Method for recycling regenerated positive electrode material from waste ternary lithium ion battery

By using ternary deep eutectic solvent and microwave-assisted leaching technology, regenerated cathode materials can be recovered from waste ternary lithium-ion batteries, solving the problems of high cost and insufficient purity in existing technologies, and realizing the preparation of efficient and high-performance regenerated cathode materials.

CN118888893AActive Publication Date: 2024-11-01CHINA ELECTRONIC SYST ENG FOURTH CONSTR CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411042923.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-01
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Existing methods for recovering metals from spent ternary lithium-ion batteries are costly and involve complex processes. Furthermore, when the recovered metals are reused to prepare lithium battery cathode materials, the purity is insufficient, resulting in poor performance of the regenerated cathode materials.

Method used

By employing a ternary deep eutectic solvent combined with microwave-assisted leaching technology, and through ball milling, microwave-assisted leaching, precipitation, and calcination processes, cathode materials are recycled from spent ternary lithium-ion batteries. The molar ratio of metal elements is adjusted to improve purity and performance.

Benefits of technology

This technology enables efficient recycling of cathode materials, resulting in high-performance lithium batteries. It solves the problems of high cost and insufficient purity in existing technologies and provides a new approach for the recycling of waste lithium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of recycling of lithium ion batteries, and particularly discloses a method for recycling a regenerated positive electrode material from a waste ternary lithium ion battery. According to the method, the positive electrode material of the waste lithium ion battery is efficiently leached in a manner of combining the ternary deep eutectic solvent with microwave-assisted leaching, and the positive electrode material is recycled and regenerated in a manner of combining subsequent precipitation and adjusting the molar ratio of metal elements. The technical scheme provided by the invention effectively solves the problems that in the prior art, a method for recycling metal from a waste ternary lithium ion battery is relatively high in cost and complex in technological process, and when the recycled metal is applied to preparation of the lithium battery positive electrode material, the cost is relatively high. The problem of poor effect of the regenerated positive electrode material caused by insufficient purity is solved, and a new idea is provided for the treatment of the waste ternary lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion battery recycling, and specifically discloses a method for recycling positive electrode materials from waste ternary lithium ion batteries. Background Art

[0002] Among the many chemical power sources, lithium-ion batteries have high energy density, long storage life, and small size. Small, light, low self-discharge efficiency and no memory effect are favored by people. With the continuous improvement of the global penetration rate of new energy vehicles, the demand for automotive power batteries and energy storage batteries continues to grow at a high rate, but at present, other battery systems are still difficult to develop on a large scale, and lithium-ion batteries will still be the mainstream energy storage chemical power source. However, due to the growing demand for lithium-ion batteries, its raw materials have gradually attracted widespread attention. Due to the global shortage of major elements such as cobalt, nickel and lithium, it is expected that the production of lithium-ion batteries will be affected by resource shortages by 2050. The positive electrode materials of waste lithium-ion batteries are rich in cobalt, nickel and lithium, so the recycling of waste lithium-ion batteries has become an important way to reduce resource pressure. What's more, waste lithium-ion batteries contain many toxic substances. If they are not properly stored and disposed of, the harm they cause to the social environment and human health cannot be underestimated.

[0003] At present, the recovery of metals from waste lithium-ion batteries is mainly achieved by combining mechanical treatment of positive electrode materials, hydrometallurgy or pyrometallurgy to extract metals or metal oxides. However, the mechanical treatment method takes a long time and causes great damage to the equipment. Hydrometallurgy is the mainstream method in the existing recycling field, with the advantages of mild reaction conditions, low tail gas emissions and high metal recovery rate. However, hydrometallurgy requires a large amount of inorganic acid or organic acid, especially organic acid, which is generally expensive and has high processing costs. Pyrometallurgy, on the other hand, recovers or refines valuable metals from waste lithium-ion batteries through physical or chemical transformation at high temperatures. The current pyrometallurgical recovery process is mainly based on roasting and leaching, that is, roasting is first performed by adding a certain amount of substances as roasting agents, and the roasting products are separated by leaching to obtain different products. Although pyrometallurgy has a high metal extraction rate, the recovery process is complicated and the cost is high. More importantly, when the recovered metal is used to prepare positive electrode materials for lithium batteries, there is a problem of insufficient purity, resulting in poor effect of regenerated positive electrode materials.

