Preparation method of all-steel-slag Kepp seal coat
Through the preparation method of the all-steel slag capping layer, high-solid content emulsified asphalt and steel slag are sprayed simultaneously to form a steel slag gravel seal, and a fog seal and micro-surface are added thereon, which solves the construction of steel slag on high-grade roads. The problems of low efficiency and poor bonding effect have achieved higher road wear resistance and water sealing performance, and expanded the application range of steel slag.
Patent Information
- Application Number
- CN202411225388.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure CN118880689A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of highway maintenance, and in particular relates to a method for preparing a full steel slag cape seal. Background Art
[0002] Steel slag is an industrial solid waste, which is produced in large quantities every year. If it is not treated, it will have an adverse impact on the environment. Although steel slag has a wide range of applications, its utilization rate in my country is still low. The rational use of steel slag to reuse resources can turn waste into treasure and create huge economic benefits. It is an effective way to achieve sustainable development and is of great significance to the country and society.
[0003] Chinese patent CN113250036A discloses a method for preparing asphalt synchronous crushed stone upper sealing layer using steel slag, which includes the following steps: the first step is pretreatment of the base layer; the second step is spraying the first layer of emulsified asphalt, rolling it flat, drying it, and spreading steel slag; the third step is spraying the second layer of emulsified asphalt, rolling it flat, and drying it. This patent adopts a variant asynchronous construction method, first spreading emulsified asphalt to break the emulsion, then spreading stones, and then spreading emulsified asphalt after the stones stick to it. The steps are relatively complicated, resulting in low construction efficiency, which leads to a long construction time; at the same time, because the process is not perfect after the emulsified asphalt is spread, the bonding effect between the stone and the asphalt is poor, and the bonding between the steel slag and the asphalt is insufficient. After opening the traffic, there may be a risk of stone falling off and scattering, which affects traffic and causes harm to vehicles. Therefore, it can only be used to make low-grade roads and cannot be used on high-grade roads.
[0004] The difference between low-grade and high-grade pavements in the highway industry is that high-grade roads refer to expressways and first-class roads, which generally have faster speeds and larger traffic volumes. Currently, the technology of directly using steel slag as raw material to prepare high-grade pavements has yet to be improved. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a full steel slag cape seal, which uses steel slag to prepare the cape seal, fully utilizes the hardness and wear resistance of the steel slag, greatly improves the wear resistance of the road surface, improves the water sealing coefficient, and increases the life of the road; reuses steel slag resources, turns waste into treasure, and creates huge economic benefits.
[0006] To achieve the above purpose, the technical solution of the present invention is as follows:
[0007] A method for preparing a full steel slag cape seal comprises the following steps:
[0008] 1) Clean and blow away the debris on the base layer and repair the base layer;
[0009] 2) Spraying fast-cracking high-solid emulsified asphalt and steel slag simultaneously, rolling the emulsified asphalt after initial demulsification, and forming a steel slag gravel seal after molding; the solid content of the high-solid emulsified asphalt is ≥65%;
[0010] 3) Adsorb pumice and spray a mist seal layer on the steel slag gravel seal layer, and the mist seal layer breaks the emulsion and takes shape;
[0011] 4) Use steel slag to perform micro-surfacing or slurry sealing on the steel slag crushed stone seal to form a composite surface wear layer, and obtain a Cape seal after molding.
[0012] Preferably, the particle size of the steel slag is 3-10 mm, the crushing value is ≤26%, and the f-CaO content is ≤5%.
[0013] Preferably, the time taken for the initial demulsification of the emulsified asphalt is 5 to 15 minutes.
[0014] Preferably, the temperature of the emulsified asphalt is 40-60°C, preferably 55-60°C.
[0015] Preferably, the thickness of the steel slag crushed stone seal is 3 to 10 mm, preferably 3 mm, 5 mm or 9 mm.
