High-efficiency up-conversion device and preparation method thereof
By introducing electron trap material and modified PEDOT:PSS hole transport layer into the upconversion device, balancing the ratio of donor to acceptor material, the problems of low light-light conversion efficiency and high threshold voltage are solved, and efficient infrared is achieved Light-visible light conversion and weak signal gain.
Patent Information
- Application Number
- CN202410883496.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-11-01
AI Technical Summary
Existing upconversion devices perform poorly in light-light conversion efficiency and high threshold voltage, especially in near-infrared spectral response and weak signal detection.
Using a bottom-up structure, high-efficiency upconversion device, including a transparent conductive electrode layer, an electron transport layer, a light emitting layer, a hole transport layer and a photosensitive layer, the electron trap material TCNQ or its derivative is introduced into the photosensitive layer, and the electron trap material TCNQ or its derivative is introduced through equilibrium to The body to acceptor material ratio and modified PEDOT:PSS hole transport layer realizes band bending and carrier injection, thereby improving light-to-photo conversion efficiency.
It realizes efficient infrared-visible light conversion efficiency, reduces the threshold voltage, enhances the response ability to weak signals, and improves the photomultiplier performance of the device.
Smart Images

Figure CN118890938A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of up-conversion devices, and in particular to a high-efficiency up-conversion device and a preparation method thereof. Background Art
[0002] Upconversion devices are optical devices that convert long-wavelength infrared light into short-wavelength visible light. They can detect infrared light information and have broad application prospects in the fields of biomedical detection, imaging, optical communications, etc. Commonly used upconverters based on organic semiconductors are non-multiplying types, and their theoretical external quantum efficiency does not exceed 100%, resulting in very small output when detecting weak signals, limiting their scope of application.
[0003] At present, in order to improve the spectral response of up-conversion devices, increase their response speed, and reduce the threshold voltage required to achieve high external quantum efficiency, the following two methods are often used to multiply them. The first type is to improve the bulk heterojunction active layer, and the second type is to improve the charge transport layer next to the electrode.
[0004] In the first method, the ratio between the donor and acceptor materials is adjusted to be mainly one material, and the ratio of the main material to the secondary material ranges from 20:1-100:1; the secondary material is isolated from the electrode, acting as a trap for the accumulation of photogenerated carriers, inducing band bending and reducing the charge injection barrier. This method of improving the active layer is effective for visible light photodiodes. However, for near-infrared devices, the exciton dissociation efficiency of its narrow bandgap materials is low, and a more balanced donor-acceptor ratio is required to reduce recombination losses and generate enough photogenerated charges to trigger photomultiplication. Therefore, this method has a poor multiplication effect on near-infrared devices. The second type of photomultiplier device designs an interface layer to enhance trap-assisted charge injection, which does not require a highly unbalanced active layer donor-acceptor ratio and is more suitable for near-infrared response.
[0005] However, the second type of devices are currently affected by high dark current when adjusting the interlayer energy level. The realization of photomultiplication will lead to an increase in dark current, resulting in reduced device performance, specifically manifested as high threshold voltage and low light-to-light conversion efficiency. Based on this, the second type of devices with improved charge transfer layers next to the electrodes still need to be improved. Summary of the invention
[0006] The present application provides a high-efficiency up-conversion device and a preparation method thereof, aiming to solve the problems of low light-to-light conversion efficiency and high threshold voltage of existing up-conversion devices.
[0007] In order to achieve the above objectives, the present application adopts the following technical solutions.
[0008] In a first aspect of the present application, a high-efficiency up-conversion device is provided, comprising a transparent conductive electrode layer, an electron transport layer, a light-emitting layer, a hole transport layer, a photosensitive layer and a metal electrode layer arranged in sequence from bottom to top;
[0009] The photosensitive layer comprises an electron donor material, an electron acceptor material and an electron trap material, wherein the LUMO energy level of the electron trap material is lower than the LUMO energy level of the electron acceptor material;
[0010] The electron donor material is PTB7-Th, the electron acceptor material is IEICO-4F; the electron trap material is TCNQ or its derivatives;
[0011] The hole transport layer is modified PEDOT:PSS.
[0012] In some embodiments, the mass ratio of the PTB7-Th to the IEICO-4F is 1:(1-2); the mass of the TCNQ is 1-3 wt % of the mass of the IEICO-4F.
[0013] In some embodiments, the modified PEDOT:PSS is prepared by the following method:
[0014] PEDOT:PSS, isopropanol and FS-31 were mixed and stirred, and allowed to stand to obtain modified PEDOT:PSS.
[0015] In some embodiments, the mass ratio of PEDOT:PSS, isopropanol, and FS-31 is 1:1:(0.002-0.005).
[0016] In some embodiments, the electron transport layer includes a zinc oxide layer disposed on the transparent conductive electrode layer and a PEIE layer disposed on the zinc oxide layer.
