Preparation method of semiconductor structure
Through the self-alignment double or quadruple patterning process, the multi-layer mask pattern layer is formed and etched layer by layer, the problem of pattern uniformity and consistency in semiconductor structures is solved, the process is simplified and the cost is reduced.
Patent Information
- Application Number
- CN202310454221.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-01
AI Technical Summary
In the preparation process of semiconductor structures, especially when forming patterns on chips, it is difficult to control the uniformity and consistency of patterns, and the process is complex and the cost is high.
A self-aligned double or quadruple patterning process is used to form a multi-layer mask pattern layer and etch it layer by layer. The opening pattern of the array region is defined through the third mask pattern layer to ensure pattern uniformity and consistency in the array region. The process of trimming edge parts multiple times is omitted.
The pattern uniformity and consistency control in the array area is achieved, the process flow is simplified, the cost is reduced, and complex operations of multiple trimming edges are avoided.
Smart Images

Figure CN118888439A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of semiconductor preparation, and in particular to a method for preparing a semiconductor structure. Background Art
[0002] As semiconductor technology continues to mature, the requirements for high density and large capacity of semiconductor memory chips are getting higher and higher. In the process of preparing semiconductor structures, the patterns are numerous and dense, and the precision requirements are also increasing. When forming patterns on the chip, the uniformity and consistency of the patterns are becoming more and more critical and more and more difficult to control. The process is complex and the cost is high.
[0003] The above information disclosed in this background section is only for enhancement of understanding of the background of the present disclosure and therefore it may include information that does not constitute the relevant technology that is already known to one of ordinary skill in the art. Summary of the invention
[0004] The embodiments of the present disclosure provide a method for preparing a semiconductor structure, which can ensure the uniformity and consistency of the pattern at the edge of the array area, and at the same time obtain a peripheral area without a pattern.
[0005] An embodiment of the present disclosure provides a method for preparing a semiconductor structure, comprising: providing a substrate, the substrate comprising a chip area and a cutting road area surrounding the chip area; forming a first mask pattern layer on the substrate, wherein the first mask pattern layer comprises a plurality of target annular patterns, each of the target annular patterns comprises two target long strip patterns located in the chip area and extending along a first direction, and the target long strip patterns in the plurality of target annular patterns are arranged at intervals in the chip area; forming a second mask pattern layer on the first mask pattern layer, wherein the second mask pattern layer comprises a plurality of target hole patterns arranged in an array; forming a third mask pattern layer on the second mask pattern layer, wherein the third mask pattern layer comprises an opening pattern for defining an array area in the chip area; using the third mask pattern layer, the second mask pattern layer and the first mask pattern layer as masks, etching layer by layer to transfer the target hole patterns and the target long strip patterns in the array area to the substrate to form a plurality of first active areas arranged in an array.
[0006] In some embodiments of the present disclosure, the plurality of target ring-shaped patterns are arranged at intervals in the chip area.
[0007] In some embodiments of the present disclosure, forming the first mask pattern layer on the substrate includes: forming the first mask pattern layer using a self-aligned double patterning process.
[0008] In some embodiments of the present disclosure, the first mask pattern layer is formed by a self-aligned double patterning process, including: forming a first mask layer on the substrate; forming a fourth mask pattern layer on the first mask layer, wherein the fourth mask pattern layer includes a plurality of long strip patterns located in the chip area and extending along the first direction; forming a first pad layer on the side walls of the plurality of long strip patterns in the fourth mask pattern layer, wherein the first pad layer includes the plurality of target ring patterns; removing the fourth mask pattern layer; etching the first mask layer using the first pad layer as a mask to transfer the plurality of target ring patterns into the first mask layer to form the first mask pattern layer.
[0009] In some embodiments of the present disclosure, the multiple target ring patterns are formed into multiple target ring pattern groups in the chip area, and the multiple target ring pattern groups are arranged at intervals in the chip area. Each target ring pattern group includes a first target ring pattern and a second target ring pattern, and the first target ring pattern is located within the second target ring pattern.
[0010] In some embodiments of the present disclosure, forming the first mask pattern layer on the substrate includes: forming the first mask pattern layer using a self-aligned quadruple patterning process.
[0011] In some embodiments of the present disclosure, a self-aligned quadruple patterning process is used to form the first mask pattern layer, including: forming a first mask layer and a fifth mask layer stacked in sequence on the substrate; forming a sixth mask pattern layer on the fifth mask layer, wherein the sixth mask pattern layer includes a plurality of long strip patterns located in the chip area and extending along the first direction; forming a second pad layer on the side walls of the plurality of long strip patterns of the sixth mask pattern layer, wherein the second pad layer includes a plurality of first ring patterns; removing the sixth mask pattern layer; etching the fifth mask layer using the second pad layer as a mask to transfer the plurality of first ring patterns into the fifth mask layer to form the fifth mask pattern layer; forming a third pad layer on the side walls of the plurality of first ring patterns of the fifth mask pattern layer, wherein the third pad layer includes the plurality of target ring patterns; removing the fifth mask pattern layer; etching the first mask layer using the third pad layer as a mask to transfer the plurality of target ring patterns into the first mask layer to form the first mask pattern layer.
[0012] In some embodiments of the present disclosure, the second mask pattern layer is formed on the first mask pattern layer, including: forming a second mask layer on the first mask pattern layer; forming a seventh mask pattern layer on the second mask layer, wherein the seventh mask pattern layer includes a plurality of second annular patterns arranged at intervals, each of the second annular patterns including two long strip patterns located in the chip area and extending along a second direction, and the second direction intersects with the first direction; forming an eighth mask pattern layer on the seventh mask pattern layer, wherein the eighth mask pattern layer includes a plurality of third annular patterns arranged at intervals, each of the third annular patterns including two long strip patterns located in the chip area and extending along a third direction, and the third direction intersects with both the first direction and the second direction; using the eighth mask pattern layer and the seventh mask pattern layer as masks, etching layer by layer to transfer the third annular patterns and the second annular patterns to the second mask layer to form the second mask pattern layer.
