Polyaniline and phytic acid double-intercalation NH4V4O10 composite material as well as preparation method and application thereof
By preparing a polyaniline and phytic acid double-intercalated NH4V4O10 composite material, the problems of structural collapse and slow diffusion rate of vanadium-based cathode materials in zinc-ion batteries were solved, achieving high specific capacity and good cycle reversibility, which is suitable for aqueous zinc-ion battery cathode materials.
Patent Information
- Application Number
- CN202410960152.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-01
AI Technical Summary
Existing vanadium-based cathode materials suffer from structural collapse and slow zinc ion diffusion rates in zinc-ion batteries, which affect the electrochemical reaction rate and cycle life.
A nanosheet array was prepared by using a polyaniline and phytic acid double-intercalated NH4V4O10 composite material and stacking nanosheets through two hydrothermal reactions. This increased the interplanar spacing and specific surface area, provided a rapid zinc ion diffusion channel, and maintained structural stability.
It achieves high specific capacity and good cycle reversibility of zinc-ion batteries, with an initial charge-discharge specific capacity of 522.8/496.1 mAh g-1 and a capacity of 345.2/344.5 mAh g-1 after 500 cycles, demonstrating excellent electrochemical performance.
Smart Images

Figure CN118888720A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new energy and electrochemical energy storage, and in particular to a polyaniline and phytic acid double intercalated NH4V4O 10 Composite materials and their preparation methods and applications. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] With the increasing shortage of energy and environmental pollution, it is urgent to develop clean and environmentally friendly new energy storage technologies. In recent years, electrochemical energy storage technology has made rapid progress. The safety, environmental protection and economy provided by aqueous zinc-ion batteries make them particularly attractive to fixed storage devices such as microgrids and distributed energy storage. They are considered to be a new generation of large-scale energy storage battery technology that is expected to replace lithium-ion batteries. Despite this, zinc-ion batteries still face many difficulties and challenges in commercial applications, such as slow electrochemical reaction rates and relatively short cycle life. Therefore, it is urgent to develop a new type of high-performance aqueous zinc-ion battery cathode material.
[0004] Vanadium-based oxides, manganese-based oxides, Prussian blue analogs, layered sulfides and polyanionic compounds have been widely studied as positive electrode materials for aqueous zinc-ion batteries. Among them, vanadium-based positive electrode materials have the advantages of low cost, abundant resources, vanadium multivalence and large tunnel skeleton, and are one of the important positive electrode materials. However, vanadium oxides are often layered structures, which are prone to structural collapse during electrochemical reactions, resulting in limited service life and limited zinc ion diffusion rate.
[0005] In order to solve the above problems, it is necessary to modify the vanadium-based cathode materials. The main methods include ion doping, vacancy engineering, heterojunction, intercalation and composite with carbon materials. In terms of intercalation technology, Wang et al. from the University of Electronic Science and Technology of China (Wang et al. Pillaring of a conductive polymer in layered V2O5 boosting ultra-fast Zn 2+ / H storage in aqueous media [J]. Electrochimica Acta 2022, 146, 140270.) prepared a polypyrrole intercalated vanadium pentoxide composite material, which was used as a positive electrode material for zinc ion batteries at 2.0 A g -1 At a current density of 1.34 W, the capacity was maintained at 263 mAh g after 800 cycles.-1 In addition, the Chinese patent with publication number CN 114084906 A discloses a rapid preparation method and application of alkali metal ion intercalated vanadium oxide nanobelts at 2 A g -1 At a current density of 274 mAh g -1 However, dual polymer intercalated vanadium oxide composites have rarely been reported as zinc-ion batteries. Summary of the invention
[0006] In view of the above problems existing in the prior art, the present invention aims to provide a polyaniline and phytic acid double intercalated NH4V4O 10 Composite material and its preparation method and application. NH4V4O double intercalated with polyaniline and phytic acid 10 The composite material is a nanosheet stacked into a nanoarray morphology, with a large specific surface area and high conductivity. It can shorten the diffusion distance of zinc ions during the charge and discharge process, provide more active sites, and the double intercalation of polyaniline and phytic acid effectively increases the NH4V4O 10 The interplanar spacing provides a wider diffusion channel for the rapid insertion and extraction of zinc ions, accelerates the electrochemical reaction of the zinc ion battery charging and discharging process, and as a pillar, maintains the structural stability during the reaction process. At the same time, the preparation method is simple and can be obtained through only two hydrothermal reactions, without the need for special equipment and harsh conditions, and has good practical value.
