Ultrathin lithium metal composite negative electrode and preparation method and application thereof
By heating the low-melting point salt with lithium metal to form a composite lithium metal material and evenly scraping it on the copper foil, the problem of insufficient self-immersion between lithium metal and copper is solved, and the efficient preparation and electrochemistry of ultra-thin lithium metal negative electrodes are achieved. The performance is improved and supports uniform coating and cycle stability of thicknesses of 1μm to 20μm.
Patent Information
- Application Number
- CN202411086556.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-08
AI Technical Summary
In the prior art, the self-immersion of lithium metal and copper is insufficient, molten lithium is difficult to spread uniformly on the surface of the copper foil, and the preparation of ultra-thin lithium metal negative electrodes has problems such as insufficient mechanical strength and poor electrochemical performance.
Mix the low-melting salt with lithium metal to a molten state to form a composite lithium metal material, and uniformly scrape it on copper foil, cool it to room temperature to form an ultra-thin lithium metal composite negative electrode, using spontaneous dopants and lithium metal The reaction increases wettability and electrochemical properties.
It realizes uniform wetting and efficient coating of lithium metal on the surface of copper foil, improves the cycle stability and electrochemical performance of lithium metal negative electrode, supports fast and uniform coating of lithium metal layers with a thickness of 1μm to 20μm, simplifies the process and Reduced costs.
Smart Images

Figure CN118888698A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of lithium battery technology, and in particular to an ultra-thin lithium metal composite negative electrode and a preparation method and application thereof. Background Art
[0002] Since its introduction into the market, lithium-ion batteries have been widely used in portable electronics and electric vehicles, which has greatly changed human society. With the continuous emergence of new application scenarios and demands, the development of next-generation consumer electronics and electric vehicles urgently requires the development of new battery systems with higher energy density. Lithium metal has an ultra-high theoretical specific capacity (3680mAh g -1 ) and the lowest reduction potential (-3.04V, relative to standard hydrogen electrode) are considered the holy grail of high energy density battery anode materials. However, lithium metal has high reactivity, low strength and high viscosity. In addition, a series of problems such as low coulombic efficiency, short cycle life and internal short circuit caused by lithium dendrite growth and high reactivity to electrolytes seriously restrict the practical application of lithium metal anodes.
[0003] At present, in order to pursue cycle performance, the thickness of commercial lithium foil is generally more than 50μm. It supplements active lithium and acts as a current collector. During the battery cycle, the metal lithium will be continuously consumed, and inactivated dead lithium will be continuously generated until the end of the life of the electrode is completely powdered and loses electrical connection and can no longer serve as a current collector. However, due to the relatively low surface capacity of the positive electrode, usually only 2-4mAh cm -2 , not more than 6mAh cm -2 , the matching lithium metal only needs a thickness of about 30μm to achieve the required capacity match. And in the case of negative electrode lithium supplementation, the required thickness will be even smaller (<20μm). At present, the thickness of commercial lithium foil ranges from 50μm to 750μm, which is seriously excessive, greatly reducing the advantage of high specific capacity of lithium metal negative electrode, resulting in a serious reduction in battery energy density. However, there are still many challenges in the preparation and performance of ultra-thin lithium metal strips (<20μm). Limited by its mechanical strength, when the thickness of lithium metal is less than 50μm, it is very easy to break, and copper foil current collector is required for attachment and reinforcement. However, the natural lithium-repellent property of copper foil leads to insufficient self-wetting of lithium metal and copper, and it is difficult for molten lithium metal to spread on the surface of copper foil to achieve uniform coating. Therefore, the controllable preparation and rapid modification of ultra-thin lithium metal negative electrode are of great practical significance for improving the utilization efficiency of lithium in batteries and improving the energy density and cycle performance of full batteries.
[0004] The prior art method for preparing lithium metal negative electrodes proposes to prepare an organic transition layer as a lithium-philic layer in advance to improve the wettability of molten lithium to the substrate. However, the wettability of the organic coating to molten lithium is still insufficient, and side reactions between the organic coating and molten lithium are prone to occur at high temperatures. Under the current state of technological development, it is still difficult to achieve uniform ultra-thin lithium negative electrode preparation. Summary of the invention
[0005] The embodiments of the present application provide an ultra-thin lithium metal composite negative electrode and a preparation method and application thereof, which solve the technical problems in the prior art that the self-wetting properties of lithium metal and copper are insufficient and molten lithium is difficult to spread evenly on the surface of copper foil.
