High-permeability soft magnetic composite material and preparation method thereof

By using insulating coating magnetic powder and release agent in soft magnetic composite materials, combined with high-temperature heat treatment and magnetic field heat treatment, the microstructure of Fe-Si-Al-Zr-R1 and Fe-Si-Ca-R2 magnetic powder is optimized, and the microstructure of Fe-Si-Al-Zr-R1 and Fe-Si-Ca-R2 magnetic powder is solved The problem that existing materials are difficult to have high magnetic permeability and low loss, and efficient medium and high-frequency magnetic performance and anti-saturation capability are achieved.

CN118888243APending Publication Date: 2024-11-01GLOBAL ENERGY INTERCONNECTION RES INST CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410967806.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing soft magnetic composite materials are difficult to have both high magnetic permeability, high saturation resistance and low, medium and high frequency losses, and cannot meet the development needs of large capacity and high efficiency of power electronic devices.

Method used

The preparation method of high magnetic permeability soft magnetic composite material using insulating coated magnetic powder and mold release agent includes two metal magnetic powders: one is Fe-Si-Al-Zr-R1 and the other is Fe-Si-Ca- R2, through V2O5 film and modified high-temperature resistant silicone resin coating, combined with high-temperature heat treatment and magnetic field heat treatment, optimizes the microstructure and magnetic properties of the material.

Benefits of technology

It realizes high permeability, low, medium and high frequency loss, good saturation resistance and resistivity, and is suitable for electrical equipment such as transformers and reactors, meeting the requirements for medium and high frequency use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004952242740000171
    Figure BDA0004952242740000171
Patent Text Reader

Abstract

The invention provides a high-permeability soft magnetic composite material and a preparation method thereof, preparation raw materials comprise insulating coated magnetic powder and a release agent, the insulating coated magnetic powder comprises metal magnetic powder, and a first coating layer and a second coating layer which sequentially coat the surface of the metal magnetic powder from inside to outside; the first coating layer is a V2O5 film insulating layer, and the second coating layer is a modified high-temperature-resistant organic silicon resin insulating layer; and the metal magnetic powder comprises a first kind of metal magnetic powder Fe-Si-Al-Zr-R1 and a second kind of metal magnetic powder Fe-Si-Ca-R2. The high-permeability soft magnetic composite material prepared by the invention has high permeability, high permeability stability, high resistivity and low medium-high frequency loss, and is suitable for electrical equipment such as transformers, reactors and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of soft magnetic composite materials, and in particular to a high magnetic permeability soft magnetic composite material and a preparation method thereof. Background Art

[0002] Soft magnetic composites (SMCs) are advanced magnetic materials that combine the advantages of metal and ferrite soft magnetic materials. It is composed of soft magnetic materials (such as iron, nickel, cobalt, etc.) and non-magnetic materials (such as polymers, ceramics, etc.), and has the characteristics of high magnetic permeability, low coercivity, good mechanical properties and corrosion resistance. This material has a wide range of applications in electronic equipment, power equipment, automobiles and other fields, such as high-frequency transformers, inductors, electromagnetic wave shielding materials, etc. With the rapid development of new energy, photovoltaic, new energy vehicles and other industries, the market demand for soft magnetic composites continues to grow, showing broad development prospects. As the alloy material with the largest market share in soft magnetic composites, the iron silicon aluminum powder core has the lowest loss among soft magnetic composites, but its anti-saturation ability is poor. The iron silicon powder core has good anti-saturation ability, but the loss is relatively high.

[0003] As power electronic devices develop towards large capacity and high efficiency, it is urgent to further improve the magnetic properties of soft magnetic composite materials as it is difficult for current soft magnetic composite materials to simultaneously possess the characteristics of high magnetic permeability, high anti-saturation ability, and low medium and high frequency losses. Summary of the invention

[0004] The purpose of the present invention is to provide a high magnetic permeability soft magnetic composite material and a preparation method thereof to overcome the problems existing in the prior art. The high magnetic permeability soft magnetic composite material prepared by the present invention has high magnetic permeability, high magnetic permeability stability, high resistivity, low medium and high frequency loss, and is suitable for electrical equipment such as transformers and reactors.

[0005] The present invention is achieved through the following technical solutions:

[0006] A high magnetic permeability soft magnetic composite material, wherein the raw materials for preparing the high magnetic permeability soft magnetic composite material include insulating coated magnetic powder and a release agent, wherein the mass ratio of the insulating coated magnetic powder to the release agent is (100-200): (0.1-0.2);

[0007] The insulating coated magnetic powder comprises metal magnetic powder and a first coating layer and a second coating layer sequentially coated on the surface of the metal magnetic powder from the inside to the outside;

[0008] The first coating layer is a V2O5 thin film insulation layer, and the second coating layer is a modified high temperature resistant silicone resin insulation layer;

[0009] The metal magnetic powder includes a first metal magnetic powder and a second metal magnetic powder;

[0010] The first metal magnetic powder includes Fe a Si b Al c Zr d R1 e , wherein R1 is Ce or Gd, a, b, c, d, e are the atomic percentages of the corresponding elements, a+b+c+d+e=100at%, 80at%≤a≤88at%, 6at%≤b≤12at%, 3at%≤c≤8at%, 1at%≤d≤2at%, 1at%≤e≤2at%;

[0011] The second metal magnetic powder includes Fe f Si g Ca h R2 i , wherein R2 is Ce or Gd, f, g, h, i are the atomic percentages of the corresponding elements, f+g+h+i=100at%, 87at%≤f≤94at%, 4at%≤g≤9at%, 1at%≤h≤2at%, 1at%≤i≤2at%.

[0012] Furthermore, the release agent is zinc stearate or calcium stearate.

[0013] Furthermore, the particle size of the first metal magnetic powder includes two ranges: -70 mesh to +160 mesh and -160 mesh to +340 mesh;

[0014] The particle size of the second metal magnetic powder includes two ranges: -120 mesh to +320 mesh and -320 mesh to +500 mesh.