[0007] In order to achieve the above object, the technical solution of the present invention is as follows: In the first aspect, the present invention provides a polyaniline and phytic acid double intercalated NH4V4O 10 The method for preparing a composite material is characterized by comprising the following steps: S1. Preparing a precursor reaction solution: Dispersing ammonium metavanadate and oxalic acid dihydrate in water, and stirring them vigorously; S2. Preparation of NH4V4O 10 Precursor: The reaction solution prepared in S1 was kept at 130 °C for 8 hours, purified and dried to obtain NH4V4O 10 Precursor; S3. Prepare the intermediate reaction solution: NH4V4O prepared in S2 10 The precursor was dispersed in water and stirred vigorously, and then 60 μL of aniline was dropped into the solution and stirred vigorously, and then 50% phytic acid was dropped into the solution and stirred vigorously; S4. Preparation of polyaniline and phytic acid double intercalated NH4V4O 10 Composite material: The intermediate reaction solution prepared by S3 was reacted at 140°C for 24 hours, purified and dried to obtain polyaniline and phytic acid double intercalated NH4V4O 10 Composite materials.
[0008] Furthermore, in step S1, the molar ratio of ammonium metavanadate to oxalic acid dihydrate is 1:1.
[0009] Furthermore, in steps S1 and S3, the vigorous stirring time is 30 minutes.
[0010] Furthermore, in steps S2 and S4, the purification process is washing and centrifugation.
[0011] Furthermore, in steps S2 and S4, the drying method is freeze drying at −40° C. for 48 hours.
[0012] Furthermore, in steps S1 and S3, the water is deionized water.
[0013] Furthermore, in step S3, the content of phytic acid is 0, 50, 100, 150 and 200 μL.
[0014] In a second aspect, the present invention provides a polyaniline and phytic acid double intercalated NH4V4O prepared by the above method. 10 Composite material, the polyaniline and phytic acid double intercalated NH4V4O 10 The composite material is a nanosheet with uniform size and a thickness of about 40nm. Its appearance is a nanoarray composed of nanosheets.
[0015] In a third aspect, the present invention provides a polyaniline and phytic acid double intercalated NH4V4O 10 Application of composite materials: the above polyaniline and phytic acid double intercalation NH4V4O 10 The composite material is used as positive electrode material for aqueous zinc-ion batteries.
[0016] In a fourth aspect, the present invention provides an aqueous zinc ion battery, wherein the zinc ion battery comprises the above-mentioned polyaniline and phytic acid double intercalation NH4V4O 10 Composite materials.
[0017] Compared with the prior art, the present invention has the following advantages and effects: (1) The present invention prepares NH4V4O by regulating the content of phytic acid and polyaniline intercalation 10 Nanoarray, it should be noted that the embedding of polyaniline and different contents of phytic acid is beneficial to increase the NH4V4O 10 The interplanar spacing of NH4V4O 10 The interlayers play a supporting role, maintaining NH4V4O 10 While maintaining structural stability, it also provides a wider channel for the insertion and extraction of zinc ions.
[0018] (2) The composite material prepared by the present invention is a nanoarray composed of nanosheets with a thickness of about 40 nm, uniform size, and a porous structure and a large specific surface area, which is conducive to the full infiltration of the electrolyte, promotes the transfer of electrons and ions, and makes the material have good electrochemical properties.
[0019] (3) The morphology and charge-discharge performance of the zinc ion battery cathode material prepared by the present invention have good repeatability and excellent cycle reversibility. -1 At the current density of 1.34 W, the specific capacity of the first charge and discharge reached 522.8 / 496.1 mAh g -1 ; at 2.0 A g -1 After 500 cycles of charge and discharge, the charge and discharge cycle capacity can still be maintained at 345.2 / 344.5 mAh g -1 , which has good practical application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 1 is the XRD diagram of the composite materials prepared in Examples 1 to 4 of the present invention and Comparative Examples 1 and 2.