[0006] To solve the above technical problems, in the first aspect, an embodiment of the present application provides a method for preparing an ultra-thin lithium metal composite negative electrode, comprising the following steps: first, mixing a low-melting point salt and lithium metal and heating them to a molten state to react and generate a molten composite lithium metal material; then, transferring the molten composite lithium metal material to a copper foil, evenly scraping the molten composite lithium metal material, and cooling to room temperature to obtain an ultra-thin lithium metal composite negative electrode.
[0007] In some exemplary embodiments, the anion of the low melting point salt includes one or more of inorganic nitrate, chloride, nitrogen, phosphorus, fluorine, sulfur, or organic bis(fluorosulfonyl)imide, bis(trifluoromethanesulfonyl)imide, hexafluorophosphate, difluorooxalatoborate, tetrafluoroborate, difluorophosphate, bisoxalatoborate, and trifluoromethanesulfonate.
[0008] In some exemplary embodiments, the cation of the low melting point salt includes one or more of magnesium, zinc, aluminum, gallium, indium, silver, tin, bismuth, germanium, antimony, or an organic 1-ethyl-3-methylimidazolium cation, N,N-diethyl-N-methyl-N-(2-methoxyethyl)ammonium cation, and N-methyl-N-propylpyrrolidinium cation.
[0009] In some exemplary embodiments, when the low melting point salt is mixed with lithium metal and heated, a redox reaction occurs, generating an inorganic fast ion conductor and a lithium-metal alloy in the lithium metal negative electrode, thereby increasing the wettability of lithium to the copper foil.
[0010] In some exemplary embodiments, the inorganic fast ion conductor includes one or more of lithium fluoride, lithium nitride, lithium sulfide, or lithium phosphide.
[0011] In some exemplary embodiments, the thickness of the lithium metal layer of the ultra-thin lithium metal composite negative electrode is 1 μm to 20 μm.
[0012] In some exemplary embodiments, the copper foil has a thickness of 5 μm to 20 μm.
[0013] In some exemplary embodiments, the molten composite lithium metal material is uniformly coated by scraping and then cooled to room temperature by natural cooling or blowing.
[0014] In a second aspect, the embodiments of the present application further provide an ultra-thin lithium metal composite negative electrode, which is prepared using the method for preparing the ultra-thin lithium metal composite negative electrode material described in the above embodiments.
[0015] In a third aspect, the embodiments of the present application also provide an application of the ultra-thin lithium metal composite negative electrode described in the above embodiments in liquid lithium metal batteries and solid lithium metal batteries.
[0016] The technical solution provided by the embodiments of the present application has at least the following advantages:
[0017] The embodiment of the present application provides an ultra-thin lithium metal composite negative electrode and a preparation method and application thereof. The preparation method comprises the following steps: first, mixing a low-melting point salt and lithium metal and heating them to a molten state to react and generate a molten composite lithium metal material; then, transferring the molten composite lithium metal material to a copper foil, uniformly scraping the molten composite lithium metal material, and cooling to room temperature to obtain an ultra-thin lithium metal composite negative electrode.
[0018] This application aims at the technical problem that the self-wetting property of lithium metal and copper is insufficient in the prior art, and molten lithium is difficult to be uniformly spread on the surface of copper foil. On the one hand, this application uses lithium metal with high reducibility and reactivity to react quickly with low melting point salt, and the self-doping of the reaction product can greatly improve the wettability of lithium metal on the surface of copper foil; on the other hand, this application is different from the organic / inorganic modification of the copper foil surface only. The doping modification of the lithium metal main body itself supports the rapid and uniform coating of 1μm to 20μm ultra-thin and thickness controllable lithium metal layer. In addition, this application cleverly utilizes the spontaneous reaction of dopants and lithium metal to achieve efficient and synchronous chemical modification of the lithium metal negative electrode body / surface during the melting reaction process, and realizes the in-situ doping of inorganic fast ion conductor components (lithium fluoride, lithium nitride, lithium sulfide, lithium phosphide and other inorganic salts) and lithium-metal alloy components and the rapid construction of rich crystal interfaces. It is efficient and simple, with simple processes and equipment and cheap raw materials. Moreover, the preparation method of the present application is universal, and low-melting-point salts such as organic salts and inorganic salts that can react with lithium metal are all feasible. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] One or more embodiments are exemplarily described by pictures in the corresponding drawings, and these exemplifications do not constitute limitations on the embodiments. Unless otherwise stated, the pictures in the drawings do not constitute proportional limitations.