[0015] Furthermore, among the metal magnetic powder, the first metal magnetic powder with a particle size range of -70 mesh to +160 mesh accounts for 60wt% to 70wt%, the first metal magnetic powder with a particle size range of -160 mesh to +340 mesh accounts for 10wt% to 25wt%, the second metal magnetic powder with a particle size of -120 mesh to +320 mesh accounts for 5wt% to 25wt%, and the second metal magnetic powder with a particle size of -320 mesh to +500 mesh accounts for 5wt% to 15wt%.

[0016] A method for preparing the high magnetic permeability soft magnetic composite material according to claim 1, comprising the following steps:

[0017] Depositing a V2O5 thin film insulating layer on the surface of the metal magnetic powder;

[0018] High temperature heat treatment is performed on the metal magnetic powder coated with the V2O5 thin film insulating layer;

[0019] A modified high temperature resistant silicone resin insulating layer is prepared on the outside of the V2O5 thin film insulating layer to obtain insulating coated magnetic powder;

[0020] The insulating coated magnetic powder is mixed with a release agent and pressed into a shape to obtain a soft magnetic powder core;

[0021] The soft magnetic powder core is subjected to a magnetic field heat treatment to obtain a high magnetic permeability soft magnetic composite material.

[0022] Furthermore, the step of depositing a V2O5 thin film insulating layer on the surface of the metal magnetic powder is specifically as follows:

[0023] The V2O5 insulating material is evaporated or sputtered in a vacuum environment by physical vapor deposition, and is deposited on the surface of the metal magnetic powder to form a V2O5 thin film insulating layer with a thickness of 10 to 20 μm.

[0024] Furthermore, the high temperature heat treatment is specifically:

[0025] Under the protection of H2 and N2 atmosphere, first heat up to 200-300°C at a heating rate of 5°C / min, keep warm for 30-90min; then continue to heat up to 650-750°C at a heating rate of 5°C / min, keep warm for 40-80min, and cool with the furnace.

[0026] Furthermore, the modified high temperature resistant silicone resin insulating layer is prepared on the outside of the V2O5 thin film insulating layer, specifically:

[0027] Preparation of modified high temperature resistant silicone resin using boric acid and silicone resin;

[0028] After the modified high temperature resistant organic silicone resin is dissolved in a solvent, a metal magnetic powder coated with a V2O5 thin film insulating layer is added, and the metal magnetic powder is uniformly dispersed by ultrasonication, and then mechanically stirred until dry and dried to obtain a modified high temperature resistant organic silicone resin insulating layer on the outside of the V2O5 thin film insulating layer;

[0029] The mass ratio of the metal magnetic powder coated with the V2O5 thin film insulating layer, the modified high temperature resistant silicone resin and the solvent is 100: (1.5-3): (200-500);

[0030] The solvent is a mixture of acetone and deionized water, and the mass ratio of acetone to deionized water is 100:(2-5);

[0031] The organic silicon resin is silicone resin.

[0032] Furthermore, the pressing pressure is 1200Mpa to 2100Mpa.

[0033] Further, the magnetic field heat treatment is specifically as follows: under the protection of N2 atmosphere, firstly heating to 200-300°C at a heating rate of 5°C / min, keeping the temperature for 30-90min; then heating to 550-650°C at a heating rate of 5°C / min, keeping the temperature for 20-60min, and cooling with the furnace;

[0034] After the temperature is raised to 200-300°C and kept at this temperature for 30-90 minutes, a magnetic field of 50-100 mA is continuously applied until the end.

[0035] Compared with the prior art, the present invention has the following beneficial technical effects:

[0036] The high magnetic permeability soft magnetic composite material of the present invention comprises two kinds of metal magnetic powders, the first kind of metal magnetic powder comprises Fe-Si-Al-Zr-R1, and the second kind of metal magnetic powder comprises Fe-Si-Ca-R2, wherein R1 and R2 are respectively one of the rare earth elements Ce and Gd, and the first kind of metal magnetic powder is obtained by adding Zr and rare earth elements to iron silicon aluminum magnetic powder, wherein the addition of Zr element can help to optimize the microstructure of the material, refine the grain structure, reduce the grain boundary resistance inside the magnetic material, thereby reducing eddy current loss, and improve its initial magnetic permeability, especially in high-frequency applications, can effectively improve the high-frequency magnetic properties of the magnetic powder core, and the addition of Zr element helps to enhance the temperature stability of the magnetic powder core; the second kind of metal magnetic powder is obtained by adding Ca and rare earth elements to iron silicon magnetic powder, wherein the addition of Ca element can improve the resistivity of the alloy and reduce the eddy current loss, the eddy current loss is more obvious under high frequency conditions, and reducing the eddy current loss can significantly reduce the high-frequency loss, and at the same time can be beneficial to the refinement of the alloy powder, and further improve the magnetic properties.

[0037] In addition, rare earth elements Ce and Gd are added to both magnetic powders. Compared with other rare earth elements, rare earth elements Ce and Gd can not only improve the oxidation resistance and corrosion resistance of magnetic powder core materials, but also have higher magnetic moments, which can improve magnetic induction intensity and better magnetic saturation characteristics. In addition, they can improve magnetic permeability by refining grains, especially in medium and high frequency applications, which can reduce medium and high frequency eddy current losses. However, if added in excess, the magnetic properties will deteriorate.

[0038] Furthermore, by selecting a suitable release agent and a corresponding ratio, different molds can be selected to press various shapes of green compacts according to different equipment or parts requirements. The best effect is achieved when the mass ratio of insulating coated magnetic powder to release agent is (100-200): (0.1-0.2).