[0016] Preferably, the amount of emulsified asphalt sprayed is 1.3-2.3 kg / m according to the thickness of the steel slag gravel seal. 2 Preferably, for steel slag thickness of 3mm, 5mm or 9mm, the amount of emulsified asphalt sprayed is 1.3-1.6kg / m 2 , 1.4~1.9kg / m 2 , 1.7~2.3kg / m 2 .
[0017] Preferably, the rolling time is 5 to 10 minutes.
[0018] Preferably, the spraying amount of the fog seal layer is 0.2-1.2 kg / m 2 , preferably 0.4kg / m 2 .
[0019] Preferably, the demulsification forming time of the mist seal layer is 0.5 to 1 hour.
[0020] The present invention uses steel slag micro-surfacing or steel slag slurry seal to prepare a chip seal based on steel slag, and improves the process into a Cape seal, so that this process can be used on high-grade pavements, while increasing the pavement life, increasing the pavement's water damage resistance, and improving the pavement's water sealing capacity. It also increases the application scope of steel slag and makes the utilization rate of steel slag more sufficient.
[0021] The present invention sprays fast-cracking high-solid emulsified asphalt and steel slag simultaneously, so that the emulsified asphalt and steel slag are mixed together to form a steel slag gravel seal; the emulsified asphalt is prepared with a fast-cracking emulsifier; the solid content of the emulsified asphalt is ≥65%, thereby increasing the viscosity of the emulsified asphalt and greatly improving the demulsification speed of the emulsified asphalt. The use temperature of the emulsified asphalt is increased to 40-60°C, preferably 55-60°C, to improve the demulsification speed of the emulsified asphalt. During construction, a gravel seal synchronous sealing vehicle is used for construction, so that the emulsified asphalt and the steel slag can be spread synchronously and quickly.
[0022] There is no restriction on the source of the steel slag, which is preferably crushed converter drum steel slag with a particle size of 3 to 10 mm and an f-CaO content of ≤5%. By limiting the particle size of the steel slag, the strength of the steel slag particles meets the requirements of road construction. The f-CaO content refers to the free CaO content in the steel slag. The f-CaO content of the steel slag is limited to ≤5%, eliminating the instability of the steel slag, making its performance indicators meet the requirements of industry standards, and preventing the subsequent disintegration and pulverization of the steel slag from causing road surface bulges and cracks. In some embodiments of the present invention, the particle size of the steel slag is 3 to 10 mm, and the f-CaO content is ≤5%. In some embodiments of the present invention, the crushing value of the steel slag is further limited to ≤26%, thereby meeting the requirements of high-grade roads.
[0023] The thickness of the steel slag gravel seal is generally 3-10mm. According to the actual road conditions and steel slag conditions, the preferred thickness of the steel slag gravel seal is 3mm, 5mm, 9mm, etc. According to the thickness of the steel slag gravel seal, the amount of emulsified asphalt to be spread is 1.3-2.3kg / m 2 For the thickness of steel slag gravel seal layer of 3mm, 5mm and 9mm, the amount of emulsified asphalt sprayed is 1.3-1.6kg / m 2 , 1.4 -1.9kg / m 2 , 1.7-2.3kg / m 2 .
[0024] After the emulsified asphalt is initially demulsified, a rubber-wheel roller is introduced to compact it, which helps to arrange the steel slag, enhances the bonding between the steel slag and asphalt, increases the bonding effect between the steel slag gravel seal layer and the original road surface, and increases the durability of the steel slag gravel seal layer.
[0025] After the steel slag gravel seal is formed, spray the mist seal on the steel slag gravel seal to break the emulsion and form the mist seal. The introduction of the mist seal also increases the durability and water sealing performance of the steel slag gravel seal. The spraying amount of the mist seal is 0.2-1.2kg / m 2 , preferably 0.4kg / m 2 .
[0026] Finally, steel slag is used for micro-surfacing or slurry sealing on the surface of the fog seal layer. After the steel slag micro-surfacing is formed, it can be directly opened to traffic without rolling.