[0020] Figure 1 A schematic diagram of a process for preparing an ultra-thin lithium metal composite negative electrode provided in one embodiment of the present application;
[0021] Figure 2 This is a SEM image of a lithium metal composite layer with a thickness of 1 μm uniformly coated on a copper substrate with a thickness of 10 μm in Example 1 of the present application;
[0022] Figure 3 This is a SEM image of a lithium metal composite layer with a thickness of 2 μm uniformly coated on a copper substrate with a thickness of 10 μm in Example 2 of the present application;
[0023] Figure 4 This is a SEM image of Example 3 of the present application, in which a lithium metal composite layer with a thickness of 5 μm is uniformly coated on a copper substrate with a thickness of 10 μm;
[0024] Figure 5 This is a SEM image of Example 4 of the present application in which a lithium metal composite layer with a thickness of 8 μm is uniformly coated on a copper substrate with a thickness of 10 μm;
[0025] Figure 6 This is a SEM image of a lithium metal composite layer with a thickness of 10 μm uniformly coated on a copper substrate with a thickness of 10 μm in Example 5 of the present application;
[0026] Figure 7 This is a SEM image of Example 6 of the present application, in which a lithium metal composite layer with a thickness of 20 μm is uniformly coated on a copper substrate with a thickness of 10 μm.
[0027] Figure 8 This is a physical picture of Example 5 of the present application, in which a lithium metal composite layer with a thickness of 10 μm is uniformly coated on a copper substrate with a thickness of 10 μm;
[0028] Fig. 9 A physical picture of the unmodified lithium metal melt coating in the comparative example provided in this application;
[0029] Fig.10 This is a performance diagram of a lithium iron phosphate-based full battery of a 10 μm lithium metal composite layer sample formed on a 10 μm thick copper substrate in Example 5 of the present application. DETAILED DESCRIPTION
[0030] As can be seen from the background technology, the preparation method of lithium metal negative electrode in the prior art has the technical problems that the self-wetting of lithium metal and copper is insufficient and the molten lithium is difficult to spread evenly on the surface of copper foil.
[0031] A related technology proposes to use at least one of lithium-philic single substances, alloys and metal inorganic compounds as raw materials, and to prepare an inorganic transition layer on a substrate in advance by magnetron sputtering, thermal evaporation or slurry coating; then melt lithium metal is coated on the surface of the inorganic transition layer to form ultra-thin metallic lithium. However, this process involves multiple steps, which is cumbersome and costly, and may cause adverse phenomena such as gas discharge, affecting the deposition quality of the modified layer. At the same time, although the evaporation and sputtering methods can directly and controllably grow certain specific lithium-philic component layers, the equipment requirements are too high, making it difficult to process on a large scale and in large quantities, and the commercial prospects are limited.
[0032] Another related technology proposes to prepare an organic transition layer as a lithium-philic layer in advance to improve the wettability of molten lithium to the substrate. However, the wettability of the organic coating to molten lithium is still insufficient, and side reactions between the organic coating and molten lithium are prone to occur at high temperatures. Under the current state of technological development, it is still difficult to achieve uniform ultra-thin lithium negative electrode preparation.
[0033] Therefore, the problems to be solved in this application are: 1. The self-wetting properties of lithium metal and copper in the prior art are insufficient, and molten lithium is difficult to spread evenly on the surface of copper foil; 2. The controllable coating and uniformity of lithium metal at various gradient thicknesses of 20μm and below; 3. Improving the uniformity and stability of lithium deposition on the lithium metal negative electrode during the cycle, and inhibiting the formation and growth of lithium dendrites.
[0034] In order to solve the above technical problems, the embodiment of the present application provides an ultra-thin lithium metal composite negative electrode and its preparation method and application, the preparation method comprising the following steps: first, mixing a low melting point salt and lithium metal and heating them to a molten state, reacting to generate a molten composite lithium metal material; then, transferring the molten composite lithium metal material to a copper foil, uniformly scraping the molten composite lithium metal material, cooling to room temperature, and obtaining an ultra-thin lithium metal composite negative electrode. The present application utilizes the spontaneous reaction of dopants and lithium metal to achieve efficient synchronous chemical modification of the lithium metal negative electrode bulk / surface during the melting reaction process, and realizes the in-situ doping of inorganic fast ion conductors (lithium fluoride, lithium nitride, lithium sulfide, lithium phosphide and other inorganic salts) components, lithium-metal alloy components, and the rapid construction of rich crystal interfaces, which is efficient and simple, with simple processes and equipment and cheap raw materials. Moreover, the preparation method of the present application is universal, and low melting point salts such as organic salts and inorganic salts that can react with lithium metal are all feasible.