[0013] In some embodiments of the present disclosure, the method further includes: conformally forming a sacrificial layer on the second mask pattern layer to reduce the aperture of the target hole pattern.
[0014] In some embodiments of the present disclosure, the seventh mask pattern layer is formed by a self-aligned double patterning process, and the eighth mask pattern layer is formed by a self-aligned double patterning process.
[0015] In some embodiments of the present disclosure, the chip area also includes a peripheral area surrounding the array area, and the method further includes: after forming the multiple first active areas, etching the substrate in the peripheral area to form a plurality of second active areas arranged in an array.
[0016] It can be seen from the above technical solutions that the method for preparing the semiconductor structure of the embodiment of the present disclosure has at least one of the following advantages and positive effects:
[0017] In the disclosed embodiment, a stacked first mask pattern layer, a second mask pattern layer, and a third mask pattern layer are formed on a substrate, and are etched layer by layer to form a plurality of first active regions arranged in an array. Since the third mask pattern layer includes an opening pattern for defining an array region in a chip region, the plurality of first active regions arranged in an array are formed only in the array region. Compared with forming a pattern of the first active region only on a mask layer in the array region and its adjacent regions, the process of trimming the edge portion in the adjacent region multiple times is omitted, and a uniform first active region is formed on the substrate located in the array region, and the uniformity and consistency of the pattern in the edge portion of the array region can be easily controlled, making the process simpler and saving costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The above and other features and advantages of the present disclosure will become more apparent by describing in detail example embodiments thereof with reference to the attached drawings.
[0019] Figure 1 A flow chart showing a method for preparing a semiconductor structure for some embodiments of the present disclosure;
[0020] Figure 2 A schematic top view of a substrate according to some embodiments of the present disclosure;
[0021] Figure 3 A schematic top view of a substrate of a chip region according to some embodiments of the present disclosure;
[0022] Figure 4 for Figure 3 sectional views of the substrate along EE and FF respectively;
[0023] Figures 5 to 9 A schematic diagram of forming a first mask pattern layer by using a self-aligned double patterning process according to some embodiments of the present disclosure;
[0024] Figures 10 to 18 A schematic diagram of forming a first mask pattern layer by using a self-aligned quadruple patterning process according to some embodiments of the present disclosure;
[0025] Figures 19 to 22 A schematic diagram of forming a seventh mask pattern layer according to some embodiments of the present disclosure;
[0026] Figure 23 to Figure 27 A schematic diagram showing forming an eighth mask pattern layer and transferring a target hole pattern into a seventh mask pattern layer according to some embodiments of the present disclosure;
[0027] Figure 28 to Figure 29 A schematic diagram of forming a second mask pattern layer having a target hole pattern with a reduced aperture according to some embodiments of the present disclosure;
[0028] Fig.30 A schematic diagram of forming a third mask pattern layer according to some embodiments of the present disclosure;
[0029] Fig.31 A schematic diagram of forming a first active region in an array region according to some embodiments of the present disclosure is shown.
[0030] Description of reference numerals:
[0031] 1. substrate; 101. chip area; 102. exposure area; 20. initial oxide layer; 2', first mask pattern layer; 2. first mask layer; 3. fourth mask layer; 3', fourth mask pattern layer; 31. first amorphous carbon layer; 32. first silicon oxynitride layer; 33. first spin-on hard mask layer; 34. second silicon oxynitride layer; 4. first photoresist layer; 5. first liner layer; 6. fifth mask layer; 6', first 5 mask pattern layer; 7, sixth mask layer; 7', sixth mask pattern layer; 8, second pad layer; 9, third pad layer; 10, second mask layer; 10', second mask pattern layer; 1001, second spin-on hard mask layer; 1002, third silicon oxynitride layer; 1003, third oxide layer; 1004, second amorphous carbon layer; 11, seventh mask layer; 11', seventh mask pattern layer; 111, polysilicon layer; 1 12. a third amorphous carbon layer; 113. a fourth silicon oxynitride layer; 12. a second photoresist layer; 13. a fourth pad layer; 14. an eighth mask layer; 141. a third spin-on hard mask layer; 142. a fifth silicon oxynitride layer; 143. a fourth spin-on hard mask layer; 144. a sixth silicon oxynitride layer; 15. a third photoresist layer; 16. a fifth pad layer; 17. a sacrificial layer; 18. a third mask pattern layer; 181. a planarization layer; 1811. a first planarization layer; 1812. a second planarization layer; 182. a blocking mask layer; D1. a first direction; D2. a second direction; D3. a third direction; S. a target annular pattern; S01. a first target annular pattern; S02. a second target annular pattern; S1. a first annular pattern; S2. a second annular pattern; S3. a third annular pattern; H. a target hole pattern; A. an array region; P. a peripheral region. DETAILED DESCRIPTION
[0032] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as limited to the embodiments set forth herein; rather, these embodiments are provided so that this disclosure will be comprehensive and complete and will fully convey the concepts of the example embodiments to those skilled in the art. The same reference numerals in the figures represent the same or similar structures, and thus their detailed description will be omitted.