[0039] Furthermore, the particle sizes of the first metal magnetic powder include two types: -70 mesh to +160 mesh, accounting for 60wt% to 70wt%, and -160 mesh to +340 mesh, accounting for 10wt% to 25wt%. The particle sizes of the second metal magnetic powder include two types: -120 mesh to +320 mesh, accounting for 5wt% to 25wt%, and -320 mesh to +500 mesh, accounting for 5wt% to 15wt%. The present invention can effectively adjust the spacing between magnetic powder particles by reasonably matching two magnetic powders with four particle sizes. The addition of small-size particles can increase the density of the magnetic powder core because they can be more tightly filled between large-size particles, making the particles more tightly bonded, thereby improving its magnetic properties and mechanical properties.

[0040] The preparation method of the soft magnetic composite material provided by the present invention comprises two kinds of metal magnetic powders, the first kind of metal magnetic powder comprises Fe-Si-Al-Zr-R1, and the second kind of metal magnetic powder comprises Fe-Si-Ca-R2. The high-frequency loss of the first kind of metal magnetic powder is lower than that of the second kind, but the anti-saturation ability is not as good as that of the second kind. The advantages of the two kinds of metal magnetic powders can be combined by mixed preparation to improve the medium and high-frequency magnetic properties of the soft magnetic composite material. Both kinds of metal magnetic powders are prepared by mechanical method or atomization method, which can accurately control the size of powder particles, generate uniform and fine particles, help to improve the density and obtain a magnetic core with more stable magnetic properties. Secondly, preferably, the rapid cooling rate during the water atomization process causes the liquid metal or alloy to quickly solidify into a microcrystalline structure, which helps to reduce the eddy current loss of the magnetic core. Finally, the powder prepared by the mechanical method or atomization process can obtain an ideal microstructure after subsequent insulation packaging and appropriate heat treatment, thereby achieving superior magnetic properties in terms of lower medium and high frequency losses, higher magnetic permeability and excellent temperature stability.

[0041] Furthermore, a double coating method is used in the insulation coating process. First, an inorganic coating is used for coating. Physical vapor deposition is used to deposit V2O5 insulating material on the surface of the magnetic powder core. The V2O5 glassy particles maintain their excellent thermoplastic forming properties during consolidation, which can largely solve the problem of not being able to obtain high density of the green compact. The magnetic powder core obtained in this way not only has high magnetic permeability, but also has low coercive force, and eddy current loss is also reduced to a certain extent. The second coating layer is coated with an organic modified coating to form a silicone resin coating layer. The organic-inorganic composite coating material can not only provide high resistivity, but also has good adhesion and thermal stability using silicone resin, so that it can provide sufficient mechanical strength. At the same time, it can also release the internal stress generated during pressing through high-temperature annealing, so as to achieve the purpose of improving the magnetic properties of the soft magnetic composite material and reducing medium and high frequency losses.

[0042] Furthermore, high-temperature heat treatment is required after the first coating, and high-temperature heat treatment can significantly optimize the structure and performance of the inorganic insulating coating. Through heat treatment, the residual stress and defects in the inorganic insulating material can be eliminated, and the inorganic insulating material can be better penetrated into the tiny pores of the magnetic powder core, making its structure more dense and uniform, which can not only improve the insulation performance of the inorganic insulating coating, but also enhance its thermal stability and mechanical strength. At the same time, while optimizing the inorganic insulating coating, the high-temperature heat treatment will not destroy the second organic insulating coating, avoiding adverse effects on the organic insulating coating.

[0043] Furthermore, during the pressing process, as the pressing pressure increases, the contact area between particles increases, and excellent density and magnetic permeability of the magnetic powder core can be obtained. The best overall performance is achieved when the pressing pressure is 1200Mpa to 2100Mpa. Further increasing the pressing pressure will lead to deterioration of performance.

[0044] Furthermore, during the magnetic field heat treatment process, the residual stress and defects inside the magnetic powder core can be further eliminated, and the magnetic domain structure can be improved, thereby improving the magnetic permeability of the magnetic powder core and reducing magnetic loss. The use of N2 as the heat treatment gas can play a protective and anti-oxidation role. In addition, the magnetic field heat treatment adopts a two-stage temperature rise heat treatment. The first stage is the stress relief stage, which can eliminate internal defects and release internal stress. The second stage makes the two magnetic powders and two layers of insulating coating more evenly distributed. At the same time, the lower heat treatment temperature in the second stage will not destroy the structure of the organic coating insulating layer, improve its heat resistance and durability, thereby ensuring that the magnetic powder core can maintain stable insulation performance during long-term use, so that the magnetic powder core has better magnetic properties in high voltage, medium and high frequency working environments. At the same time, a magnetic field is applied in the second stage, which can further improve the magnetic domain structure inside the composite material.

[0045] The high magnetic permeability soft magnetic composite material prepared by the present invention has a loss of P1.2T / 50Hz=17.66W / dm3~19.21W / dm3, P0.05T / 50kHz=38.37W / dm3~41.23W / dm3, an effective magnetic permeability of greater than 90 at 100kHz, a closed magnetic circuit anti-saturation capability (magnetic permeability attenuation rate under 100Oe magnetic field) greater than 79%, and a resistivity higher than 2×10 11 The soft magnetic composite material provided by the present invention has the advantages of high high-frequency magnetic permeability, high resistivity, low medium and high frequency loss, good anti-saturation ability, etc., and meets the requirements for medium and high frequency use. DETAILED DESCRIPTION

[0046] The present invention is described in detail below:

[0047] The invention provides a high magnetic permeability soft magnetic composite material. The raw materials for preparing the composite material comprise insulating coated magnetic powder and a release agent. The mass ratio of the insulating coated magnetic powder to the release agent is (100-200): (0.1-0.2). The release agent is zinc stearate or calcium stearate.

[0048] The insulating coated magnetic powder includes metal magnetic powder and a first coating layer and a second coating layer sequentially wrapped on the surface of the metal magnetic powder from the inside to the outside; the first coating layer is a V2O5 thin film insulating layer, and the second coating layer is a modified high-temperature resistant silicone resin insulating layer; the metal magnetic powder includes a first metal magnetic powder and a second metal magnetic powder.