[0035] The following will describe the various embodiments of the present application in detail with reference to the accompanying drawings. However, it will be appreciated by those skilled in the art that in the various embodiments of the present application, many technical details are provided in order to enable the reader to better understand the present application. However, even without these technical details and various changes and modifications based on the following embodiments, the technical solution claimed in the present application can be implemented.
[0036] See also Figure 1 The present invention provides a method for preparing an ultra-thin lithium metal composite negative electrode, comprising the following steps:
[0037] Step S1, mixing a low melting point salt and lithium metal and heating them to a molten state to react and generate a molten composite lithium metal material.
[0038] Step S2, transferring the molten composite lithium metal material to the copper foil, evenly coating the molten composite lithium metal material with a scraper, and cooling to room temperature to obtain an ultra-thin lithium metal composite negative electrode.
[0039] The preparation method of the ultra-thin lithium metal composite negative electrode provided in the present application is to heat and melt-mix lithium metal and a low-melting-point salt so that the two react rapidly in a molten state, and transfer the composite lithium metal material in a molten state after the reaction to a metal copper foil. The self-doping of the reaction product effectively improves the wettability of lithium metal on the surface of the copper foil, and supports the rapid and uniform coating of an ultra-thin lithium metal layer of 1 μm to 20 μm with controllable thickness. Secondly, the presence of inorganic fast ion conductor components, lithium-metal alloy components, and crystal interfaces in the reaction products contributes to the rapid conduction of lithium ions on the surface and bulk of lithium metal, inhibits uneven lithium deposition and the growth of lithium dendrites, effectively improves the coulombic efficiency, and improves its cycle stability. The present application has low equipment requirements, short preparation time, can achieve ultra-thin coating of lithium metal, and has high consistency in controllable thickness uniformity and good cycle stability, and is expected to contribute to the high-performance application of lithium metal batteries.
[0040] The preparation method of the ultra-thin lithium metal composite negative electrode provided in the present application is to first heat the low melting point salt and lithium metal to a molten state and fully mix them to react; then transfer the molten composite lithium metal material after the reaction to a copper foil, keep heating to maintain the molten state of the composite lithium metal material and evenly scrape the lithium metal in this state, and cool to room temperature to obtain an ultra-thin lithium metal composite negative electrode.
[0041] In some embodiments, the anion of the low melting point salt includes one or more of inorganic nitrate, chloride, nitrogen, phosphorus, fluorine, sulfur, or organic bis(fluorosulfonyl)imide, bis(trifluoromethanesulfonyl)imide, hexafluorophosphate, difluorooxalatoborate, tetrafluoroborate, difluorophosphate, bisoxalatoborate, and trifluoromethanesulfonate.
[0042] In some embodiments, the cation of the low melting point salt includes one or more of magnesium, zinc, aluminum, gallium, indium, silver, tin, bismuth, germanium, antimony, or an organic 1-ethyl-3-methylimidazolium cation, N,N-diethyl-N-methyl-N-(2-methoxyethyl)ammonium cation, and N-methyl-N-propylpyrrolidinium cation.
[0043] In some embodiments, when the low melting point salt is mixed with lithium metal and heated, a redox reaction occurs, generating an inorganic fast ion conductor and a lithium-metal alloy in the lithium metal negative electrode, thereby increasing the wettability of lithium to the copper foil.
[0044] Specifically, the present application utilizes a low-melting-point salt (molten salt) to undergo an oxidation-reduction reaction with lithium metal to generate an inorganic fast ion conductor and a lithium-metal alloy in the lithium metal negative electrode, thereby increasing the wettability of lithium to copper foil and solving the problem of non-wetting of molten lithium and substrate in the preparation process of ultra-thin lithium foil.
[0045] In some embodiments, the inorganic fast ion conductor includes one or more of lithium fluoride, lithium nitride, lithium sulfide, or lithium phosphide.