[0004] In view of this, developing a method for recovering positive electrode materials from waste ternary lithium-ion batteries with a simple process flow and convenient operation has important practical significance for the field of lithium-ion battery recycling technology. Summary of the invention

[0005] In view of the fact that the methods for recovering metals from waste ternary lithium-ion batteries in the prior art are high in cost and complicated in process flow, and that when the recovered metals are used to prepare positive electrode materials for lithium batteries, the purity is insufficient, resulting in poor effect of the regenerated positive electrode materials, the present invention provides a method for recovering and regenerating positive electrode materials from waste ternary lithium-ion batteries.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions: The first aspect of the present invention provides a method for recovering and regenerating positive electrode materials from waste ternary lithium-ion batteries, comprising the following steps: Step 1: ball-milling the waste ternary lithium-ion battery positive electrode powder to obtain pretreated positive electrode powder; Step 2: uniformly mixing the pretreated positive electrode powder and the ternary deep eutectic solvent, performing microwave-assisted leaching, and filtering to obtain a metal leaching solution; Step 3, adding a reducing crystallizer and a first precipitant to the metal leaching solution, filtering to obtain a nickel-cobalt-manganese co-precipitate and a lithium salt solution; adding a second precipitant to the lithium salt solution, precipitating at 90-100° C., filtering to obtain a lithium salt precipitate; Step 4: adjusting the molar ratio of nickel, cobalt and manganese in the nickel-cobalt-manganese co-precipitate, calcining once at 700-800° C. to obtain a primary sintered product; adding the lithium salt precipitate to the primary sintered product, and calcining twice at 700-850° C. to obtain a regenerated positive electrode material; Wherein, the ternary deep eutectic solvent is a mixture of tartaric acid, sorbitol and choline bitartrate.

[0007] The present invention designs a ternary deep eutectic solvent, with tartaric acid and sorbitol as hydrogen bond donors and choline bitartrate as a hydrogen bond acceptor. The ternary deep eutectic solvent is a strong-coordinated, low-viscosity acid-based deep eutectic solvent, has good proton activity and reducing ability, and can achieve efficient and gentle leaching of lithium, nickel, cobalt, and manganese. Among them, the ternary deep eutectic solvent can extract high-valent metal elements (cobalt, nickel, and manganese) in the positive electrode material through complexation to form high-valent metal complexes. In addition, since the metal oxides in the positive electrode material have excellent wave absorption properties, microwave action can assist in improving the leaching efficiency of the ternary deep eutectic solvent for the metal oxides.

[0008] By adding a reducing crystallizer, a high-valent metal can be reduced to a low-valent metal, changing the stability of the metal complex, and converting it into a low-valent metal complex with poor stability, which is easier to combine with the first precipitant to form a nickel-cobalt-manganese co-precipitated lithium salt solution. A second precipitant is then added to the lithium salt solution to obtain a lithium salt precipitate. In order to better apply and regenerate the recovered metal precipitate, the present invention can determine the metal content in the metal leaching solution, obtain the molar ratio of each metal element by calculation, precipitate the metal in turn, and then adjust the molar ratio of each metal element in the recovered metal precipitate by supplementing metal oxide and lithium salt precipitation, and combine the calcination process to obtain a regenerated positive electrode material.