[0033] In the following description of different exemplary embodiments of the present disclosure, reference is made to the accompanying drawings, which form a part of the present disclosure and in which different exemplary structures that can implement multiple aspects of the present disclosure are shown by way of example. It should be understood that other specific schemes of components, structures, exemplary devices, systems and steps can be used, and structural and functional modifications can be made without departing from the scope of the present disclosure. Moreover, although the terms "above", "between", "within", etc. can be used in this specification to describe different exemplary features and elements of the present disclosure, these terms are used herein only for convenience, such as according to the direction of the examples in the accompanying drawings. Nothing in this specification should be construed as requiring a specific three-dimensional direction of the structure to fall within the scope of the present disclosure. In addition, the terms "first", "second", etc. are used only as marks and are not numerical restrictions on their objects.
[0034] The flowcharts shown in the accompanying drawings are only exemplary and do not necessarily include all the contents and operations / steps, nor must they be executed in the order described. For example, some operations / steps can be decomposed, and some operations / steps can be combined or partially combined, so the actual execution order may change according to actual conditions.
[0035] In addition, in the description of the present disclosure, “plurality” means at least two, for example, two, three, etc., unless otherwise clearly and specifically defined.
[0036] With the continuous advancement of semiconductor technology, the requirements for high density and large capacity of semiconductor memory chips are becoming higher and higher. In the process of preparing semiconductor structures, the patterns are numerous and dense, and the requirements for precision are also increasing.
[0037] The substrate 1 of the semiconductor structure of the embodiment of the present disclosure includes a chip area 101 and a scribe line area surrounding the chip area 101. A chip is prepared in each chip area 101. The preparation method in the embodiment of the present disclosure is implemented on the substrate 1. For ease of description, only a single chip structure is used in the drawings of the specification.
[0038] refer to Figure 2 , the substrate 1 has a plurality of exposure regions 102, each of which includes a plurality of chip regions 101. In the embodiment of the present disclosure, Figure 2 As shown, taking one of the exposure areas 102 as an example, each exposure area 102 includes six chip areas 101 , and there are scribe line areas between the chip areas 101 , and other test element groups can be set in the scribe line areas.
[0039] like Figure 3As shown, the chip area 101 generally includes an array area A and a peripheral area P, and the peripheral area P surrounds the array area A. Semiconductor functional devices are generally formed in the array area A, and logic circuits are generally formed in the peripheral area P. The patterns of the array area A and the peripheral area P are different. At the edge of the array area A, that is, at the junction of the array area A and the peripheral area P, it is expected that the pattern of the edge of the array area A can be consistent with the pattern of the non-edge of the array area A to avoid affecting the electrical performance of the semiconductor structure. However, in the actual process, it is difficult to control the uniformity and consistency of the pattern of the edge. For example, in the process of forming the pattern, the pattern is first formed on the array area A and its adjacent areas, and the pattern of the edge in the adjacent area needs to be trimmed multiple times to achieve a pattern of the edge of the array area A that meets the requirements. In this way, it is increasingly difficult to control the consistency of the pattern of the edge of the array area A, the process is complicated, and the cost is increased.
[0040] Based on this, the present disclosure provides a method for preparing a semiconductor structure. Figure 1 As shown, the method includes the following steps S110 to S150.
[0041] S110 : providing a substrate 1 , wherein the substrate 1 includes a chip region 101 and a scribe line region surrounding the chip region 101 .
[0042] S120: forming a first mask pattern layer 2' on the substrate 1, wherein the first mask pattern layer 2' comprises a plurality of target ring patterns S, each target ring pattern S comprises two target long strip patterns located in the chip area 101 and extending along the first direction D1, and the target long strip patterns in the plurality of target ring patterns S are arranged at intervals in the chip area 101.
[0043] S130: forming a second mask pattern layer 10' on the first mask pattern layer 2', wherein the second mask pattern layer 10' comprises a plurality of target hole patterns H arranged in an array.
[0044] S140 : forming a third mask pattern layer 18 on the second mask pattern layer 10 ′, wherein the third mask pattern layer 18 includes an opening pattern for defining an array region A in the chip region 101 .
[0045] S150: using the third mask pattern layer 18, the second mask pattern layer 10' and the first mask pattern layer 2' as masks, etching layer by layer, transferring the target hole pattern H and the target strip pattern in the array area A to the substrate 1, so as to form a plurality of first active areas arranged in an array.
[0046] In the embodiment of the present disclosure, a stacked first mask pattern layer 2', a second mask pattern layer 10' and a third mask pattern layer 18 are formed on the substrate 1, and are etched layer by layer to form a plurality of first active regions arranged in an array. Since the third mask pattern layer 18 includes an opening pattern for defining the array region A in the chip region 101, the plurality of first active regions arranged in an array are only formed in the array region A. Compared with forming the pattern of the first active region only on the mask layer of the array region A and its adjacent regions, the process of trimming the edge portion in the adjacent region multiple times is omitted, and a uniform first active region is formed on the substrate 1 located in the array region A, and the uniformity and consistency of the pattern located in the edge portion of the array region A can be easily controlled, making the process simpler and saving costs.
[0047] The following is a detailed description of the method for preparing the semiconductor structure according to the embodiment of the present disclosure.
[0048] S110 : providing a substrate 1 , wherein the substrate 1 includes a chip region 101 and a scribe line region surrounding the chip region 101 .
[0049] The substrate 1 may be a wafer. In some embodiments, the material of the substrate 1 may be silicon, silicon carbide, silicon on insulator, silicon on insulator, silicon germanium on insulator, silicon germanium on insulator, or germanium on insulator, etc. The substrate 1 may also be implanted with certain doping particles to change electrical parameters according to design requirements.
[0050] S120: forming a first mask pattern layer 2' on the substrate 1, wherein the first mask pattern layer 2' comprises a plurality of target ring patterns S, each target ring pattern S comprises two target long strip patterns located in the chip area 101 and extending along the first direction D1, and the target long strip patterns in the plurality of target ring patterns S are arranged at intervals in the chip area 101.