[0046] Moreover, by cleverly utilizing the spontaneous reaction between dopants and lithium metal, efficient synchronous chemical modification of the lithium metal negative electrode bulk / surface can be achieved during the melting reaction process, in-situ doping of inorganic fast ion conductor components and lithium-metal alloy components can be achieved, and rapid construction of rich crystal interfaces can be achieved, thereby achieving rapid conduction of lithium ions, inhibiting uneven deposition and dendritic growth of lithium, and improving coulombic efficiency, thereby enhancing the electrochemical performance of the lithium metal negative electrode.
[0047] The preparation method of the ultra-thin lithium metal composite negative electrode provided in the present application and the self-doping modification of lithium metal can better control the thickness of the coated lithium layer and maintain uniformity, and can prepare uniform lithium foil with various thickness gradients below 20μm.
[0048] In some embodiments, the thickness of the lithium metal layer of the ultra-thin lithium metal composite negative electrode is 1 μm to 20 μm. For example, the thickness of the lithium metal layer of the ultra-thin lithium metal composite negative electrode may be 1 μm, 2 μm, 5 μm, 8 μm, 10 μm, 15 μm or 20 μm. Preferably, the thickness of the lithium metal layer of the ultra-thin lithium metal composite negative electrode is 10 μm.
[0049] The present application utilizes the rapid reaction of highly reducible and reactive lithium metal with low melting point salt, and the self-doping of the reaction product can greatly improve the wettability of lithium metal on the surface of copper foil. Moreover, unlike the organic / inorganic modification of the copper foil surface only, the preparation method provided by the present application supports the rapid and uniform coating of an ultra-thin lithium metal layer of 1μm to 20μm with controllable thickness through the doping modification of the lithium metal body itself.
[0050] In some embodiments, the thickness of the copper foil is 5 μm to 20 μm. For example, the thickness of the copper foil is 5 μm, 10 μm, 15 μm or 20 μm. Preferably, the thickness of the copper foil is 10 μm.
[0051] In some embodiments, the molten composite lithium metal material is uniformly coated by scraping and then cooled to room temperature by natural cooling or blowing.
[0052] For example, the present application may use a variety of heating auxiliary means including: hot plate heating, infrared lamp heating, etc.
[0053] The embodiment of the present application also provides an ultra-thin lithium metal composite negative electrode, which is prepared using the preparation method of the ultra-thin lithium metal composite negative electrode material described in the above embodiment.
[0054] The present application obtains ultra-thin lithium metal composite negative electrodes of Examples 1 to 6 by uniformly coating lithium metal composite layers of different thicknesses (1 μm to 20 μm) on a copper substrate with a thickness of 10 μm. The SEM images of each example are shown in FIG. Figures 2 to 8 As shown, unmodified lithium metal is used as a comparative example (the actual figure is as shown in Fig. 9 ), and combined with the performance diagram of the lithium iron phosphate-based full battery of the 10 μm lithium metal composite layer sample formed on the copper substrate with a thickness of 10 μm in Example 5 (as shown in Fig.10 As shown), the experimental results show that when a 10 μm thick lithium metal composite layer is uniformly coated on a 10 μm thick copper substrate, the battery performance of the ultra-thin lithium metal composite negative electrode is optimal.
[0055] The embodiments of the present application also provide the application of an ultra-thin lithium metal composite negative electrode. The modified lithium metal negative electrode prepared in the present application can be used for both liquid lithium metal batteries and solid lithium metal batteries.
[0056] Based on the above technical scheme, the embodiment of the present application provides an ultra-thin lithium metal composite negative electrode and its preparation method and application. The preparation method includes the following steps: first, a low-melting point salt and lithium metal are mixed and heated to a molten state, and a molten composite lithium metal material is reacted to generate a molten composite lithium metal material; then, the molten composite lithium metal material is transferred to a copper foil, the molten composite lithium metal material is evenly scraped, and cooled to room temperature to obtain an ultra-thin lithium metal composite negative electrode.