[0009] The technical solution designed by the present invention can recycle the regenerated positive electrode material from the waste lithium-ion battery positive electrode material. Through the process design of waste material-raw material-regenerated product, the reuse of the waste lithium battery positive electrode material is realized to the greatest extent. More importantly, the regenerated positive electrode material finally provided by the present invention has excellent performance and can be used to prepare regenerated lithium batteries. The technical solution of the present invention effectively solves the problem that the method of recovering metals from waste ternary lithium-ion batteries is high in cost and complicated in process flow, and when the recovered metals are used to prepare lithium battery positive electrode materials, there is insufficient purity resulting in poor effect of the regenerated positive electrode material, which provides a new idea for the recycling and reuse of waste lithium battery positive electrode materials.

[0010] Preferably, the molar ratio of tartaric acid, sorbitol and choline bitartrate in the ternary deep eutectic solvent is 0.2:3:1-0.8:5:1.

[0011] Further preferably, the preparation method of the ternary deep eutectic solvent comprises the following steps: weighing each raw material component according to the designed ratio, mixing them evenly, and obtaining a deep eutectic solvent precursor; adding deionized water to the deep eutectic solvent precursor, mixing and stirring at 80-100°C until the liquid is colorless and transparent, and obtaining a ternary deep eutectic solvent.

[0012] More preferably, the amount of deionized water added is 10%-15% of the mass of the deep eutectic solvent precursor.

[0013] The viscosity of the deep eutectic solvent represents the difficulty of the components in the system moving to the holes, and has a great influence on the dissolution efficiency of metal oxides. Too high viscosity is not conducive to the dissolution of metal oxides, thereby reducing their leaching of valuable metal elements. Therefore, the present invention adds deionized water to the deep eutectic solvent precursor to reduce the viscosity of the ternary deep eutectic solvent and improve the leaching rate of the ternary deep eutectic solvent to metal oxides.

[0014] Preferably, in step 1, the rotation speed of the ball mill is 500-700 rpm, and the ball milling time is 3-5 h.

[0015] Preferably, in step 2, the mass ratio of the pretreated positive electrode powder to the ternary deep eutectic solvent is 1:30-2:50.

[0016] Preferably, in step 2, the temperature of the microwave-assisted leaching is 70-90° C., and the time of the microwave-assisted leaching is 1-3 h.

[0017] Preferably, in step three, the reducing crystallization agent is a hydrogen peroxide solution with a mass concentration of 50%-65%.

[0018] Preferably, in step three, the first precipitant is a 0.5-1 mol / L oxalic acid solution.

[0019] Preferably, in step three, the second precipitant is a 0.5-1 mol / L sodium carbonate solution.

[0020] Further preferably, the molar ratio of the hydrogen peroxide in the reducing crystallizer to the total metal amount in the metal leaching solution is 1:1-2:1.

[0021] Further preferably, the molar ratio of oxalic acid in the first precipitant to the total amount of nickel, cobalt and manganese ions in the metal leaching solution is 1:1-2:1.

[0022] Further preferably, the molar ratio of sodium carbonate in the second precipitant to lithium ions in the lithium salt solution is 1:1-1.5:1.

[0023] Further preferably, in step 4, the holding time of the first calcination is 2-4h.

[0024] Further preferably, in step 4, the holding time of the secondary calcination is 10-12 hours.

[0025] Further preferably, in step 4, the molar ratio of nickel, cobalt and manganese in the nickel-cobalt-manganese co-precipitate is adjusted to 6:2:2.

[0026] The present invention adjusts the molar ratio of lithium, nickel, cobalt and manganese to 1:0.6:0.2:0.2, and combines the calcination process to obtain the regenerated positive electrode material LiNi 0.6 Co 0.2 Mn 0.2 O2.

[0027] The second aspect of the present invention provides a regenerated positive electrode material, which is recovered and prepared by using the method for recovering regenerated positive electrode material from waste ternary lithium-ion batteries.