[0051] In some embodiments, a plurality of target ring-shaped patterns S are arranged at intervals in the chip region 101 .
[0052] In some embodiments, forming the first mask pattern layer 2 ′ on the substrate 1 includes: forming the first mask pattern layer 2 ′ using a self-aligned double patterning (SADP) process.
[0053] For example, in some embodiments, the first mask pattern layer 2 ′ is formed by a self-aligned double patterning process, including the following steps A1 to A5 .
[0054] A1: forming a first mask layer 2 on a substrate 1 .
[0055] like Figure 5As shown, a deposition process may be used to form a first mask layer 2 on a substrate 1. The first mask layer 2 refers to a first mask pattern layer 2' where no target annular pattern S is formed.
[0056] In some embodiments, the deposition process may be any one of a chemical vapor deposition process, a physical vapor deposition process, and an atomic layer deposition process, which is not particularly limited herein.
[0057] In some embodiments, the first mask layer 2 may include a polysilicon layer 111 , that is, the first mask layer 2 may be a hard mask layer.
[0058] Continue to refer Figure 5 In some embodiments, before forming the first mask layer 2, an initial oxide layer 20 may be formed on the semiconductor substrate 1. Then, the first mask layer 2 is formed on the initial oxide layer 20. In this way, when etching the first mask layer 2 in the subsequent process, the initial oxide layer 20 may be used as an etching stop layer to avoid over-etching and damage to the substrate 1.
[0059] A2: forming a fourth mask pattern layer 3 ′ on the first mask layer 2 , wherein the fourth mask pattern layer 3 ′ includes a plurality of long strip patterns located in the chip region 101 and extending along the first direction D1 .
[0060] For example, Figure 5 As shown, a fourth mask layer 3 may be formed on the first mask layer 2 by a deposition process. The fourth mask layer 3 may include a first spin-on hard mask layer 33 and a second silicon oxynitride layer 34 sequentially stacked on the first mask layer 2.
[0061] A first photoresist layer 4 is formed on the fourth mask layer 3 . The first photoresist layer 4 has a first exposure pattern. The first exposure pattern is formed by exposing and developing the first photoresist layer 4 , and the first exposure pattern includes a plurality of long strip patterns extending along the first direction D1 .
[0062] like Figure 6 As shown, the first exposure pattern of the first photoresist layer 4 is transferred to the first spin-coated hard mask layer 33 and the second silicon oxynitride layer 34, that is, the first exposure pattern is transferred to the fourth mask layer 3, so that the fourth mask layer 3 has a plurality of long strip patterns to form a fourth mask pattern layer 3'. The long strip patterns extend along the first direction D1 in the chip region 101.
[0063] A3: forming a first liner layer 5 on the sidewalls of the plurality of long strip patterns of the fourth mask pattern layer 3 ′, wherein the first liner layer 5 includes a plurality of target ring patterns S.
[0064] Continue to refer Figure 6The first liner layer 5 can be formed on the fourth mask pattern layer 3' by a deposition process. The first liner layer 5 is formed on the surface of the second silicon oxynitride layer 34 of the fourth mask pattern layer 3' and the top surface of the first mask layer 2 under the fourth mask pattern layer 3'.
[0065] The first liner layer 5 located on the top surface of the second silicon oxynitride layer 34 and the surface of the first mask layer 2 is removed by an etching process, and the first liner layer 5 located on the sidewall of the fourth mask pattern layer 3 ′ is retained.
[0066] A4: removing the fourth mask pattern layer 3 ′.
[0067] like Figure 7 and Figure 8 As shown, Figure 7 for Figure 8 In the top view of the semiconductor structure, the fourth mask pattern layer 3 ′ located in the target annular pattern S can be removed by an etching process, and only the first liner layer 5 is retained. The first liner layer 5 includes a plurality of target annular patterns S.
[0068] A5: using the first liner layer 5 as a mask, etching the first mask layer 2, transferring a plurality of target annular patterns S into the first mask layer 2, so as to form a first mask pattern layer 2'.
[0069] like Fig. 9 As shown, the first liner layer 5 is used as a mask layer, and etching is performed downward to the first mask layer 2 to transfer the multiple target annular patterns S of the first liner layer 5 into the first mask layer 2, so that the first mask layer 2 is formed into a first mask pattern layer 2' having multiple target annular patterns S.
[0070] In some embodiments, multiple target ring patterns S are formed into multiple target ring pattern groups in the chip area 101, and the multiple target ring pattern groups are arranged at intervals in the chip area 101. Each target ring pattern group includes a first target ring pattern S01 and a second target ring pattern S02, and the first target ring pattern S01 is located within the second target ring pattern S02.
[0071] In some embodiments, forming the first mask pattern layer 2 ′ on the substrate 1 may include: forming the first mask pattern layer 2 ′ using a self-aligned quadruplicity patterning (SAQP) process.
[0072] In some embodiments, the first mask pattern layer 2 ′ is formed by a self-aligned quadruple patterning process, including the following steps B1 - B8 .
[0073] B1: A first mask layer 2 and a fifth mask layer 6 which are stacked in sequence are formed on a substrate 1 .
[0074] like Fig.10 As shown, a deposition process can be used to form a first mask layer 2 and a fifth mask layer 6 on the substrate 1. The material of the first mask layer 2 is the same as that of the first mask layer 2 in the above embodiment, which will not be described again.
[0075] The fifth mask layer 6 includes a first amorphous carbon layer 31 and a first silicon oxynitride layer 32 which are sequentially stacked.
[0076] In some embodiments, Fig.10 As shown, before forming the first mask layer 2 , an initial oxide layer 20 may be deposited on the substrate 1 .