[0027] The original process of emulsified asphalt, steel slag, and emulsified asphalt step-by-step spreading and waiting is simplified to a fast process of emulsified asphalt / steel slag and fog seal. At the same time, fast-cracking high-solid emulsified asphalt and fog seal are selected to increase the demulsification speed, increase construction efficiency, and achieve the purpose of rapid opening of traffic. The molding time is 0.5-1h, and the molding time in the present invention refers to the demulsification and solidification of emulsified asphalt.
[0028] Compared with the existing process, the invention has the following beneficial effects:
[0029] Using steel slag as aggregate for crushed stone seal can replace commonly used aggregates such as basalt, which is a recycling of resources. The Cape seal structure increases the life of the road surface, and the porous structure of steel slag itself can better combine with emulsified asphalt and asphalt, thereby increasing the life of the road surface.
[0030] Micro-surfacing can resist water damage and separate water, but if the wrong materials are used, the effect will not be very good, and may even have a counter-effect. The present invention uses steel slag for micro-surfacing. The biggest advantage is that the steel slag itself is hard and wear-resistant, which makes the road surface have a longer life. If the stone has poor wear resistance, as the road is opened to traffic, the aggregate will gradually wear out quickly, causing road surface diseases. Secondly, steel slag is relatively stable, which can effectively ensure the life of the road surface. If traditional stone is used, on the one hand, the wear resistance is poor, and on the other hand, the stone itself is greatly affected by the mining time and mining location, and the quality varies greatly, making it difficult to guarantee the quality of the prepared road surface.
[0031] The invention simultaneously sprays quick-cracking high-solid content emulsified asphalt and steel slag when preparing the steel slag crushed stone seal, thereby simplifying the process flow and shortening the time. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 Schematic diagram of a flow chart of an embodiment of the present invention. DETAILED DESCRIPTION
[0033] The present invention will be further described below in conjunction with the embodiments and drawings.
[0034] See also Figure 1 , Example 1
[0035] A method for preparing a full steel slag cape seal comprises the following steps:
[0036] 1) Clean and blow away the debris and soil on the road base, and cover the surface layers that need to be protected, such as curbstones and manhole covers, with plastic film;
[0037] 2) Spraying fast-cracking high-solid emulsified asphalt and steel slag simultaneously, after the emulsified asphalt is initially demulsified, rolling it with a rubber-wheel roller for 10 minutes, and forming a steel slag gravel seal layer after molding; the emulsified asphalt is prepared using the fast-cracking emulsifier Indulin AA-63D of Shanghai Invitrogen, with a solid content of 66% and a temperature of 60°C; the steel slag used is the converter drum slag of Shanghai Baosteel, with a particle size range of 8-10mm and an f-CaO content of no more than 5%;
[0038] 3) Adsorb pumice and spray a mist seal layer on the steel slag gravel seal layer. The mist seal layer will break up and take shape. The next step of construction will be carried out one week after the traffic is opened.
[0039] 4) For paving MS-III micro-surfacing, emulsified asphalt was used. The slow-cracking and fast-setting emulsifier Indulin MQ3 produced by Shanghai Invitrogen was used to prepare the emulsified asphalt. The steel slag used was from the converter drum slag of Shanghai Baosteel. The particle size range was: 0-9mm continuous graded steel slag, the f-CaO content did not exceed 5%, and the slag was opened to traffic after molding.
[0040] Example 2
[0041] The difference from Example 1 is that the next step of micro-surfacing construction is directly carried out after the mist seal layer is demulsified and formed.
[0042] Example 3
[0043] The difference from Example 1 is that the micro-surfacing uses the spreading micro-surfacing MS-II type micro-surfacing, and the steel slag used is from the converter drum slag of Shanghai Baosteel, with a particle size range of: 0-5mm continuous graded steel slag, and the f-CaO content does not exceed 5%.
[0044] Comparative Example 1
[0045] The difference from Example 1 is that basalt with the same particle size is used instead of steel slag.
[0046] Comparative Example 2
[0047] The difference from Example 2 is that the micro-surfacing is directly spread without spreading the mist seal layer.
[0048] Comparative Example 3
[0049] The difference from Example 2 is that no micro-surfacing is applied after spreading the mist seal layer.