[0028] In summary, the present invention provides a method for recovering and regenerating positive electrode materials from waste ternary lithium-ion batteries, wherein the waste lithium-ion battery positive electrode materials are efficiently leached by a ternary deep eutectic solvent combined with microwave-assisted leaching, and the positive electrode materials are recovered and regenerated by combining subsequent precipitation and adjusting the molar ratio of metal elements. The obtained recycled and regenerated positive electrode materials have good electrochemical properties. The technical solution provided by the present invention effectively solves the problems of high cost and complicated process flow of the methods for recovering metals from waste ternary lithium-ion batteries in the prior art, and the problem that when the recovered metals are used to prepare lithium battery positive electrode materials, the purity is insufficient, resulting in poor effect of the regenerated positive electrode materials, and provides a new idea for the treatment of waste ternary lithium-ion batteries. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1 This embodiment provides a method for recovering and regenerating positive electrode materials from waste ternary lithium-ion batteries, comprising the following steps: Step 1: ball mill the waste ternary lithium-ion battery positive electrode powder at a speed of 600 rpm for 4 hours to obtain 50 g of pretreated positive electrode powder; Step 2: Evenly mix the pretreated positive electrode powder and the ternary deep eutectic solvent, perform microwave-assisted leaching at 85° C. for 2 h, and filter to obtain a metal leachate; determine the content of each metal ion in the metal leachate by inductively coupled plasma atomic emission spectrometry, and calculate the molar ratio of each metal element to be nickel: cobalt: manganese: lithium = 7.9: 1.6: 1.7: 17.2; Step 3: Add 1500 mL of 60% hydrogen peroxide solution and 200 mL of 1 mol / L oxalic acid solution to the metal leachate, let stand for 12 hours, filter, and obtain nickel-cobalt-manganese co-precipitate and lithium salt solution; add 250 mL of 1 mol / L sodium carbonate solution to the lithium salt solution, let stand at 95° C. for 8 hours, filter the precipitate, and obtain lithium salt precipitate; Step 4: Add 1.9 g of cobalt oxalate and 1.3 g of manganese oxalate to adjust the molar ratio of nickel, cobalt and manganese in the nickel-cobalt-manganese coprecipitate to 6:2:2, and calcine once at 700 ° C. for 3 hours to obtain a primary sintered product; add 76.5% of the lithium salt precipitate to the primary sintered product, calcine twice at 750 ° C. for 12 hours to obtain a regenerated positive electrode material LiNi 0.6 Co 0.2 Mn0.2 O2.

[0031] Among them, the ternary deep eutectic solvent is a mixture of tartaric acid, sorbitol and choline bitartrate in a molar ratio of 0.5:4:1. The specific preparation method includes the following steps: weighing 90g of tartaric acid, 874g of sorbitol and 304g of choline bitartrate according to the designed ratio, mixing them evenly to obtain a deep eutectic solvent precursor; adding 155g of deionized water to the deep eutectic solvent precursor, mixing and stirring at 90°C until the liquid is colorless and transparent, to obtain a ternary deep eutectic solvent.

[0032] Example 2 This embodiment provides a method for recovering and regenerating positive electrode materials from waste ternary lithium-ion batteries, comprising the following steps: Step 1: ball mill the waste ternary lithium-ion battery positive electrode powder at a speed of 500 rpm for 4 hours to obtain 50 g of pretreated positive electrode powder; Step 2: Evenly mix the pretreated positive electrode powder and the ternary deep eutectic solvent, perform microwave-assisted leaching at 75° C. for 3 h, and filter to obtain a metal leachate; determine the content of each metal ion in the metal leachate by inductively coupled plasma atomic emission spectrometry, and calculate the molar ratio of each metal element to be nickel: cobalt: manganese: lithium = 9.2: 3.1: 3.7: 19.9; Step 3: Add 1500 mL of 55% hydrogen peroxide solution and 350 mL of 0.8 mol / L oxalic acid solution to the metal leachate, let stand for 12 hours, filter, and obtain nickel-cobalt-manganese co-precipitate and lithium salt solution; add 210 mL of 1 mol / L sodium carbonate solution to the lithium salt solution, let stand at 95° C. for 8 hours, filter the precipitate, and obtain lithium salt precipitate; Step 4: Add 2.78 g of nickel oxalate and 1.1 g of cobalt oxalate to adjust the molar ratio of nickel, cobalt and manganese in the nickel-cobalt-manganese coprecipitate to 6:2:2, calcine once at 720 ° C, keep warm for 3 hours, and obtain a primary sintered product; add 92.7% of the lithium salt precipitate to the primary sintered product, calcine twice at 800 ° C, keep warm for 12 hours, and obtain the regenerated positive electrode material LiNi 0.6 Co 0.2 Mn 0.2 O2.