[0077] B2: forming a sixth mask pattern layer 7 ′ on the fifth mask layer 6 , wherein the sixth mask pattern layer 7 ′ includes a plurality of long strip patterns located in the chip region 101 and extending along the first direction D1 .
[0078] For example, Fig.10 As shown, a sixth mask layer 7 and a first photoresist layer 4 are sequentially stacked on the fifth mask layer 6 by a deposition process. The sixth mask layer 7 includes a first spin-on hard mask layer 33 and a second silicon oxynitride layer 34 sequentially stacked on the fifth mask layer 6. The first photoresist layer 4 has a plurality of long strip patterns extending along a first direction D1. Fig.11 As shown, the plurality of strip patterns of the first photoresist layer 4 are transferred to the first spin-on hard mask layer 33 and the second silicon oxynitride layer 34. Fig.11 As shown, the plurality of long strip patterns are transferred to the sixth mask layer 7, so that the sixth mask layer 7 is formed into a sixth mask pattern layer 7' having a plurality of long strip patterns extending along the first direction D1.
[0079] B3: forming a second liner layer 8 on the sidewalls of the plurality of long strip patterns of the sixth mask pattern layer 7 ′, wherein the second liner layer 8 includes a plurality of first ring patterns S1 .
[0080] like Fig.11 As shown, a second liner layer 8 can be formed by a deposition process on the outer surface of the plurality of long strip patterns of the sixth mask pattern layer 7' and on the surface of the first silicon oxynitride layer 32 of the fifth mask layer 6. Then, an etching process can be used to remove the second liner layer 8 located on the top surface of the long strip patterns and on the surface of the first silicon oxynitride layer 32, so that the second liner layer 8 includes a plurality of first ring patterns S1.
[0081] B4: removing the sixth mask pattern layer 7 ′.
[0082] like Fig.12As shown, the first spin-on hard mask layer 33 and the second silicon oxynitride layer 34 are removed respectively by an etching process, that is, the sixth mask pattern layer 7 ′ is removed, and only the second liner layer 8 having the first ring pattern S1 remains.
[0083] B5: using the second liner layer 8 as a mask, etching the fifth mask layer 6, transferring the plurality of first ring patterns S1 into the fifth mask layer 6, so as to form a fifth mask pattern layer 6'.
[0084] For example, Fig.13 As shown, the first amorphous carbon layer 31 and the first silicon oxynitride layer 32 of the fifth mask layer 6 may be etched respectively by an etching process to transfer the first target ring-shaped pattern S01 into the fifth mask layer 6 .
[0085] B6: forming a third liner layer 9 on the sidewalls of the plurality of first target ring-shaped patterns S01 of the fifth mask pattern layer 6 ′, wherein the third liner layer 9 includes a plurality of second target ring-shaped patterns S02 .
[0086] like Fig.14 As shown, a third liner layer 9 can be formed on the surface of the fifth mask pattern layer 6' and the surface of the first mask layer 2 by a deposition process, and then the third liner layer 9 located on the top surface of the fifth mask pattern layer 6' and the third liner layer 9 located on the surface of the first mask layer 2 can be removed by an etching process, so that the third liner layer 9 has a target annular pattern S. The target annular pattern S includes a first target annular pattern S01 and a second target annular pattern S02, and the first target annular pattern S01 is located in the second target annular pattern S02. Among them, the second target annular pattern S02 is a pattern of the third liner layer 9 surrounding the fifth mask pattern layer 6' having the first target annular pattern S01.
[0087] B7: removing the fifth mask pattern layer 6 ′.
[0088] like Fig.15 and Fig.16 As shown, the first amorphous carbon layer 31 and the first silicon oxynitride layer 32 can be removed by an etching process, that is, the fifth mask pattern layer 6' is removed, and the third liner layer 9 having the target ring pattern S remains. Fig.15 As shown, the first target annular pattern S01 in the target annular pattern S is located inside the second target annular pattern S02.
[0089] B8: Using the third liner layer 9 as a mask, the first mask layer 2 is etched to transfer a plurality of target annular patterns S into the first mask layer 2 to form a first mask pattern layer 2'.
[0090] like Fig.17 and Fig.18As shown, the first mask layer 2 is etched using the third liner layer 9 as a mask, and the target annular pattern S having the first target annular pattern S01 and the second target annular pattern S02 is transferred to the first mask layer 2, so that the first mask layer 2 is formed into a first mask pattern layer 2' having the target annular pattern S.
[0091] S130: forming a second mask pattern layer 10' on the first mask pattern layer 2', wherein the second mask pattern layer 10' comprises a plurality of target hole patterns H arranged in an array.
[0092] For example, S130 may include the following steps C1 to C4.
[0093] C1: forming a second mask layer 10 on the first mask pattern layer 2 ′.
[0094] like Fig.19 As shown, a second mask layer 10 may be formed on the first mask pattern layer 2' by a deposition process. The second mask layer 10 may include a second spin-on hard mask layer 1001, a third silicon oxynitride layer 1002, a third oxide layer 1003, and a second amorphous carbon layer 1004 stacked in sequence.
[0095] C2: forming a seventh mask pattern layer 11' on the second mask layer 10, wherein the seventh mask pattern layer 11' comprises a plurality of second annular patterns S2 arranged at intervals, each second annular pattern S2 comprises two long strip patterns located in the chip region 101 and extending along a second direction D2, and the second direction D2 intersects with the first direction D1.
[0096] Continue to refer Fig.19 , a seventh mask layer 11 is formed on the second mask layer 10. In some embodiments, the seventh mask layer 11 includes a polysilicon layer 111, a third amorphous carbon layer 112, and a fourth silicon oxynitride layer 113 sequentially stacked on the second mask layer 10. The seventh mask pattern layer 11' may be formed by a self-aligned double patterning process.