[0021] Figure 2 The polyaniline and phytic acid double intercalated NH4V4O prepared in Example 1 of the present invention 10 FESEM image of the composite material, with a magnification of 10,000 times.
[0022] Figure 3 The polyaniline and phytic acid double intercalated NH4V4O prepared in Example 1 of the present invention 10 FESEM image of the composite material, with a magnification of 20,000 times.
[0023] Figure 4 The polyaniline and phytic acid double intercalated NH4V4O prepared in Example 1 of the present invention 10 Charge and discharge curves of the composite material.
[0024] Figure 5 The polyaniline and phytic acid double intercalated NH4V4O prepared in Example 1 of the present invention 10 Graph of the cyclic performance of the composite material. DETAILED DESCRIPTION
[0025] The present invention will be further described in detail below with reference to the accompanying drawings and by way of examples. The following examples are intended to explain the present invention but the present invention is not limited to the following examples.
[0026] Example 1 A kind of polyaniline and phytic acid double intercalated NH4V4O10 The preparation method of the composite material comprises the following steps: Step S1. Preparation of precursor reaction solution 0.58 g NH4VO3 was dispersed in 35 mL deionized water and stirred vigorously for 30 min to obtain a light yellow suspension; then, 0.7 g H2C2O4·2H2O was added to the above suspension and continued to stir vigorously for 30 min to obtain a clear yellow-green solution.
[0027] Step S2. Preparation of NH4V4O 10 Precursor The precursor reaction solution prepared in step S1 was transferred to a 50 mL polytetrafluoroethylene-lined autoclave and maintained at 130 °C for 8 h. After cooling to room temperature, the precipitate was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. It was freeze-dried at −40 °C for 48 h to obtain NH4V4O 10 Precursor.
[0028] Step S3. Preparation of intermediate reaction solution The NH4V4O prepared in step S2 10 The precursor (1.91 g) was dispersed in 30 mL of deionized water and stirred vigorously for 30 minutes to form a suspension; then, 60 μL of aniline was added dropwise to the suspension and stirred vigorously for another 30 minutes; next, 100 μL of 50% phytic acid solution was added dropwise to the suspension and stirred vigorously for another 30 minutes.
[0029] Step S4. Preparation of polyaniline and phytic acid double intercalated NH4V4O 10 Composite Materials The intermediate reaction solution prepared in step S3 was transferred to a 50 mL polytetrafluoroethylene-lined autoclave and kept at 140 °C for 24 h. After cooling to room temperature, the precipitate was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. Finally, it was freeze-dried at −40 °C for 48 h to obtain polyaniline and phytic acid double intercalated NH4V4O 10 Composite materials.
[0030] Example 2 A kind of polyaniline and phytic acid double intercalated NH4V4O 10 The preparation method of the composite material comprises the following steps: Step S1. Preparation of precursor reaction solution 0.58 g NH4VO3 was dispersed in 35 mL deionized water and stirred vigorously for 30 min to obtain a light yellow suspension; then, 0.7 g H2C2O4·2H2O was added to the above suspension and continued to stir vigorously for 30 min to obtain a clear yellow-green solution.
[0031] Step S2. Preparation of NH4V4O 10 Precursor The precursor reaction solution prepared in step S1 was transferred to a 50 mL polytetrafluoroethylene-lined autoclave and maintained at 130 °C for 8 h. After cooling to room temperature, the precipitate was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. It was freeze-dried at −40 °C for 48 h to obtain NH4V4O 10 Precursor.
[0032] Step S3. Preparation of intermediate reaction solution The NH4V4O prepared in step S2 10 The precursor (1.91 g) was dispersed in 30 mL of deionized water and stirred vigorously for 30 minutes to form a suspension; then, 60 μL of aniline was added dropwise to the suspension and stirred vigorously for another 30 minutes; next, 50 μL of 50% phytic acid solution was added dropwise to the suspension and stirred vigorously for another 30 minutes.