[0033] Among them, the ternary deep eutectic solvent is a mixture of tartaric acid, sorbitol and choline bitartrate in a molar ratio of 0.5:4:1. The specific preparation method includes the following steps: weighing 90g of tartaric acid, 874g of sorbitol and 304g of choline bitartrate according to the designed ratio, mixing them evenly to obtain a deep eutectic solvent precursor; adding 155g of deionized water to the deep eutectic solvent precursor, mixing and stirring at 90°C until the liquid is colorless and transparent, to obtain a ternary deep eutectic solvent.

[0034] Example 3 This embodiment provides a method for recovering and regenerating positive electrode materials from waste ternary lithium-ion batteries, comprising the following steps: Step 1: ball mill the waste ternary lithium-ion battery positive electrode powder at a speed of 700 rpm for 4 hours to obtain 50 g of pretreated positive electrode powder; Step 2: Evenly mix the pretreated positive electrode powder and the ternary deep eutectic solvent, perform microwave-assisted leaching at 90° C. for 1 h, and filter to obtain a metal leachate; determine the content of each metal ion in the metal leachate by inductively coupled plasma atomic emission spectrometry, and calculate the molar ratio of each metal element to be nickel: cobalt: manganese: lithium = 8.5: 2.9: 2.3: 18.6; Step 3: add 1500 mL of 60% hydrogen peroxide solution and 250 mL of 1 mol / L oxalic acid solution to the metal leachate, let stand for 12 hours, filter, and obtain nickel-cobalt-manganese co-precipitate and lithium salt solution; add 220 mL of 1 mol / L sodium carbonate solution to the lithium salt solution, let stand at 95° C. for 8 hours, filter the precipitate, and obtain lithium salt precipitate; Step 4: Add 0.29 g of nickel oxalate and 0.85 g of manganese oxalate to adjust the molar ratio of nickel, cobalt and manganese in the nickel-cobalt-manganese coprecipitate to 6:2:2, calcine once at 760 ° C, keep warm for 3 hours, and obtain a primary sintered product; add 78% of the lithium salt precipitate to the primary sintered product, calcine twice at 850 ° C, keep warm for 12 hours, and obtain the regenerated positive electrode material LiNi 0.6 Co 0.2 Mn 0.2 O2.

[0035] Among them, the ternary deep eutectic solvent is a mixture of tartaric acid, sorbitol and choline bitartrate in a molar ratio of 0.5:4:1. The specific preparation method includes the following steps: weighing 90g of tartaric acid, 874g of sorbitol and 304g of choline bitartrate according to the designed ratio, mixing them evenly to obtain a deep eutectic solvent precursor; adding 155g of deionized water to the deep eutectic solvent precursor, mixing and stirring at 90°C until the liquid is colorless and transparent, to obtain a ternary deep eutectic solvent.

[0036] Comparative Example 1 This comparative example provides a method for recovering and regenerating positive electrode materials from waste ternary soft-pack lithium batteries. The difference from Example 1 is that the deep eutectic solvent is a mixture of sorbitol and choline chloride, which specifically includes the following contents.