[0097] For example, Fig.19 As shown, a second photoresist layer 12 is formed on the surface of the fourth silicon oxynitride layer 113 in the seventh mask layer 11. The second photoresist layer 12 has a strip-shaped pattern extending along the second direction D2. The strip-shaped pattern of the second photoresist layer 12 is transferred to the seventh mask layer 11 by an etching process. Fig. 20 As shown, the strip-shaped pattern of the second photoresist layer 12 is transferred to the third amorphous carbon layer 112 in the seventh mask layer 11, and the fourth silicon oxynitride layer 113 is removed.
[0098] Continue to refer Fig. 20, a fourth liner layer 13 is formed on the seventh mask layer 11. For example, the fourth liner layer 13 is formed on the surface of the third amorphous carbon layer 112 and the surface of the polysilicon layer 111. The fourth liner layer 13 located on the top surface of the third amorphous carbon layer 112 and the surface of the polysilicon layer 111 is removed by an etching process, and the fourth liner layer 13 located on the sidewall of the third amorphous carbon layer 112 is retained, and the third amorphous carbon layer 112 is removed by an etching process, and only the fourth liner layer 13 located on the sidewall of the third amorphous carbon layer 112 is retained, so that the fourth liner layer 13 has a second ring-shaped pattern S2.
[0099] The second annular pattern S2 is transferred to the seventh mask layer 11 by an etching process to form a seventh mask pattern layer 11' having the second annular pattern S2. Fig.21 and Fig. 22 As shown, the polysilicon layer 111 finally has a second ring-shaped pattern S2 , that is, the polysilicon layer 111 is formed into a seventh mask pattern layer 11 ′.
[0100] C3: An eighth mask pattern layer is formed on the seventh mask pattern layer 11', wherein the eighth mask pattern layer includes a plurality of third annular patterns S3 arranged at intervals, each of the third annular patterns S3 includes two long strip patterns located in the chip region 101 and extending along a third direction D3, and the third direction D3 intersects both the first direction D1 and the second direction D2. The eighth mask pattern layer may be formed by a self-aligned double patterning process.
[0101] like Fig.23 As shown, an eighth mask layer 14 may be formed on the seventh mask pattern layer 11' by a deposition process. In some embodiments, the eighth mask layer 14 may include a third spin-on hard mask layer 141, a fifth silicon oxynitride layer 142, a fourth spin-on hard mask layer 143, and a sixth silicon oxynitride layer 144 stacked sequentially on the seventh mask pattern layer 11'. The eighth mask pattern layer may be formed by a self-aligned double patterning process.
[0102] For example, a third photoresist layer 15 is formed on the surface of the sixth silicon oxynitride layer 144 in the eighth mask layer 14, and the third photoresist layer 15 has a strip-shaped pattern extending along a third direction D3, wherein the third direction D3 intersects with the first direction D1 and the second direction D2 respectively. The strip-shaped pattern of the third photoresist layer 15 is transferred to the eighth mask layer 14 by an etching process. Fig.24 As shown, the stripe pattern of the third photoresist layer 15 is transferred to the sixth silicon oxynitride layer 144 and the fourth spin-on hard mask layer 143 in the eighth mask layer 14 .
[0103] Continue to refer Fig.24, a fifth liner layer 16 is formed on the eighth mask layer 14. For example, the fifth liner layer 16 is formed on the sixth silicon oxynitride layer 144, the surface of the fourth spin-coated hard mask layer 143, and the surface of the fifth silicon oxynitride layer 142, and the fifth liner layer 16 located on the top surface of the sixth silicon oxynitride layer 144 and the surface of the fifth silicon oxynitride layer 142 is removed by an etching process, and the fifth liner layer 16 located on the sidewalls of the sixth silicon oxynitride layer 144 and the fourth spin-coated hard mask layer 143 is retained, and then the sixth silicon oxynitride layer 144 and the fourth spin-coated hard mask layer 143 are removed by an etching process, such as Fig.25 and Fig.26 The third annular pattern S3 is transferred to the fifth silicon oxynitride layer 142 and the third spin-on hard mask layer 141 in the eighth mask layer 14 by an etching process, so that the eighth mask layer 14 is formed into an eighth mask pattern layer having the third annular pattern S3.
[0104] C4: using the eighth mask pattern layer and the seventh mask pattern layer 11 ′ as masks, etching layer by layer to transfer the third annular pattern S3 and the second annular pattern S2 to the second mask layer 10 to form a second mask pattern layer 10 ′.
[0105] like Fig. 27 As shown, the eighth mask pattern layer is used as a mask and the third annular pattern S3 of the eighth mask pattern layer is transferred to the seventh mask pattern layer 11 ′ by an etching process, so that the pattern of the seventh mask pattern layer 11 ′ is formed into a target hole pattern H.
[0106] Using the seventh mask pattern layer 11' as a mask, etching downwards, such as Fig.28 As shown, the pattern of the seventh mask pattern layer 11' is transferred to the second mask layer 10, so that the second mask layer 10 is formed into a second mask pattern layer 10' having a target hole pattern H. For example, Fig.28 As shown, the target hole pattern H is transferred into the third oxide layer 1003 of the second mask layer 10 .
[0107] In some embodiments, Fig.28 As shown, a sacrificial layer 17 is conformally formed on the second mask pattern layer 10 ′, so that the aperture of the target hole pattern H is reduced.
[0108] For example, Fig.28 As shown, a sacrificial layer 17 can be conformally formed on the second mask pattern layer 10' by a deposition process, that is, the sacrificial layer 17 is formed on the surface of the third oxide layer 1003 and the surface of the third silicon oxynitride layer 1002. Since the sacrificial layer 17 is attached to the inner wall of the target hole pattern H of the second mask pattern layer 10', the aperture of the target hole pattern H can be reduced to meet the size requirements.