[0050] Table 1
[0051]
[0052] The construction time includes the time of each step, among which the time of covering and removing the plastic film is calculated as the same time. For the methods of sweeping loss rate and gravel shedding rate, please refer to T / CECS G: M54-01-2023 Technical Specification for Highway Maintenance Gravel Seal. The sweeping loss rate indicates the forming speed of the gravel seal; the gravel shedding rate indicates the bonding effect of the gravel seal; the water permeability coefficient indicates the water sealing effect; and the wet wheel wear indicates the anti-water damage effect.
[0053] From the data in Table 1, it can be seen that the present invention uses steel slag instead of basalt to prepare the Cape seal, and the obtained Cape seal performance can meet the pavement performance requirements, proving that steel slag can replace basalt as road aggregate. Moreover, on the basis of conventional Cape seal, the present invention further adds a micro-surfacing design to improve the water damage resistance of the Cape seal.
[0054] Comparative Example 1 shows that compared with traditional basalt, the performance of steel slag can meet the pavement performance requirements and can replace basalt as road aggregate. In addition, the introduction of steel slag results in smaller wet wheel wear data, which means that the road durability and water damage resistance are stronger.
[0055] In comparative example 2, the construction was carried out directly without spreading the fog seal layer. The crushed stone loss rate was high and the floating stone was easy to fall off, which prolonged the construction time.
[0056] Comparative Example 3 shows that if micro-surfacing is not added, the water damage resistance and wear resistance are poor, and there is a certain amount of water seepage, which shows that steel slag micro-surfacing brings good water sealing effect and water damage resistance effect.
Claims
1. A method for preparing a full steel slag Cape seal, characterized in that: The steps include: 1) Clean and blow away the debris on the base layer and repair the base layer; 2) Spraying fast-cracking high-solid emulsified asphalt and steel slag simultaneously, rolling the emulsified asphalt after initial demulsification, and forming a steel slag gravel seal after molding; the solid content of the high-solid emulsified asphalt is ≥65%; 3) Adsorb pumice and spray a mist seal layer on the steel slag gravel seal layer, and the mist seal layer breaks the emulsion and takes shape; 4) Use steel slag to perform micro-surfacing or slurry sealing on the steel slag crushed stone seal to form a composite surface wear layer, and obtain a Cape seal after molding.
2. The method for preparing the all-steel slag cape seal as claimed in claim 1, characterized in that: The particle size of the steel slag is 3-10 mm, the crushing value is ≤26%, and the f-CaO content is ≤5%.
3. The method for preparing a cape seal using steel slag as claimed in claim 1, characterized in that: The temperature of the emulsified asphalt is 40-60°C, preferably 55-60°C.
4. The method for preparing the all-steel slag cape seal as claimed in claim 1, characterized in that: The time required for the initial demulsification of emulsified asphalt is 5 to 15 minutes.
5. The method for preparing the all-steel slag cape seal as claimed in claim 1, characterized in that: The thickness of the steel slag crushed stone seal layer is 3 to 10 mm, preferably 3 mm, 5 mm or 9 mm.
6. The method for preparing the all-steel slag cape seal as claimed in claim 1 or 5, characterized in that: According to the thickness of steel slag gravel seal, the amount of emulsified asphalt to be spread is 1.3-2.3kg / m 2 Preferably, for steel slag thickness of 3mm, 5mm or 9mm, the amount of emulsified asphalt sprayed is 1.3-1.6kg / m 2 , 1.4~1.9kg / m 2 , 1.7~2.3kg / m 2 .
7. The method for preparing the all-steel slag cape seal as claimed in claim 1, characterized in that: The rolling time is 5 to 10 minutes.
8. The method for preparing the all-steel slag cape seal as claimed in claim 1, characterized in that: The spraying amount of the fog seal layer is 0.2~1.2kg / m 2 , preferably 0.4kg / m 2 .
9. The method for preparing the all-steel slag cape seal as claimed in claim 1, characterized in that: The demulsification and forming time of the fog seal layer is 0.5 to 1h.