[0037] Step 1: ball mill the waste ternary lithium-ion battery positive electrode powder at a speed of 600 rpm for 4 hours to obtain 50 g of pretreated positive electrode powder; Step 2: Evenly mix the pretreated positive electrode powder and the deep eutectic solvent, perform microwave-assisted leaching at 85° C. for 2 h, and filter to obtain a metal leachate; determine the content of each metal ion in the metal leachate by inductively coupled plasma atomic emission spectrometry, and calculate the molar ratio of each metal element to be nickel: cobalt: manganese: lithium = 7.9: 1.6: 1.7: 17.2; Step 3: Add 1500 mL of 60% hydrogen peroxide solution and 200 mL of 1 mol / L oxalic acid solution to the metal leachate, let stand for 12 hours, filter, and obtain nickel-cobalt-manganese co-precipitate and lithium salt solution; add 250 mL of 1 mol / L sodium carbonate solution to the lithium salt solution, let stand at 95° C. for 8 hours, filter the precipitate, and obtain lithium salt precipitate; Step 4: Add 1.9 g of cobalt oxalate and 1.3 g of manganese oxalate to adjust the molar ratio of nickel, cobalt and manganese in the nickel-cobalt-manganese coprecipitate to 6:2:2, and calcine once at 700 ° C. for 3 hours to obtain a primary sintered product; add 76.5% of the lithium salt precipitate to the primary sintered product, calcine twice at 750 ° C. for 12 hours to obtain a regenerated positive electrode material LiNi 0.6 Co 0.2 Mn 0.2 O2.

[0038] Among them, the ternary deep eutectic solvent is a mixture of sorbitol and choline chloride in a molar ratio of 4:1, and the specific preparation method includes the following steps: weighing 874g of sorbitol and 304g of choline chloride according to the designed ratio, mixing them evenly, and obtaining a deep eutectic solvent precursor; adding 141g of deionized water to the deep eutectic solvent precursor, mixing and stirring at 90°C until the liquid is colorless and transparent, and obtaining a ternary deep eutectic solvent.

[0039] Comparative Example 2 This comparative example provides a method for recovering and regenerating positive electrode materials from waste ternary soft-pack lithium batteries, which differs from Example 1 in that microwave-assisted leaching is not used, and specifically includes the following contents.

[0040] Step 1: ball mill the waste ternary lithium-ion battery positive electrode powder at a speed of 600 rpm for 4 hours to obtain 50 g of pretreated positive electrode powder; Step 2: Evenly mix the pretreated positive electrode powder and the ternary deep eutectic solvent, let stand for 2 hours, and filter to obtain a metal leachate; use an inductively coupled plasma atomic emission spectrometer to determine the content of each metal ion in the metal leachate, and calculate the molar ratio of each metal element to be nickel: cobalt: manganese: lithium = 7.9: 1.6: 1.7: 17.2; Step 3: Add 1500 mL of 60% hydrogen peroxide solution and 200 mL of 1 mol / L oxalic acid solution to the metal leachate, let stand for 12 hours, filter, and obtain nickel-cobalt-manganese co-precipitate and lithium salt solution; add 250 mL of 1 mol / L sodium carbonate solution to the lithium salt solution, let stand at 95° C. for 8 hours, filter the precipitate, and obtain lithium salt precipitate; Step 4: Add 1.9 g of cobalt oxalate and 1.3 g of manganese oxalate to adjust the molar ratio of nickel, cobalt and manganese in the nickel-cobalt-manganese coprecipitate to 6:2:2, and calcine once at 700 ° C. for 3 hours to obtain a primary sintered product; add 76.5% of the lithium salt precipitate to the primary sintered product, calcine twice at 750 ° C. for 12 hours to obtain a regenerated positive electrode material LiNi 0.6 Co 0.2 Mn 0.2 O2.