[0049] The first metal magnetic powder includes Fe a Si b Al c Zr d R1 e , wherein R1 is Ce or Gd, a, b, c, d, e are the atomic percentages of the corresponding elements, a+b+c+d+e=100at%, 80at%≤a≤88at%, 6at%≤b≤12at%, 3at%≤c≤8at%, 1at%≤d≤2at%, 1at%≤e≤2at%; the second metal magnetic powder includes Fe f Si g Ca h R2 i , wherein R2 is Ce or Gd, f, g, h, i are the atomic percentages of the corresponding elements, f+g+h+i=100at%, 87at%≤f≤94at%, 4at%≤g≤9at%, 1at%≤h≤2at%, 1at%≤i≤2at%.

[0050] The particle size of the first metal magnetic powder includes two ranges: -70 mesh to +160 mesh and -160 mesh to +340 mesh; the particle size of the second metal magnetic powder includes two ranges: -120 mesh to +320 mesh and -320 mesh to +500 mesh; among the metal magnetic powders, the first metal magnetic powder with a particle size range of -70 mesh to +160 mesh accounts for 60wt% to 70wt%, the first metal magnetic powder with a particle size range of -160 mesh to +340 mesh accounts for 10wt% to 25wt%, the second metal magnetic powder with a particle size of -120 mesh to +320 mesh accounts for 5wt% to 25wt%, and the second metal magnetic powder with a particle size of -320 mesh to +500 mesh accounts for 5wt% to 15wt%.

[0051] The present invention also provides a method for preparing the above-mentioned high magnetic permeability soft magnetic composite material, comprising vacuum alloy smelting → mechanical or atomization powder making → powder screening and particle size grading → first coating of metal magnetic powder surface → high temperature heat treatment → second coating of metal magnetic powder surface → pressing and molding → magnetic field heat treatment.

[0052] During the vacuum alloy smelting process, the first metal magnetic powder raw material is smelted first, cooled to form an alloy ingot, and then the second metal magnetic powder raw material is smelted; the powder is made by mechanical or atomization method, preferably, water atomization method is used, the particle size of the first metal magnetic powder includes two types of -70 mesh to +160 mesh, -160 mesh to +340 mesh, and the particle size of the second metal magnetic powder includes two types of -120 mesh to +320 mesh, -320 mesh to +500 mesh; the metal magnetic powder Among them, the first particle size of the first metal magnetic powder (-70 mesh ~ +160 mesh) accounts for 60wt% ~ 70wt%, the second particle size of the first metal magnetic powder (160 mesh ~ +340 mesh) accounts for 10wt% ~ 25wt%, the first particle size of the second metal magnetic powder (-120 mesh ~ +320 mesh) accounts for 5wt% ~ 25wt%, and the second particle size of the second metal magnetic powder (-320 mesh ~ +500 mesh) accounts for 5wt% ~ 15wt%.

[0053] During the magnetic powder surface coating process, a first coating layer and a second coating layer are sequentially coated on the surface of the metal magnetic powder from the inside to the outside.

[0054] The first coating layer is coated with an inorganic coating, and the V2O5 insulating material is evaporated or sputtered in a vacuum environment by physical vapor deposition, so that it is deposited on the surface of the metal magnetic powder to form a V2O5 thin film insulating layer with a thickness of 10 to 20 μm.

[0055] After the first coating on the surface of the metal magnetic powder, high-temperature heat treatment is required. The high-temperature heat treatment process includes: under the protection of H2+N2 atmosphere, first heating to 200-300℃ at a heating rate of 5℃ / min, keeping warm for 30-90min; then continue heating to 650-750℃ at a heating rate of 5℃ / min, keeping warm for 40-80min, and cooling with the furnace.

[0056] The second coating layer is coated with an organic modified coating. First, a modified high-temperature resistant silicone resin is prepared using boric acid and silicone resin. For example, it is a silicone resin. Then, the modified high-temperature resistant silicone resin is dissolved in a solvent and the dried V2O5-coated metal magnetic powder is added. The metal magnetic powder is evenly dispersed in the resin / organic solvent by ultrasonic action for 15 minutes. The metal magnetic powder is mechanically stirred until dry and further dried in a dryer to prepare an insulating layer coated with the modified high-temperature resistant silicone resin to obtain an insulating coated magnetic powder.

[0057] The mass ratio of the metal magnetic powder coated with V2O5, the modified high temperature resistant silicone resin and the solvent is 100:(1.5-3):(200-500), and the solvent is a mixture of acetone and deionized water, and the mass ratio thereof is 100:(2-5).

[0058] The insulating coated magnetic powder and the release agent are mixed in a mass ratio of (100-200): (0.1-0.2) and pressed into a mold at a pressure of 1200Mpa-2100Mpa to obtain a soft magnetic powder core.

[0059] The soft magnetic powder core is subjected to magnetic field heat treatment to obtain a soft magnetic composite material, wherein the magnetic field heat treatment process includes: under the protection of N2 atmosphere, first heating to 200-300°C at a heating rate of 5°C / min, and keeping warm for 30-90min; then applying a 50-100mA magnetic field until the end, continuing to heat to 550-650°C at a heating rate of 5°C / min, keeping warm for 20-60min, and cooling with the furnace.

[0060] The embodiments of the present invention will be described in detail below in conjunction with the examples. The implementation cases are preferred embodiments of the present invention and should not be used to limit the scope of the present invention. In the following examples, the methods and experimental equipment used are all conventional methods and instruments unless otherwise specified.

[0061] Example 1

[0062] This embodiment provides a method for preparing a high magnetic permeability soft magnetic composite material, comprising the following steps:

[0063] (1) Vacuum alloy smelting: two kinds of metal magnetic powder are prepared. The first kind of metal magnetic powder has the following composition in atomic percentage: Fe 83%, Si 9%, Al 5%, Zr 2%, Ce 1%; the second kind of metal magnetic powder has the following composition in atomic percentage: Fe 90%, Si 7%, Ca 1%, Gd 2%.