[0017] In some embodiments, the light-emitting layer includes polymer-based hole transport materials, small molecule hole transport materials, bipolar carrier transport materials, and phosphorescent light-emitting materials.
[0018] In some embodiments, the polymer-based hole transport material is PVK, the small molecule hole transport material is TCTA, the bipolar carrier transport material is 26DCzppy, and the phosphorescent light-emitting material is Ir(ppy)3.
[0019] In some embodiments, the mass ratio of PVK, TCTA, 26DCzppy and Ir(ppy)3 is (4-6):(1-3):(1-3):(0.5-1).
[0020] In some embodiments, the transparent conductive electrode layer is ITO; and the metal electrode layer is Al.
[0021] The second aspect of the present application provides a method for preparing the above-mentioned high-efficiency up-conversion device, characterized by comprising:
[0022] S1, take an ITO substrate, spin-coat a layer of zinc oxide precursor solution, and anneal at 170-190° C.; spin-coat a PEIE precursor solution on the zinc oxide layer, and anneal at 80-120° C. to obtain an electron transport layer;
[0023] S2, spin coating a light-emitting layer on the electron transport layer and annealing at 110-130° C.;
[0024] S3, spin coating a hole transport layer on the light-emitting layer, and annealing at 70-90° C. in vacuum;
[0025] S4, spin coating a photosensitive layer on the hole transport layer and annealing at 100-120° C.;
[0026] S5, evaporating a metal electrode layer on the photosensitive layer.
[0027] Compared with the prior art, the beneficial effects of this application are:
[0028] The up-conversion device of the present application introduces deep-level electron traps in the photosensitive layer to assist in generating unbalanced hole and electron concentrations, thereby achieving active layer band bending and causing the injection of carriers in the external circuit to achieve a multiplication effect. The ratio of donors and acceptors with photogenerated carrier functions in the photosensitive layer is more balanced to reduce recombination losses and generate sufficient photogenerated carriers to trigger multiplication, thereby achieving amplification of weak signals, and its infrared light-visible light conversion efficiency is high, achieving a high-efficiency infrared visualization function. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments recorded in the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0030] Figure 1 is a schematic diagram of the structure of a high-efficiency up-conversion device;
[0031] Figure 2 This is the working principle diagram of the high-efficiency up-conversion device;
[0032] Figure 3 The absorption spectrum and luminescence spectrum of the high-efficiency up-conversion device of Example 1;
[0033] Figure 4 is a response time diagram of the high-efficiency up-conversion device of Example 1;
[0034] Figure 5 Graph showing the photon conversion efficiency of the up-conversion devices of Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0035] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0036] In the following description of this embodiment, the terms "include", "comprising", "having" and "containing" are all open terms, meaning including but not limited to.
[0037] In the following description of this embodiment, the term "and / or" is used to describe the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, B exists alone, and A and B exist at the same time. A and B can be singular or plural. The character " / " generally indicates that the associated objects before and after are in an "or" relationship.
[0038] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0039] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0040] Those skilled in the art should understand that in the following description of the embodiments of the present application, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0041] Those skilled in the art will appreciate that the numerical ranges in the embodiments of the present application are to be construed as specifically disclosing each intermediate value between the upper and lower limits of the scope. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present application. The upper and lower limits of these smaller ranges may be independently included or excluded in the scope.
[0042] Unless otherwise specified, the technical / scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which this application belongs. Although this application only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of this application. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0043] In a first aspect, the present application provides a high-efficiency up-conversion device, the structure of which is as follows: Figure 1 As shown, it includes a transparent conductive electrode layer, an electron transport layer, a light-emitting layer, a hole transport layer, a photosensitive layer and a metal electrode layer arranged in sequence from bottom to top;
[0044] The photosensitive layer includes an electron donor material, an electron acceptor material and an electron trap material, and the LUMO energy level of the electron trap material is lower than the LUMO energy level of the electron acceptor material. Specifically, the electron donor material is PTB7-Th, and the electron acceptor material is IEICO-4F; the electron trap material is TCNQ or its derivatives; such as F4-TCNQ, F2-TCNQ, F6-TCNQ, etc., and the electron trap material in this application is preferably TCNQ or F4-TCNQ. Among them, the mass ratio of the PTB7-Th and IEICO-4F is 1: (1 to 2); the mass of the TCNQ is 1 to 3wt% of the mass of IEICO-4F. The balanced ratio of the electron donor material PTB7-Th with the function of photogenerated carriers and the electron acceptor material IEICO-4F in the photosensitive layer can reduce the recombination loss and generate sufficient photogenerated carriers to trigger multiplication.
[0045] The hole transport layer is modified PEDOT:PSS, which is prepared by the following method: PEDOT:PSS, isopropanol, and FS-31 are mixed and stirred, and allowed to stand to obtain modified PEDOT:PSS, wherein the mass ratio of PEDOT:PSS, isopropanol, and FS-31 is 1:1:(0.002-0.005), preferably 1:1:0.003.