[0041] Among them, the ternary deep eutectic solvent is a mixture of tartaric acid, sorbitol and choline bitartrate in a molar ratio of 0.5:4:1. The specific preparation method includes the following steps: weighing 90g of tartaric acid, 874g of sorbitol and 304g of choline bitartrate according to the designed ratio, mixing them evenly to obtain a deep eutectic solvent precursor; adding 155g of deionized water to the deep eutectic solvent precursor, mixing and stirring at 90°C until the liquid is colorless and transparent, to obtain a ternary deep eutectic solvent.

[0042] In order to further demonstrate the technical effect of the present invention, the present invention tests the regenerated positive electrode materials obtained in Examples 1-3 and Comparative Examples 1-2 and makes them into lithium-ion button batteries, as shown in the test examples.

[0043] Test example S1, 0.08 g of the recovered positive electrode material, 0.01 g of acetylene black, 0.01 g of polyvinylidene fluoride and 2 mL of N-methylpyrrolidone were mixed uniformly to obtain a positive electrode slurry; S2. The positive electrode slurry is coated on aluminum foil to make a positive electrode sheet. In an inert atmosphere, graphite is used as a negative electrode sheet, the electrolyte is an electrolyte containing LiPF6, and the isolation membrane is a ceramic-coated polypropylene / polyethylene (PP / PE) isolation membrane. Assemble and obtain a lithium-ion battery.

[0044] The present invention conducts discharge capacity test, rate test and cycle performance test on lithium ion batteries made by using the recycled positive electrode materials obtained in each embodiment and comparative example, which specifically include the following contents: Discharge capacity test: The charge and discharge cut-off voltage is 3.0-4.48V, the first charge and discharge rate is 0.5C, the lithium-ion battery is charged to 4.48V at 0.5C, then charged to 0.05C at a constant voltage, and then discharged to 3.0V at 0.5C to obtain the discharge capacity, which is the first discharge capacity. Discharge capacity = first discharge capacity (mAh) / cathode active material weight (g).

[0045] Rate test: The charge and discharge cut-off voltage is 3.0-4.48V. The lithium-ion battery is charged to 4.48V at 0.5C, then charged to 0.05C at a constant voltage, and then discharged to 3.0V at 2C to obtain the 2C discharge capacity of the lithium-ion battery. The 2C discharge capacity retention rate = 2C discharge capacity / 0.5C discharge capacity.

[0046] Cycle performance test: The lithium-ion battery is charged to 4.48V at 0.7C, then charged to 0.05C at a constant voltage, and then discharged to 3.0V at 1C. This is a charge and discharge cycle. Repeat the above process and record the capacity retention rate of the lithium-ion battery after 500 cycles. The test results are shown in Table 1.

[0047] Table 1 Recycled positive electrode material LiNi obtained from various examples and comparative examples 0.6 Co 0.2 Mn 0.2 Electrochemical performance test results of lithium-ion button batteries made with O2

[0048] It can be seen from Table 1 that the lithium ion battery prepared by using the positive electrode material recycled from the waste ternary lithium ion battery provided by the present invention has excellent electrochemical performance, which provides a new treatment idea for waste ternary lithium ion batteries.

[0049] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for recovering and regenerating positive electrode materials from waste ternary lithium-ion batteries, characterized in that: The steps include: Step 1: ball-milling the waste ternary lithium-ion battery positive electrode powder to obtain pretreated positive electrode powder; Step 2: uniformly mixing the pretreated positive electrode powder and the ternary deep eutectic solvent, performing microwave-assisted leaching, and filtering to obtain a metal leaching solution; Step 3, adding a reducing crystallizing agent and a first precipitating agent to the metal leaching solution, filtering, and obtaining a nickel-cobalt-manganese co-precipitate and a lithium salt solution; Adding a second precipitant to the lithium salt solution, precipitating at 90-100° C., and filtering to obtain a lithium salt precipitate; Step 4: adjusting the molar ratio of nickel, cobalt and manganese in the nickel-cobalt-manganese co-precipitate, calcining once at 700-800° C. to obtain a primary sintered product; adding the lithium salt precipitate to the primary sintered product, and calcining twice at 700-800° C. to obtain a regenerated positive electrode material; Wherein, the ternary deep eutectic solvent is a mixture of tartaric acid, sorbitol and choline bitartrate.