[0064] (2) Mechanical or atomization powder making: using mechanical or water atomization method, the particle size of the first metal magnetic powder includes two types: -70 mesh to +160 mesh, -160 mesh to +340 mesh, and the particle size of the second metal magnetic powder includes two types: -120 mesh to +320 mesh, -320 mesh to +500 mesh;

[0065] (3) Powder screening and particle size grading: the first particle size of the first metal magnetic powder accounts for 60wt%, the second particle size of the first metal magnetic powder accounts for 25wt%, the first particle size of the second metal magnetic powder accounts for 10wt%, and the second particle size of the second metal magnetic powder accounts for 5wt%.

[0066] (4) The first coating of the metal magnetic powder surface: The first coating layer is coated with an inorganic coating. The V2O5 insulating material is evaporated or sputtered in a vacuum environment by physical vapor deposition, so that it is deposited on the surface of the magnetic powder core to form a V2O5 thin film insulating layer with a thickness of 10 μm.

[0067] (5) High temperature heat treatment: Under the protection of H2+N2 atmosphere, first heat the sample to 250℃ at a heating rate of 5℃ / min and keep it at that temperature for 45min; then heat the sample to 700℃ at a heating rate of 5℃ / min and keep it at that temperature for 60min, then cool it with the furnace.

[0068] (6) Second coating on the surface of magnetic powder: The second coating layer is coated with an organic modified coating. First, a modified high-temperature resistant silicone resin is prepared using boric acid and organic silicone resin. Then, the modified high-temperature resistant silicone resin is dissolved in an organic solvent and added with the dried V2O5-coated metal magnetic powder. Ultrasonication is applied for 15 minutes to make it evenly dispersed in the resin / organic solvent. The powder is mechanically stirred until dry and dried to prepare an insulating layer coated with the modified high-temperature resistant silicone resin.

[0069] The mass ratio of the metal magnetic powder coated with V2O5, the modified high temperature resistant silicone resin and the solvent in the second coating layer is 100:1.5:200, and the solvent is acetone and deionized water, and the mass ratio thereof is 100:2.

[0070] (7) The insulating coated magnetic powder and the release agent are mixed in a mass ratio of 100:0.1 and pressed into shape. The pressing pressure of the soft magnetic powder core is 1800 MPa.

[0071] (8) Magnetic field heat treatment: Under the protection of N2 atmosphere, the temperature was first increased to 250°C at a heating rate of 5°C / min and kept at this temperature for 60 min. Then, a 70 mA magnetic field was applied until the end, and the temperature was continued to be increased to 600°C at a heating rate of 5°C / min, kept at this temperature for 30 min, and cooled in the furnace to obtain a soft magnetic composite material.

[0072] Example 2

[0073] This embodiment provides a method for preparing a high magnetic permeability soft magnetic composite material, comprising the following steps:

[0074] This embodiment provides a method for preparing a soft magnetic composite material, comprising the following steps:

[0075] (1) Vacuum alloy smelting: two kinds of metal magnetic powders are prepared. The first kind of metal magnetic powder has a composition, by mass percentage, of Fe 87%, Si 7%, Al 4%, Zr 1%, and Ce 1%. The second kind of metal magnetic powder has a composition, by mass percentage, of Fe 88%, Si 9%, Ca 2%, and Ce 1%.

[0076] (2) Mechanical or atomization powder making: using mechanical or water atomization method, the particle size of the first metal magnetic powder includes two types: -70 mesh to +160 mesh, -160 mesh to +340 mesh, and the particle size of the second metal magnetic powder includes two types: -120 mesh to +320 mesh, -320 mesh to +500 mesh;

[0077] (3) Powder screening and particle size grading: the first particle size of the first metal magnetic powder accounts for 70wt%, the second particle size of the first metal magnetic powder accounts for 10wt%, the first particle size of the second metal magnetic powder accounts for 5wt%, and the second particle size of the second metal magnetic powder accounts for 15wt%.

[0078] (4) The first coating of the magnetic powder surface: The first coating layer is coated with an inorganic coating. The V2O5 insulating material is evaporated or sputtered in a vacuum environment by physical vapor deposition, so that it is deposited on the surface of the magnetic powder core to form a V2O5 thin film insulating layer with a thickness of 20 μm.

[0079] (5) High temperature heat treatment: Under the protection of H2+N2 atmosphere, first heat the sample to 200℃ at a heating rate of 5℃ / min and keep it at that temperature for 30min; then continue to heat the sample to 650℃ at a heating rate of 5℃ / min and keep it at that temperature for 40min, then cool it with the furnace.

[0080] (6) Second coating on the surface of magnetic powder: The second coating layer is coated with an organic modified coating. First, a modified high-temperature resistant silicone resin is prepared using boric acid and organic silicone resin. Then, the modified high-temperature resistant silicone resin is dissolved in an organic solvent and added with the dried V2O5-coated metal magnetic powder. Ultrasonication is applied for 15 minutes to make it evenly dispersed in the resin / organic solvent. The powder is mechanically stirred until dry and dried to prepare an insulating layer coated with the modified high-temperature resistant silicone resin.

[0081] The mass ratio of the metal magnetic powder coated with V2O5, the modified high temperature resistant silicone resin and the solvent in the second coating layer is 100:2:300. The solvent is acetone and deionized water, and the mass ratio thereof is 100:3.

[0082] (7) The insulating coated magnetic powder and the release agent are mixed in a mass ratio of 100:0.2 and pressed into shape. The pressing pressure of the soft magnetic powder core is 1900 MPa.

[0083] (8) Magnetic field heat treatment: Under the protection of N2 atmosphere, the temperature was first increased to 200°C at a heating rate of 5°C / min and kept at this temperature for 30 min. Then a 100 mA magnetic field was applied until the end, and the temperature was continued to be increased to 550°C at a heating rate of 5°C / min, kept at this temperature for 20 min, and cooled in the furnace to obtain a soft magnetic composite material.