[0033] Step S4. Preparation of polyaniline and phytic acid double intercalated NH4V4O 10 Composite Materials The intermediate reaction solution prepared in step S3 was transferred to a 50 mL polytetrafluoroethylene-lined autoclave and kept at 140 °C for 24 h. After cooling to room temperature, the precipitate was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. Finally, it was freeze-dried at −40 °C for 48 h to obtain polyaniline and phytic acid double intercalated NH4V4O 10 Composite materials.
[0034] Example 3 A kind of polyaniline and phytic acid double intercalated NH4V4O 10 The preparation method of the composite material comprises the following steps: Step S1. Preparation of precursor reaction solution 0.58 g NH4VO3 was dispersed in 35 mL deionized water and stirred vigorously for 30 min to obtain a light yellow suspension; then, 0.7 g H2C2O4·2H2O was added to the above suspension and continued to stir vigorously for 30 min to obtain a clear yellow-green solution.
[0035] Step S2. Preparation of NH4V4O 10 Precursor The precursor reaction solution prepared in step S1 was transferred to a 50 mL polytetrafluoroethylene-lined autoclave and maintained at 130 °C for 8 h. After cooling to room temperature, the precipitate was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. It was freeze-dried at −40 °C for 48 h to obtain NH4V4O10 Precursor.
[0036] Step S3. Preparation of intermediate reaction solution The NH4V4O prepared in step S2 10 The precursor (1.91 g) was dispersed in 30 mL of deionized water and stirred vigorously for 30 minutes to form a suspension; then, 60 μL of aniline was added dropwise to the suspension and stirred vigorously for another 30 minutes; next, 150 μL of 50% phytic acid solution was added dropwise to the suspension and stirred vigorously for another 30 minutes.
[0037] Step S4. Preparation of polyaniline and phytic acid double intercalated NH4V4O 10 Composite Materials The intermediate reaction solution prepared in step S3 was transferred to a 50 mL polytetrafluoroethylene-lined autoclave and kept at 140 °C for 24 h. After cooling to room temperature, the precipitate was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. Finally, it was freeze-dried at −40 °C for 48 h to obtain polyaniline and phytic acid double intercalated NH4V4O 10 Composite materials.
[0038] Example 4 A kind of polyaniline and phytic acid double intercalated NH4V4O 10 The preparation method of the composite material comprises the following steps: Step S1. Preparation of precursor reaction solution 0.58 g NH4VO3 was dispersed in 35 mL deionized water and stirred vigorously for 30 min to obtain a light yellow suspension; then, 0.7 g H2C2O4·2H2O was added to the above suspension and continued to stir vigorously for 30 min to obtain a clear yellow-green solution.
[0039] Step S2. Preparation of NH4V4O 10 Precursor The precursor reaction solution prepared in step S1 was transferred to a 50 mL polytetrafluoroethylene-lined autoclave and maintained at 130 °C for 8 h. After cooling to room temperature, the precipitate was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. It was freeze-dried at −40 °C for 48 h to obtain NH4V4O 10 Precursor.
[0040] Step S3. Preparation of intermediate reaction solution The NH4V4O prepared in step S2 10The precursor (1.91 g) was dispersed in 30 mL of deionized water and stirred vigorously for 30 minutes to form a suspension; then, 60 μL of aniline was added dropwise to the suspension and stirred vigorously for another 30 minutes; next, 200 μL of 50% phytic acid solution was added dropwise to the suspension and stirred vigorously for another 30 minutes.
[0041] Step S4. Preparation of polyaniline and phytic acid double intercalated NH4V4O 10 Composite Materials The intermediate reaction solution prepared in step S3 was transferred to a 50 mL polytetrafluoroethylene-lined autoclave and kept at 140 °C for 24 h. After cooling to room temperature, the precipitate was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. Finally, it was freeze-dried at −40 °C for 48 h to obtain polyaniline and phytic acid double intercalated NH4V4O 10 Composite materials.