[0109] Afterwards, the sacrificial layer 17 located on the surface of the third silicon oxynitride layer 1002 is removed, so that the sacrificial layer 17 has a target hole pattern H with a reduced aperture. Fig.29 As shown, the sacrificial layer 17 is used as a mask to at least etch the third silicon oxynitride layer 1002 in the second mask pattern layer 10 ′, so that the second mask pattern layer 10 ′ has a target hole pattern H with a reduced aperture.
[0110] In some embodiments, the material of the sacrificial layer 17 may be silicon oxide or silicon oxynitride, which is not particularly limited herein.
[0111] S140 : forming a third mask pattern layer 18 on the second mask pattern layer 10 ′, wherein the third mask pattern layer 18 includes an opening pattern for defining an array region A in the chip region 101 .
[0112] like Fig.30 As shown, a third mask pattern layer 18 may be formed on the second mask pattern layer 10 ′ by a deposition process. The third mask pattern layer 18 includes a planarization layer 181 formed in the chip region 101 and a blocking mask layer 182 formed only in the peripheral region P.
[0113] For example, a first planarization layer 1811 is formed in the chip region 101 , and a second planarization layer 1812 is formed on the first planarization layer 1811 .
[0114] Since the second mask pattern layer 10' has a target hole pattern H, in order to achieve the planarization effect of the planarization layer 181, the planarization layer 181 can be set as two layers, the first planarization layer 1811 can planarize the target aperture pattern in the second mask pattern layer 10', so that the second mask pattern layer is initially planarized, and the second planarization layer 1812 is set on the first planarization layer 1811, which can further planarize the first planarization layer 1811. The purpose of setting the planarization layer 181 is to make the blocking mask layer 182 formed on the planarization layer 181 in the peripheral area P in the subsequent process more regular and accurate, and further ensure the consistency of the pattern in the boundary area of the array area A.
[0115] In some embodiments, the first planarization layer 1811 may be a spin-coated layer, and the second planarization layer 1812 may be a silicon oxynitride layer.
[0116] The process of forming the spin coating layer is to apply a film-forming liquid to the first mask pattern layer 2', and then rotate the substrate 1 at a high speed. The film-forming liquid diffuses into the first mask pattern layer 2' and its edge under the action of centrifugal force. The film-forming liquid can be evenly applied to the first mask pattern layer 2' by using the centrifugal force. The spin coating layer can be a spin-on hard mask (SpinOn Hard Mask, SOH). The spin coating process can be carried out at a low temperature to avoid damage to other film layers caused by high temperature, and a uniform spin coating layer can be formed.
[0117] After the spin-coated layer is formed, the spin-coated layer has a flat surface, and then a silicon oxynitride layer can be formed on the surface of the spin-coated layer by a deposition process to form a more uniform and flat film layer.
[0118] S150: Using the third mask pattern layer 18, the second mask pattern layer 10' and the first mask pattern layer 2' as masks, etching layer by layer, transferring the target hole pattern H and the target strip pattern in the array area A to the substrate 1, so as to form a plurality of first active areas arranged in an array. Fig.31 As shown, after removing the planarization layer 181 of the array area A, the peripheral area P is shielded by the planarization layer 181 and the blocking mask layer 182. In the array area A, the second mask pattern layer 10' and the first mask pattern layer 2' are used as mask layers to etch layer by layer to transfer the target hole pattern H and the target long strip pattern in the array area A to the substrate 1 to form a plurality of first active areas arranged in an array.
[0119] The planarization layer 181 and the blocking mask layer 182 located in the peripheral region P are removed, so that no pattern is formed in the peripheral region P.
[0120] In some embodiments, the preparation method further includes: after forming the plurality of first active regions, etching the substrate 1 in the peripheral region P to form a plurality of second active regions arranged in an array.
[0121] For example, a pattern having a second active area may be formed in the chip area 101 , the array area A may be shielded, and only the substrate 1 in the peripheral area P may be etched, so that a plurality of second active areas arranged in an array may be formed in the peripheral area P.
[0122] It can be understood that, in the embodiments of the present disclosure, various patterns provided to form the first active region are distributed in the entire chip area, rather than only in the array area and its adjacent areas.
[0123] In summary, in the embodiment of the present disclosure, a stacked first mask pattern layer 2', a second mask pattern layer 10' and a third mask pattern layer are formed on the substrate 1, and are etched layer by layer to form a plurality of first active regions arranged in an array. Since the third mask pattern layer 18 includes an opening pattern for defining the array region A in the chip region 101, the plurality of first active regions arranged in an array are only formed in the array region A. Compared with forming the pattern of the first active region only on the mask layer of the array region A and its adjacent regions, the process of trimming the edge portion in the adjacent region multiple times is omitted, and a uniform first active region is formed on the substrate 1 located in the array region A, and the uniformity and consistency of the pattern located in the edge portion of the array region A can be easily controlled, making the process simpler and saving costs.
[0124] The present disclosure also provides a semiconductor structure, which can be prepared by the preparation method in any of the above embodiments. The semiconductor structure includes a substrate 1, the substrate 1 includes an array region A and a peripheral region P surrounding the array region A, and the substrate 1 located in the array region A has a uniform pattern of a first active region.
[0125] The semiconductor structure prepared by the preparation method of the embodiment of the present disclosure has a uniform pattern at the edge portion of the array area A of the substrate 1, which improves the electrical performance of the semiconductor structure. For the specific content of the preparation method, please refer to the description of any of the above embodiments, which will not be repeated here.
[0126] The semiconductor structure may further include a functional device, such as a transistor, disposed in the first active region of the array region A to form a buried transistor.