[0084] Example 3

[0085] This embodiment provides a method for preparing a high magnetic permeability soft magnetic composite material, comprising the following steps:

[0086] (1) Vacuum alloy smelting: two kinds of metal magnetic powder are prepared. The first kind of metal magnetic powder has the following composition in atomic percentage: Fe 88%, Si 6%, Al 3%, Zr 1%, Gd 2%; the second kind of metal magnetic powder has the following composition in atomic percentage: Fe 87%, Si 9%, Ca 2%, Gd 2%.

[0087] (2) Mechanical or atomization powder making: using mechanical or water atomization method, the particle size of the first metal magnetic powder includes two types: -70 mesh to +160 mesh, -160 mesh to +340 mesh, and the particle size of the second metal magnetic powder includes two types: -120 mesh to +320 mesh, -320 mesh to +500 mesh;

[0088] (3) Powder screening and particle size grading: the first particle size of the first metal magnetic powder accounts for 60% by weight, the second particle size of the first metal magnetic powder accounts for 10wt%, the first particle size of the second metal magnetic powder accounts for 25wt%, and the second particle size of the second metal magnetic powder accounts for 5wt%.

[0089] (4) The first coating of the metal magnetic powder surface: The first coating layer is coated with an inorganic coating. The V2O5 insulating material is evaporated or sputtered in a vacuum environment by physical vapor deposition, so that it is deposited on the surface of the magnetic powder core to form a V2O5 thin film insulating layer with a thickness of 15 μm.

[0090] (5) High temperature heat treatment: Under the protection of H2+N2 atmosphere, first heat the sample to 300℃ at a heating rate of 5℃ / min and keep it at that temperature for 90min; then continue to heat the sample to 750℃ at a heating rate of 5℃ / min and keep it at that temperature for 80min, then cool it with the furnace.

[0091] (6) Second coating on the surface of magnetic powder: The second coating layer is coated with an organic modified coating. First, a modified high-temperature resistant silicone resin is prepared using boric acid and organic silicone resin. Then, the modified high-temperature resistant silicone resin is dissolved in an organic solvent and added with the dried V2O5-coated metal magnetic powder. Ultrasonication is applied for 15 minutes to make it evenly dispersed in the resin / organic solvent. The powder is mechanically stirred until dry and dried to prepare an insulating layer coated with the modified high-temperature resistant silicone resin.

[0092] The mass ratio of the metal magnetic powder coated with V2O5, the modified high temperature resistant silicone resin and the solvent in the second coating layer is 100:3:500, and the solvent is acetone and deionized water, and the mass ratio thereof is 100:5.

[0093] (7) The insulating coated magnetic powder and the release agent are mixed in a mass ratio of 200:0.1 and pressed into shape. The pressing pressure of the soft magnetic powder core is 1200 MPa.

[0094] (8) Magnetic field heat treatment: Under the protection of N2 atmosphere, the temperature was first increased to 300°C at a heating rate of 5°C / min and kept at this temperature for 90 min. Then, a 50 mA magnetic field was applied until the end, and the temperature was continued to be increased to 650°C at a heating rate of 5°C / min, kept at this temperature for 60 min, and cooled in the furnace to obtain a soft magnetic composite material.

[0095] Example 4

[0096] This embodiment provides a method for preparing a high magnetic permeability soft magnetic composite material, comprising the following steps:

[0097] (1) Vacuum alloy smelting: two kinds of metal magnetic powder are prepared. The first kind of metal magnetic powder has the following composition in atomic percentage: Fe 80%, Si 12%, Al 6%, Zr 1%, Gd 1%; the second kind of metal magnetic powder has the following composition in atomic percentage: Fe 94%, Si 4%, Ca 1%, Ce 1%.

[0098] (2) Mechanical or atomization powder making: using mechanical or water atomization method, the particle size of the first metal magnetic powder includes two types: -70 mesh to +160 mesh, -160 mesh to +340 mesh, and the particle size of the second metal magnetic powder includes two types: -120 mesh to +320 mesh, -320 mesh to +500 mesh;

[0099] (3) Powder screening and particle size grading: the first particle size of the first metal magnetic powder accounts for 65wt%, the second particle size of the first metal magnetic powder accounts for 15wt%, the first particle size of the second metal magnetic powder accounts for 10wt%, and the second particle size of the second metal magnetic powder accounts for 10wt%.

[0100] (4) The first coating of the metal magnetic powder surface: The first coating layer is coated with an inorganic coating. The V2O5 insulating material is evaporated or sputtered in a vacuum environment by physical vapor deposition, so that it is deposited on the surface of the magnetic powder core to form a V2O5 thin film insulating layer with a thickness of 15 μm.

[0101] (5) High temperature heat treatment: Under the protection of H2+N2 atmosphere, first heat the sample to 280℃ at a heating rate of 5℃ / min and keep it at that temperature for 60min; then continue to heat the sample to 720℃ at a heating rate of 5℃ / min and keep it at that temperature for 50min, then cool it with the furnace.

[0102] (6) Second coating on the surface of magnetic powder: The second coating layer is coated with an organic modified coating. First, a modified high-temperature resistant silicone resin is prepared using boric acid and organic silicone resin. Then, the modified high-temperature resistant silicone resin is dissolved in an organic solvent and added with the dried V2O5-coated metal magnetic powder. Ultrasonication is applied for 15 minutes to make it evenly dispersed in the resin / organic solvent. The powder is mechanically stirred until dry and dried to prepare an insulating layer coated with the modified high-temperature resistant silicone resin.

[0103] The mass ratio of the metal magnetic powder coated with V2O5, the modified high temperature resistant silicone resin and the solvent in the second coating layer is 100:1.5:400, and the solvent is acetone and deionized water, and the mass ratio thereof is 100:4.