[0042] Comparative Example 1 A kind of polyaniline and phytic acid double intercalated NH4V4O 10 The preparation method of the composite material comprises the following steps: Step S1. Preparation of precursor reaction solution 0.58 g NH4VO3 was dispersed in 35 mL deionized water and stirred vigorously for 30 min to obtain a light yellow suspension; then, 0.7 g H2C2O4·2H2O was added to the above suspension and continued to stir vigorously for 30 min to obtain a clear yellow-green solution.
[0043] Step S2. Preparation of NH4V4O 10 Precursor The precursor reaction solution prepared in step S1 was transferred to a 50 mL polytetrafluoroethylene-lined autoclave and maintained at 130 °C for 8 h. After cooling to room temperature, the precipitate was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. It was freeze-dried at −40 °C for 48 h to obtain NH4V4O 10 Precursor.
[0044] Step S3. Preparation of intermediate reaction solution The NH4V4O prepared in step S2 10 The precursor (1.91 g) was dispersed in 30 mL of deionized water and stirred vigorously for 30 minutes to form a suspension; then, 60 μL of aniline was added dropwise to the suspension and stirred vigorously for another 30 minutes.
[0045] Step S4. Preparation of polyaniline intercalated NH4V4O 10 Composite Materials The intermediate reaction solution prepared in step S3 was transferred to a 50 mL polytetrafluoroethylene-lined autoclave and kept at 140 °C for 24 h. After cooling to room temperature, the precipitate was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. Finally, it was freeze-dried at −40 °C for 48 h to obtain polyphenylene intercalated NH4V4O 10 Composite materials.
[0046] Comparative Example 2 A kind of polyaniline and phytic acid double intercalated NH4V4O 10 The preparation method of the composite material comprises the following steps: Step S1. Preparation of precursor reaction solution 0.58 g NH4VO3 was dispersed in 35 mL deionized water and stirred vigorously for 30 min to obtain a light yellow suspension; then, 0.7 g H2C2O4·2H2O was added to the above suspension and continued to stir vigorously for 30 min to obtain a clear yellow-green solution.
[0047] Step S2. Preparation of NH4V4O 10 Precursor The precursor reaction solution prepared in step S1 was transferred to a 50 mL polytetrafluoroethylene-lined autoclave and maintained at 130 °C for 8 h. After cooling to room temperature, the precipitate was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. It was freeze-dried at −40 °C for 48 h to obtain NH4V4O 10 Precursor.
[0048] Figure 1 It is a double intercalated NH4V4O of polyaniline and phytic acid 10 XRD pattern of the composite material shows that all diffraction peaks are consistent with NH4V4O 10 The standard card (PDF # 31-0075) is consistent, and no other impurities appear, indicating that the product is polyaniline and phytic acid double intercalated NH4V4O 10 It should be noted that after adding polyaniline, the diffraction peak shifted to the left and the interplanar spacing increased, indicating that the polyaniline intercalation was successful; with the increase of phytic acid content, the interplanar spacing gradually increased, indicating that the content of phytic acid had an effect on the NH4V4O 10 The interplanar spacing has an important influence on the
[0049] Figure 2 and 3 It is a double intercalated NH4V4O of polyaniline and phytic acid 10 From the FESEM image of the composite material, it can be seen that the composite material prepared by the present invention is a nanoarray composed of nanosheets with a thickness of about 40 nm and uniform size.