2. The method for recovering and regenerating positive electrode materials from waste ternary lithium-ion batteries according to claim 1, characterized in that: The molar ratio of tartaric acid, sorbitol and choline bitartrate in the ternary deep eutectic solvent is 0.2:3:1-0.8:5:

1.

3. The method for recovering and regenerating positive electrode materials from waste ternary lithium-ion batteries as claimed in claim 2, characterized in that: The preparation method of the ternary deep eutectic solvent comprises the following steps: weighing each raw material component according to the designed ratio, mixing them evenly, and obtaining a deep eutectic solvent precursor; adding deionized water to the deep eutectic solvent precursor, mixing and stirring at 80-100° C. until the liquid is colorless and transparent, and obtaining a ternary deep eutectic solvent.

4. The method for recovering and regenerating positive electrode materials from waste ternary lithium-ion batteries as claimed in claim 3, characterized in that: The amount of deionized water added is 10%-15% of the mass of the deep eutectic solvent precursor.

5. The method for recovering and regenerating positive electrode materials from waste ternary lithium-ion batteries according to claim 1, characterized in that: In step 1, the rotation speed of the ball mill is 500-700 rpm, and the ball milling time is 3-5 h.

6. The method for recovering and regenerating positive electrode materials from waste ternary lithium-ion batteries according to claim 1, characterized in that: In step 2, the mass ratio of the pretreated positive electrode powder to the ternary deep eutectic solvent is 1:30-2:50; and / or In step 2, the temperature of the microwave-assisted leaching is 70-90° C., and the time of the microwave-assisted leaching is 1-3 h.

7. The method for recovering and regenerating positive electrode materials from waste ternary lithium-ion batteries according to claim 1, characterized in that: In step 3, the reducing crystallization agent is a hydrogen peroxide solution with a mass concentration of 50%-65%; and / or In step 3, the first precipitant is a 0.5-1 mol / L oxalic acid solution; and / or In step 3, the second precipitant is a 0.5-1 mol / L sodium carbonate solution.

8. The method for recovering and regenerating positive electrode materials from waste ternary lithium-ion batteries as claimed in claim 7, characterized in that: The molar ratio of the hydrogen peroxide in the reducing crystallizer to the total metal amount in the metal leaching solution is 1:1-2:1; and / or The molar ratio of oxalic acid in the first precipitant to the total amount of nickel, cobalt and manganese ions in the metal leaching solution is 1:1-2:1; and / or The molar ratio of sodium carbonate in the second precipitant to lithium ions in the lithium salt solution is 1:1-1.5:

1.

9. The method for recovering and regenerating positive electrode materials from waste ternary lithium-ion batteries as claimed in claim 5, characterized in that: In step 4, the holding time of the first calcination is 2-4h; and / or In step 4, the holding time of the secondary calcination is 10-12 hours.

10. A regenerated positive electrode material, characterized in that: The positive electrode material is recovered by the method for recovering and regenerating positive electrode material from waste ternary lithium-ion batteries as described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Method for recovering valuable metals from active material of waste lithium ion battery

    CN113322376A

  • Process for recycling and regenerating ternary lithium battery positive electrode material by using deep eutectic solvent

    CN116417701A

  • Novel method for recycling valuable metal in waste ternary lithium battery by using eutectic solvent

    CN117821774A

  • Compositions and methods for extracting metals using non-aqueous solvents

    CN117999370A

  • Recycling li-ion batteries using green chemicals and processes

    US20200399737A1