquinone (BQ) [k(·O 2 - )=(0.9~1.0)×10 9 M -1 S -1 ] is used to quench superoxide free radicals (O2· - ). The experimental conditions of each group are as follows: the bleaching agent of Example 8 is added into the reactor, the pH is adjusted to 9.5 and then the quenching agent is added immediately, and the reaction is carried out in a controllable water bath at 50° C. for half an hour and then the reaction is terminated.
[0069] Control group: bleaching agent of Example 8; Methanol group: bleaching agent of Example 8 + 500 mmol / L methanol; Tert-butyl alcohol group: the bleaching agent of Example 8 + 500 mmol / L tert-butyl alcohol; L-histidine group: the bleaching agent of Example 8 + 10 mmol / L L-histidine; p-Benzoquinone group: the bleaching agent of Example 8 + 3 mmol / L p-benzoquinone.
[0070] The quenching experiment results are as follows Fig.11 After adding methanol and tert-butyl alcohol to the bleaching agent in Example 8, the whiteness of the refined cotton obtained is not much different from that obtained in Example 8, indicating that the bleaching effect is not significantly inhibited. This shows that sulfate radicals (SO4· - ) and hydroxyl radicals (·OH) have little effect on removing colored substances in the bleaching method of the present invention. It is found that the whiteness of refined cotton decreases significantly when histidine and p-benzoquinone are added to the bleaching agent. This shows that singlet oxygen ( 1 O2) and superoxide radicals (O2 - ) plays a major role. In addition, after adding four quenchers to the bleaching agent of Example 8, the polymerization degree increased, approaching that of unbleached cotton linter pulp, indicating that the four active substances may cause certain damage to the cellulose structure, resulting in a slight decrease in the polymerization degree. Among them, singlet oxygen ( 1 O2) has the greatest ability to destroy cellulose structure.
[0071] In order to further determine the generation of various active species in the PMS bleaching system, EPR spectroscopy was used with DMPO or TEMP as free radical scavengers. DMPO was used to capture sulfate radicals (SO4· - ), hydroxyl radical (·OH) or superoxide anion radical (O2· - ), TEMP is used to capture singlet oxygen. Free radical scavengers were added to different reaction systems, the pH value was adjusted to 9.5, and the reaction was carried out at 50°C for 15 minutes, where: PMS group: PMS concentration was 5.3 g / L, pH value was 9.5, and free radical scavenger 50 mmol / L was added.
[0072] PMS+SDBS group: PMS concentration was 5.3 g / L, SBDS concentration was 6.6 g / L, pH value was 9.5; 50 mmol / L of free radical scavenger was added.
[0073] PMS+PA+PB group: PMS concentration was 5.3 g / L, PA concentration was 6.6 g / L, PB concentration was 5.3 g / L, pH value was 9.5; 50 mmol / L of free radical scavenger was added.
[0074] PMS+PA+PB+SDBS group: PMS concentration was 5.3 g / L, PA concentration was 6.6 g / L, PB concentration was 5.3 g / L, SBDS concentration was 6.6 g / L, pH value was 9.5; 50 mmol / L of free radical scavenger was added.
[0075] like Fig.12 As shown in the figure, sulfate radicals (SO4·- ) and hydroxyl radicals (·OH), of which the four strong peaks correspond to hydroxyl radicals (·OH), and the ones interspersed in the middle are sulfate radicals (SO4· - ) characteristic peaks. Fig.13 As shown, the 1:1:1 triplet peak is singlet oxygen ( 1 O2) characteristic peaks. Fig.14 As shown, the four large and two small sextet peaks are superoxide free radicals (O2· - These active substances give the bleaching system of the present invention a stronger oxidizing property.
[0076] Depend on Figure 12-14 It can be seen that when there is only PMS in the reaction system, the intensity of the generated free radicals is not high, resulting in a poor bleaching effect. When SDBS is added to the reaction system, the intensity of the free radicals does not change much. However, when PA and PB are added to the reaction system, the intensity of the free radicals is significantly enhanced, and the bleaching effect is significantly enhanced. Polyphosphate can act as a nucleophile (Nu) to attack the asymmetric OO covalent bond of PMS, promote the heterolytic cleavage of the OO bond, and produce sulfate radicals and hydroxyl radicals, as shown in the following formula (1), and then further produce superoxide radicals and singlet oxygen, as shown in the following formulas (2) and (3). Therefore, the PMS / polyphosphate bleaching system of the present invention has higher oxidation performance, the colored substances attached to the cotton linter pulp are removed more efficiently, and the whiteness of the refined cotton is improved.