[0050] The polyaniline obtained in Example 1 and phytic acid were double intercalated into NH4V4O 10 The composite material is made into an electrode as follows: Double intercalation of polyaniline and phytic acid into NH4V4O 10 The composite material, Super-P and polyvinylidene fluoride were mixed in N-methylpyrrolidone at a mass ratio of 7:2:1 to prepare the working electrode, and then the slurry was coated on Ti foil and dried in vacuum at 80℃ for 24h to obtain the working electrode (positive electrode). Metal zinc sheet, glass fiber (Whatman, Grade GF / D) and 3 M ZnSO4 aqueous solution were used as the negative electrode, separator and electrolyte of the zinc ion battery, respectively, and assembled into a CR2032 type zinc ion battery. All constant current charge and discharge tests were performed by the blue electric test system (LAND CT 2001A) at a test temperature of 25℃. Figure 4 The assembled battery is at 2.0 A g -1 The first charge and discharge performance under current density, the electrode material of the present invention is 2.0 A g -1 At the current density, the charge-discharge specific capacity reaches 522.8 / 496.1 mAh g -1 ; Figure 5 The assembled battery is at 2.0 A g -1 Cyclic performance under current density, the electrode material of the present invention has a current density of 2.0 A g -1 After 500 cycles of charge and discharge, the charge and discharge cycle capacity can still be maintained at 345.2 / 344.5 mAh g -1 .
[0051] The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.
[0052] Although the present invention has been disclosed as above by way of embodiments, it is not intended to limit the protection scope of the present invention. Any changes and modifications made by any technician familiar with the technology without departing from the concept and scope of the present invention should fall within the protection scope of the present invention.
Claims
1. A double intercalated NH4V4O of polyaniline and phytic acid 10 A method for preparing a composite material, characterized in that: The following steps are involved: S1. Preparing a precursor reaction solution: Dispersing ammonium metavanadate and oxalic acid dihydrate in water, and stirring them vigorously; S2. Preparation of NH4V4O 10 Precursor: The reaction solution prepared in S1 was kept at 130 °C for 8 hours, purified and dried to obtain NH4V4O 10 Precursor; S3. Prepare the intermediate reaction solution: NH4V4O prepared in S2 10 The precursor was dispersed in water and stirred vigorously, and then 60 μL of aniline was dropped into the solution and stirred vigorously, and then 50% phytic acid was dropped into the solution and stirred vigorously; S4. Preparation of polyaniline and phytic acid double intercalated NH4V4O 10 Composite material: The intermediate reaction solution prepared by S3 was reacted at 140°C for 24 hours, purified and dried to obtain polyaniline and phytic acid double intercalated NH4V4O 10 Composite materials.
2. The polyaniline and phytic acid double intercalation NH4V4O according to claim 1 10 A method for preparing a composite material, characterized in that: In step S1, the molar ratio of ammonium metavanadate to oxalic acid dihydrate is 1:
1.
3. The polyaniline and phytic acid double intercalation NH4V4O according to claim 1 10 A method for preparing a composite material, characterized in that: In steps S1 and S3, the vigorous stirring time is 30 minutes.
4. The polyaniline and phytic acid double intercalation NH4V4O according to claim 1 10 A method for preparing a composite material, characterized in that: In steps S2 and S4, the purification process is washing and centrifugation.
5. The polyaniline and phytic acid double intercalation NH4V4O according to claim 1 10 A method for preparing a composite material, characterized in that: In steps S2 and S4, the drying method is freeze drying at −40° C. for 48 hours.
6. The polyaniline and phytic acid double intercalation NH4V4O according to claim 1 10 A method for preparing a composite material, characterized in that: In steps S1 and S3, the water is deionized water.
7. The polyaniline and phytic acid double intercalation NH4V4O according to claim 1 10 A method for preparing a composite material, characterized in that: In step S3, the content of phytic acid is 0, 50, 100, 150 and 200 μL.
8. A double intercalated NH4V4O of polyaniline and phytic acid 10 A composite material, characterized in that Prepared by the preparation method according to any one of claims 1 to 7, the NH4V4O 10 The composite material is a nanosheet stacked into a nanoarray morphology; the polyaniline is intercalated in NH4V4O 10 In the crystal plane, the phytic acid is also intercalated in NH4V4O 10 In the crystal plane, the polyaniline and phytic acid form a double intercalation structure.
9. A polyaniline and phytic acid double intercalation NH4V4O 10 The application of composite materials is characterized by: The polyaniline and phytic acid double intercalation NH4V4O 10 Composite materials for aqueous zinc-ion batteries.
10. An aqueous zinc ion battery, characterized in that: The positive electrode material of the zinc ion battery is the polyaniline and phytic acid double intercalation NH4V4O 10 Composite materials.