[0127] In summary, the pattern of the array region of the semiconductor structure of the embodiment of the present disclosure is uniform and consistent, which can improve the electrical performance and precision requirements of the semiconductor structure.
[0128] It should be understood that the present disclosure does not limit its application to the detailed structure and arrangement of the components proposed in this specification. The present disclosure can have other embodiments and can be implemented and executed in a variety of ways. The aforementioned variations and modifications fall within the scope of the present disclosure. It should be understood that the present disclosure disclosed and defined in this specification extends to all alternative combinations of two or more individual features mentioned or evident in the text and / or the drawings. All these different combinations constitute multiple alternative aspects of the present disclosure. The embodiments described in this specification illustrate the best mode known for implementing the present disclosure and will enable those skilled in the art to adopt the present disclosure.
Claims
1. A method for preparing a semiconductor structure, characterized in that: include: Providing a substrate, the substrate comprising a chip area and a scribe line area surrounding the chip area; Forming a first mask pattern layer on the substrate, wherein the first mask pattern layer includes a plurality of target annular patterns, each of the target annular patterns includes two target long strip patterns located in the chip region and extending along a first direction, and the target long strip patterns in the plurality of target annular patterns are arranged at intervals in the chip region; forming a second mask pattern layer on the first mask pattern layer, wherein the second mask pattern layer comprises a plurality of target hole patterns arranged in an array; forming a third mask pattern layer on the second mask pattern layer, wherein the third mask pattern layer includes an opening pattern for defining an array region in the chip region; Using the third mask pattern layer, the second mask pattern layer and the first mask pattern layer as masks, etching is performed layer by layer to transfer the target hole pattern and the target strip pattern in the array area into the substrate to form a plurality of first active areas arranged in an array.
2. The method according to claim 1, characterized in that The plurality of target annular patterns are arranged at intervals in the chip region.
3. The method according to claim 2, characterized in that Forming the first mask pattern layer on the substrate includes: The first mask pattern layer is formed by a self-aligned double patterning process.
4. The method according to claim 3, characterized in that The first mask pattern layer is formed by a self-aligned double patterning process, comprising: forming a first mask layer on the substrate; forming a fourth mask pattern layer on the first mask layer, wherein the fourth mask pattern layer includes a plurality of long strip patterns located in the chip region and extending along the first direction; forming a first liner layer on the sidewalls of the plurality of long strip patterns of the fourth mask pattern layer, wherein the first liner layer includes the plurality of target ring patterns; removing the fourth mask pattern layer; The first liner layer is used as a mask to etch the first mask layer, and the plurality of target annular patterns are transferred into the first mask layer to form the first mask pattern layer.
5. The method according to claim 1, characterized in that The multiple target annular patterns are formed into multiple target annular pattern groups in the chip area. The multiple target annular pattern groups are arranged at intervals in the chip area. Each target annular pattern group includes a first target annular pattern and a second target annular pattern. The first target annular pattern is located within the second target annular pattern.
6. The method according to claim 5, characterized in that Forming the first mask pattern layer on the substrate includes: The first mask pattern layer is formed by a self-aligned quadruple patterning process.
7. The method according to claim 6, characterized in that The first mask pattern layer is formed by a self-aligned quadruple patterning process, comprising: forming a first mask layer and a fifth mask layer stacked in sequence on the substrate; forming a sixth mask pattern layer on the fifth mask layer, wherein the sixth mask pattern layer includes a plurality of long strip patterns located in the chip region and extending along the first direction; forming a second liner layer on the sidewalls of the plurality of long strip patterns of the sixth mask pattern layer, wherein the second liner layer includes a plurality of first ring patterns; removing the sixth mask pattern layer; Using the second liner layer as a mask, etching the fifth mask layer, transferring the plurality of first ring-shaped patterns into the fifth mask layer, so as to form a fifth mask pattern layer; forming a third liner layer on sidewalls of the plurality of first ring-shaped patterns of the fifth mask pattern layer, wherein the third liner layer includes the plurality of target ring-shaped patterns; removing the fifth mask pattern layer; The first mask layer is etched using the third liner layer as a mask to transfer the plurality of target annular patterns into the first mask layer to form the first mask pattern layer.
8. The method according to any one of claims 1 to 6, characterized in that: Forming the second mask pattern layer on the first mask pattern layer includes: forming a second mask layer on the first mask pattern layer; forming a seventh mask pattern layer on the second mask layer, wherein the seventh mask pattern layer comprises a plurality of second annular patterns arranged at intervals, each of the second annular patterns comprises two long strip patterns located in the chip region and extending along a second direction, and the second direction intersects the first direction; forming an eighth mask pattern layer on the seventh mask pattern layer, wherein the eighth mask pattern layer comprises a plurality of third annular patterns arranged at intervals, each of the third annular patterns comprises two long strip patterns located in the chip region and extending along a third direction, and the third direction intersects both the first direction and the second direction; The eighth mask pattern layer and the seventh mask pattern layer are used as masks to perform etching layer by layer, and the third annular pattern and the second annular pattern are transferred to the second mask layer to form the second mask pattern layer.
9. The method according to claim 8, characterized in that Also includes: A sacrificial layer is conformally formed on the second mask pattern layer to reduce the aperture of the target hole pattern.
10. The method according to claim 8, characterized in that The seventh mask pattern layer is formed by a self-aligned double patterning process, and the eighth mask pattern layer is formed by a self-aligned double patterning process.
11. The method according to any one of claims 1 to 6, characterized in that: The chip region also includes a peripheral region surrounding the array region, and the method further includes: After forming the plurality of first active regions, the substrate in the peripheral region is etched to form a plurality of second active regions arranged in an array.
Citation Information
Cited By
Placement method, device and equipment of semiconductor test structure and medium
CN119742301A