[0104] (7) The insulating coated magnetic powder and the release agent are mixed in a mass ratio of 150:0.1 and pressed into shape. The pressing pressure of the soft magnetic powder core is 2100 MPa.

[0105] (8) Magnetic field heat treatment: Under the protection of N2 atmosphere, the temperature was first increased to 250°C at a heating rate of 5°C / min and kept at this temperature for 60 min. Then, a 70 mA magnetic field was applied until the end, and the temperature was continued to be increased to 600°C at a heating rate of 5°C / min, kept at this temperature for 30 min, and cooled in the furnace to obtain a soft magnetic composite material.

[0106] Comparative Example 1

[0107] The soft magnetic composite material of this comparative example uses an alloy composition similar to that of Example 1. The first metal magnetic powder has an atomic percentage of Fe 84%, Si 9%, Al 5%, and Zr 2%. The second metal magnetic powder has an atomic percentage of Fe 91%, Si 8%, and Ca 1%. The difference is that the comparative example does not add rare earth elements. The preparation process of the soft magnetic composite material is the same as that of Example 1.

[0108] Comparative Example 2

[0109] The soft magnetic composite material of this comparative example uses an alloy composition similar to that of Example 1. The first metal magnetic powder has an atomic percentage of Fe 84%, Si 9%, Al 5%, and Ce 2%. The second metal magnetic powder has an atomic percentage of Fe 91%, Si 8%, and Gd 1%. The difference is that the comparative example does not add Zr and Ca elements. The preparation process of the soft magnetic composite material is the same as that of Example 1.

[0110] Comparative Example 3

[0111] The soft magnetic composite material of this comparative example uses an alloy composition similar to that of Example 1, but only one kind of metal magnetic powder is selected, and the composition is: Fe 83%, Si 9%, Al 5%, Zr 2%, Ce 1%, and the particle size includes two types of -70 mesh to +160 mesh and -160 mesh to +340 mesh, with mass proportions of 65wt% and 35wt% respectively. The rest of the preparation process is the same as that of Example 1.

[0112] Comparative Example 4

[0113] The soft magnetic composite material of this comparative example uses an alloy composition similar to that of Example 1, but only one kind of metal magnetic powder is selected, and the composition is: Fe 90%, Si 7%, Ca 1%, Gd 2%, and the particle size includes two types of -120 mesh to +320 mesh and -320 mesh to +500 mesh, with mass proportions of 70wt% and 30wt% respectively. The rest of the preparation process is the same as that of Example 1.

[0114] Comparative Example 5

[0115] The soft magnetic composite material of this comparative example uses the same alloy composition as that of Example 1, except that only the first insulating coating layer is used, and the rest of the preparation process is the same as that of Example 1.

[0116] Comparative Example 6

[0117] The soft magnetic composite material of this comparative example uses the same alloy composition as that of Example 1, except that only the second insulating coating layer is used, and the rest of the preparation process is the same as that of Example 1.

[0118] Comparative Example 7

[0119] The soft magnetic composite material of this comparative example uses the same alloy composition as that of Example 1, except that high-temperature heat treatment is not used. The rest of the preparation process is the same as that of Example 1.

[0120] Comparative Example 8

[0121] The soft magnetic composite material of this comparative example uses the same alloy composition as that of Example 1, except that N2 atmosphere heat treatment is used in the high-temperature heat treatment stage, and the rest of the preparation process is the same as that of Example 1.

[0122] Comparative Example 9

[0123] The soft magnetic composite material of this comparative example uses the same alloy composition as that of Example 1, except that the magnetic field in the magnetic field heat treatment stage of Example 1 is removed, and the rest of the preparation process is the same as that of Example 1.

[0124] Table 1 shows the effective magnetic permeability at 100kHz, the anti-saturation capability of the closed magnetic circuit, the resistivity, and the loss P at a frequency of 50Hz and 50kHz in Examples 1 to 4 and Comparative Examples 1 to 9.

[0125] Table 1

[0126]

[0127] It can be seen from Table 1 that, compared with Example 1, the soft magnetic properties of the soft magnetic composite materials without adding rare earth elements or without adding Zr and Ca elements in Comparative Examples 1 and 2 are not as good as those with adding rare earth elements, Zr and Ca elements. This is because adding these elements is beneficial to optimizing the microstructure of the material, refining the alloy powder, and improving the magnetic properties; compared with Example 1, the soft magnetic properties of the soft magnetic composite materials using only one magnetic powder are not as good as those using two magnetic powders. This is because the advantages of the two metal magnetic powders can be combined to improve the oxidation resistance and corrosion resistance of the magnetic powder core material and improve the magnetic permeability; compared with Example 1, the soft magnetic properties of the soft magnetic composite materials using only the first insulating coating layer or only the second insulating coating layer are not as good as those using two insulating coating layers. This is because the organic-inorganic composite The composite coating material not only provides high resistivity, but also has good adhesion and thermal stability, so as to achieve the purpose of improving the magnetic properties of the soft magnetic composite material; Compared with Example 1, Comparative Example 7 does not adopt high-temperature heat treatment to improve the insulating properties of the inorganic insulating coating layer, and can also enhance its thermal stability and mechanical strength; Compared with Example 1, the soft magnetic properties of the soft magnetic composite material that adopts N2 atmosphere heat treatment in the heat treatment stage are not as good as the magnetic properties of the soft magnetic composite material that adopts N2+H2 atmosphere. This is because the use of N2+H2 atmosphere can better eliminate the residual stress and defects in the inorganic insulating material; Compared with Example 1, the soft magnetic properties of the soft magnetic composite material that does not apply a magnetic field in the heat treatment stage are not as good as the magnetic properties of the soft magnetic composite material that applies a magnetic field in the heat treatment stage. This is because applying a magnetic field can effectively improve the magnetic domain structure inside the composite material, and ultimately improve the magnetic properties of the soft magnetic composite material.