[0057] This application aims at the technical problem that the self-wetting property of lithium metal and copper is insufficient in the prior art, and molten lithium is difficult to be uniformly spread on the surface of copper foil. On the one hand, this application uses lithium metal with high reducibility and reactivity to react quickly with low melting point salt, and the self-doping of the reaction product can greatly improve the wettability of lithium metal on the surface of copper foil; on the other hand, this application is different from the organic / inorganic modification of the copper foil surface only. The doping modification of the lithium metal main body itself supports the rapid and uniform coating of 1μm to 20μm ultra-thin and thickness controllable lithium metal layer. In addition, this application cleverly utilizes the spontaneous reaction of dopants and lithium metal to achieve efficient and synchronous chemical modification of the lithium metal negative electrode body / surface during the melting reaction process, and realizes the in-situ doping of inorganic fast ion conductor components (lithium fluoride, lithium nitride, lithium sulfide, lithium phosphide and other inorganic salts) and lithium-metal alloy components and the rapid construction of rich crystal interfaces. It is efficient and simple, with simple processes and equipment and cheap raw materials. Moreover, the present application is universal, and organic salts, inorganic salts and other low-melting-point salts that can react with lithium metal are all feasible.
[0058] Those skilled in the art can understand that the above-mentioned embodiments are specific examples for implementing the present application, and in practical applications, various changes can be made to them in form and detail without departing from the spirit and scope of the present application. Any person skilled in the art can make their own changes and modifications without departing from the spirit and scope of the present application, so the scope of protection of the present application shall be based on the scope defined in the claims.
Claims
1. A method for preparing an ultra-thin lithium metal composite negative electrode, It is characterized in that The following steps are involved: The low melting point salt and lithium metal are mixed and heated to a molten state to react and generate a molten composite lithium metal material; The molten composite lithium metal material is transferred to the copper foil, the molten composite lithium metal material is evenly scraped and cooled to room temperature to obtain an ultra-thin lithium metal composite negative electrode.
2. The method for preparing the ultra-thin lithium metal composite negative electrode according to claim 1, It is characterized in that The anion of the low melting point salt includes one or more of inorganic nitrate, chlorine, nitrogen, phosphorus, fluorine, sulfur, or organic bis(fluorosulfonyl)imide, bis(trifluoromethanesulfonyl)imide, hexafluorophosphate, difluorooxalatoborate, tetrafluoroborate, difluorophosphate, bisoxalatoborate, and trifluoromethanesulfonate.
3. The method for preparing the ultra-thin lithium metal composite negative electrode according to claim 1, It is characterized in that The cation of the low melting point salt includes one or more of magnesium, zinc, aluminum, gallium, indium, silver, tin, bismuth, germanium, antimony, or an organic 1-ethyl-3-methylimidazolium cation, N,N-diethyl-N-methyl-N-(2-methoxyethyl)ammonium cation, and N-methyl-N-propylpyrrolidinium cation.
4. The method for preparing the ultra-thin lithium metal composite negative electrode according to claim 1, It is characterized in that When the low-melting-point salt is mixed with lithium metal and heated, a redox reaction occurs, generating an inorganic fast ion conductor and a lithium-metal alloy in the lithium metal negative electrode, thereby increasing the wettability of lithium to the copper foil.
5. The method for preparing the ultra-thin lithium metal composite negative electrode according to claim 4, It is characterized in that The inorganic fast ion conductor includes one or more of lithium fluoride, lithium nitride, lithium sulfide or lithium phosphide.
6. The method for preparing the ultra-thin lithium metal composite negative electrode according to claim 1, It is characterized in that The thickness of the lithium metal layer of the ultra-thin lithium metal composite negative electrode is 1 μm to 20 μm.
7. The method for preparing the ultra-thin lithium metal composite negative electrode according to claim 1, It is characterized in that The copper foil has a thickness of 5 μm to 20 μm.
8. The method for preparing the ultra-thin lithium metal composite negative electrode material according to claim 1, It is characterized in that The molten composite lithium metal material is evenly coated and cooled to room temperature by natural cooling or blowing.
9. An ultra-thin lithium metal composite negative electrode, It is characterized in that The ultra-thin lithium metal composite negative electrode material is prepared by the method for preparing the ultra-thin lithium metal composite negative electrode material according to any one of claims 1 to 8.
10. Use of the ultra-thin lithium metal composite negative electrode as claimed in claim 9 in liquid lithium metal batteries and solid lithium metal batteries.
Citation Information
Patent Citations
Ultrathin metal lithium composite material as well as preparation method and application thereof
CN114927660A
Preparation method of surface-modified lithium metal negative electrode, lithium metal negative electrode and lithium metal battery
CN115954440A
Negative electrode and preparation method thereof, battery and electric device
CN117476876A
Preparation method and application of composite metal lithium negative electrode
CN117542965A
Cited By
Ultrathin lithium negative electrode with bulk-phase ion channel as well as preparation method and application of ultrathin lithium negative electrode