[0077] (1) (2) (3) The present invention adopts PMS as the main bleaching agent to prepare the bleaching agent, and bleaching the unbleached cotton linter pulp, the obtained refined cotton has a whiteness of more than 70 (70-86), a polymerization degree of more than 1000 (1000-2210), and a degree of polymerization reduction of 15%-64% relative to the unbleached cotton linter pulp. The test results show that the process of the present invention not only has a good bleaching effect, can effectively remove the colored substances attached to the cellulose, but also has a small degree of damage to the cellulose. The bleaching method of the present invention obtains refined cotton with high whiteness and high polymerization degree in a relatively short time and mild process conditions. Compared with the traditional bleaching method, this process does not contain chlorine element, does not produce organic chlorides and other teratogenic and mutagenic substances, can reduce the pollution load, and the COD content in the waste liquid after bleaching is less than 280 mg / L, which is green and environmentally friendly.
[0078] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A chlorine-free bleaching agent for cotton linter pulp, characterized in that: The invention comprises, by weight, 1.4 to 7.9 parts of persulfate, 2.7 to 9.2 parts of pyrophosphate, 1.4 to 7.9 parts of polyphosphate, 1.4 to 7.9 parts of anionic surfactant and 1000 parts of water; the pH value of the chlorine-free bleaching agent for cotton linter pulp is 8.5 to 11.
0.
2. The chlorine-free bleaching agent for cotton linter pulp according to claim 1, characterized in that: The invention comprises, by weight, 2.7 to 7.9 parts of persulfate, 4 to 7.9 parts of pyrophosphate, 2.7 to 6.6 parts of polyphosphate, 1.4 to 6.6 parts of anionic surfactant and 1000 parts of water; the pH value of the chlorine-free bleaching agent for cotton linter pulp is 9.0 to 10.
5.
3. The chlorine-free bleaching agent for cotton linter pulp according to claim 1, characterized in that: The invention comprises, by weight, 4 to 6.6 parts of persulfate, 5.3 to 6.6 parts of pyrophosphate, 4 to 5.3 parts of polyphosphate, 2.7 to 6.6 parts of anionic surfactant and 1000 parts of water; the pH value of the chlorine-free bleaching agent for cotton linter pulp is 9.0 to 10.
0.
4. The chlorine-free bleaching agent for cotton linter pulp according to claim 1, characterized in that: By mass, it includes 5.3 parts of persulfate, 6.6 parts of pyrophosphate, 5.3 parts of polyphosphate, 6.6 parts of anionic surfactant and 1000 parts of water; the pH value of the cotton linter pulp chlorine-free bleaching agent is 9.
5.
5. The chlorine-free bleaching agent for cotton linter pulp according to claim 1, characterized in that: The persulfate includes potassium persulfate, the pyrophosphate includes sodium pyrophosphate, the polyphosphate includes sodium tripolyphosphate, and the anionic surfactant includes sodium dodecylbenzene sulfonate.
6. A method for bleaching cotton linter pulp, characterized in that: The following steps are involved: soaking cotton linter pulp in a bleaching agent, mixing them evenly, to obtain a mixture; the bleaching agent is the bleaching agent according to any one of claims 1 to 5; The pH of the mixture is adjusted to alkaline, a bleaching reaction is carried out, and after the reaction is completed, the mixture is cleaned and dried to complete the bleaching of the cotton linter pulp.
7. The method for bleaching cotton linter pulp according to claim 6, characterized in that: The bath ratio of the cotton linter pulp to the bleaching agent is 1:(10-60).
8. The method for bleaching cotton linter pulp according to claim 6, characterized in that: The pH of the mixture was adjusted to 8.5-11.
9. The method for bleaching cotton linter pulp according to claim 6, characterized in that: The bleaching reaction is carried out at 30-80° C. for 10-60 minutes.
10. The method for bleaching cotton linter pulp according to claim 6, characterized in that: During the bleaching reaction, stirring is performed every 3 to 8 minutes.
Citation Information
Patent Citations
Acidic oxidation bleaching process of cashmere fibers
CN103485152A
Detergent composition
GB1477546A
Improvements in and relating to the bleaching of cotton fibres
GB894070A
Peroxide-dipersulfate bleaching of cotton fibers
US3026166A