[0128] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.

Claims

1. A high magnetic permeability soft magnetic composite material, characterized in that: The raw materials for preparing the high magnetic permeability soft magnetic composite material include insulating coated magnetic powder and a release agent, and the mass ratio of the insulating coated magnetic powder to the release agent is (100-200): (0.1-0.2); The insulating coated magnetic powder comprises metal magnetic powder and a first coating layer and a second coating layer sequentially coated on the surface of the metal magnetic powder from the inside to the outside; The first coating layer is a V2O5 thin film insulation layer, and the second coating layer is a modified high temperature resistant silicone resin insulation layer; The metal magnetic powder includes a first metal magnetic powder and a second metal magnetic powder; The first metal magnetic powder includes Fe a Si b Al c Zr d R1 e , wherein R1 is Ce or Gd, a, b, c, d, e are the atomic percentages of the corresponding elements, a+b+c+d+e=100at%, 80at%≤a≤88at%, 6at%≤b≤12at%, 3at%≤c≤8at%, 1at%≤d≤2at%, 1at%≤e≤2at%; The second metal magnetic powder includes Fe f Si g Ca h R2 i , wherein R2 is Ce or Gd, f, g, h, i are the atomic percentages of the corresponding elements, f+g+h+i=100at%, 87at%≤f≤94at%, 4at%≤g≤9at%, 1at%≤h≤2at%, 1at%≤i≤2at%.

2. A high magnetic permeability soft magnetic composite material according to claim 1, characterized in that: The release agent is zinc stearate or calcium stearate.

3. The high magnetic permeability soft magnetic composite material according to claim 1, characterized in that: The particle size of the first metal magnetic powder includes two ranges: -70 mesh to +160 mesh and -160 mesh to +340 mesh; The particle size of the second metal magnetic powder includes two ranges: -120 mesh to +320 mesh and -320 mesh to +500 mesh.

4. The high magnetic permeability soft magnetic composite material according to claim 3, characterized in that: Among the metal magnetic powder, the first metal magnetic powder with a particle size range of -70 mesh to +160 mesh accounts for 60wt% to 70wt%, the first metal magnetic powder with a particle size range of -160 mesh to +340 mesh accounts for 10wt% to 25wt%, the second metal magnetic powder with a particle size of -120 mesh to +320 mesh accounts for 5wt% to 25wt%, and the second metal magnetic powder with a particle size of -320 mesh to +500 mesh accounts for 5wt% to 15wt%.

5. A method for preparing the high magnetic permeability soft magnetic composite material according to claim 1, characterized in that: The following steps are involved: Depositing a V2O5 thin film insulating layer on the surface of the metal magnetic powder; High temperature heat treatment is performed on the metal magnetic powder coated with the V2O5 thin film insulating layer; A modified high temperature resistant silicone resin insulating layer is prepared on the outside of the V2O5 thin film insulating layer to obtain insulating coated magnetic powder; The insulating coated magnetic powder is mixed with a release agent and pressed into a shape to obtain a soft magnetic powder core; The soft magnetic powder core is subjected to a magnetic field heat treatment to obtain a high magnetic permeability soft magnetic composite material.

6. The method for preparing a high magnetic permeability soft magnetic composite material according to claim 5, characterized in that: The step of depositing a V2O5 thin film insulating layer on the surface of the metal magnetic powder is specifically as follows: The V2O5 insulating material is evaporated or sputtered in a vacuum environment by physical vapor deposition, and is deposited on the surface of the metal magnetic powder to form a V2O5 thin film insulating layer with a thickness of 10 to 20 μm.

7. The method for preparing a high magnetic permeability soft magnetic composite material according to claim 5, characterized in that: The high temperature heat treatment is specifically: Under the protection of H2 and N2 atmosphere, first heat up to 200-300°C at a heating rate of 5°C / min, keep warm for 30-90min; then continue to heat up to 650-750°C at a heating rate of 5°C / min, keep warm for 40-80min, and cool with the furnace.

8. The method for preparing a high magnetic permeability soft magnetic composite material according to claim 5, characterized in that: The modified high temperature resistant silicone resin insulating layer is prepared on the outside of the V2O5 thin film insulating layer, specifically: Preparation of modified high temperature resistant silicone resin using boric acid and silicone resin; After the modified high temperature resistant organic silicone resin is dissolved in a solvent, a metal magnetic powder coated with a V2O5 thin film insulating layer is added, and the metal magnetic powder is uniformly dispersed by ultrasonication, and then mechanically stirred until dry and dried to obtain a modified high temperature resistant organic silicone resin insulating layer on the outside of the V2O5 thin film insulating layer; The mass ratio of the metal magnetic powder coated with the V2O5 thin film insulating layer, the modified high temperature resistant silicone resin and the solvent is 100: (1.5-3): (200-500); The solvent is a mixture of acetone and deionized water, and the mass ratio of acetone to deionized water is 100:(2-5); The organic silicon resin is silicone resin.

9. The method for preparing a high magnetic permeability soft magnetic composite material according to claim 5, characterized in that: The pressure of the pressing molding is 1200Mpa to 2100Mpa.

10. The method for preparing a high magnetic permeability soft magnetic composite material according to claim 5, characterized in that: The magnetic field heat treatment is specifically as follows: under the protection of N2 atmosphere, firstly heating to 200-300°C at a heating rate of 5°C / min, keeping the temperature for 30-90min; then heating to 550-650°C at a heating rate of 5°C / min, keeping the temperature for 20-60min, and cooling with the furnace; After the temperature is raised to 200-300°C and kept at this temperature for 30-90 minutes, a magnetic field of 50-100 mA is continuously applied until the end.

Citation Information

Cited By

  • Soft magnetic composite material, preparation method of soft magnetic composite material, preparation method of inductor and inductor

    CN120690535A

  • Soft magnetic composite, method for manufacturing soft magnetic composite, method for manufacturing inductor, and inductor

    CN120690535B