[0046] In the present application, the transparent conductive electrode layer is preferably ITO; the metal electrode layer is preferably Al.
[0047] In the present application, the electron transport layer includes a zinc oxide layer disposed on the transparent conductive electrode layer and a PEIE layer disposed on the zinc oxide layer.
[0048] In the present application, the light-emitting layer includes a polymer-based hole transport material, a small molecule hole transport material, a bipolar carrier transport material and a phosphorescent luminescent material, and the thickness of the light-emitting layer is preferably 60-80 nm. Among them, the polymer-based hole transport material is preferably PVK, the small molecule hole transport material is preferably TCTA, the bipolar carrier transport material is preferably 26DCzppy, and the phosphorescent luminescent material is preferably Ir(ppy)3.
[0049] The mass ratio of PVK, TCTA, 26DCzppy and Ir(ppy)3 is (4-6):(1-3):(1-3):(0.5-1), and the preferred mass ratio of PVK, TCTA, 26DCzppy and Ir(ppy)3 is 5:2:2:1.
[0050] The high-efficiency upconverter of the present application uses a high-efficiency infrared response system PTB7-Th:IEICO-4F for its photosensitive layer, whose spectral response can reach 1000nm, and has strong absorption and photoelectric conversion capabilities in the near-infrared region; TCNQ electron traps with a deeper LUMO energy level (-4.5eV), whose LUMO is much lower than the LUMO energy level of the acceptor material IEICO-4F (-3.9eV), have excellent electron capture capabilities. In order to avoid the formation of a continuous phase and the loss of the electron trap effect, the amount of TCNQ added is not more than 3% of the total mass of the electron-donating acceptor material to ensure that the electron traps form independent dispersed phases. The light-emitting layer uses a high-efficiency composite phosphorescent luminescent material system, including a polymer-based hole transport material PVK, a small molecule hole transport material TCTA, a bipolar carrier transport material 26DCzppy, and a phosphorescent luminescent material Ir(ppy)3.
[0051] The working principle of the up-conversion device is as follows Figure 2 As shown. Figure 2(a) is the working principle of the electron trap-assisted up-conversion device of the present application, in which 1 wt% of the electron trap TCNQ of the mass of IEICO-4F is introduced into the photosensitive layer PTB7-Th:IEICO-4F and directly contacts the electrode; the LUMO energy level of TCNQ (-4.5 eV) is deeper than the LUMO energy level (-3.9 eV) of the electron acceptor material IEICO-4F in the bulk heterojunction, and a small amount of electron traps are difficult to form a continuous phase in the photosensitive layer, and will form an island structure with many discontinuous items. When a reverse voltage is applied and light is applied, the bulk heterojunction electron acceptor material will be excited to produce excitons and dissociate into hole-electron pairs at the interface; the hole-electron pairs dissociate into holes and electrons under the action of the external voltage, among which the photogenerated holes are transmitted along the HOMO energy level of the electron donor material through the bulk heterojunction and collected by the electrode, and the photogenerated electrons are captured by the electron traps with deeper LUMO energy levels and cannot be transmitted to the external circuit through the continuous phase, thereby achieving electron accumulation inside the active layer and causing energy band bending in the active layer, reducing the barrier for hole injection at the anode, allowing holes in the external circuit to be injected into the device and pass through the active layer, and then be collected by the cathode through the hole transport layer, thereby achieving the photoelectric gain of the upconverter. In addition, TCNQ will form a TCNQ-Al complex with the evaporated Al electrode and further reduce the barrier for hole injection from the Al electrode into the device. The combined effect of the two allows holes from the external circuit to be injected into the device, migrate to the light-emitting layer through the hole transport layer PEDOT:PSS, and be blocked by the ZnO layer in the light-emitting layer to participate in luminescence, thus breaking through the restriction of the photon conversion efficiency being subject to the photoelectric conversion efficiency of the photosensitive layer and the external quantum efficiency of the light-emitting layer, and greatly improving the light-to-light conversion efficiency.
[0052] Figure 2 (b) is the working principle diagram of the up-conversion device without electron trap assistance. This type of up-conversion device has no electron trap assistance. Since the HOMO energy level of the Al electrode and the HOMO energy level of the electron donor polymer have a certain potential barrier, it is difficult for the holes in the external circuit to be injected into the device, so that the photon conversion efficiency is restricted by the photoelectric conversion efficiency of the photosensitive layer and the external quantum efficiency of the light-emitting layer. The photoelectric gain capacity of the external circuit is not effectively utilized, and it is difficult to significantly improve the light-light conversion efficiency. In this type of device model, the gain of the external circuit is not considered. The photon conversion efficiency of the up-conversion device can generally be estimated by the external quantum efficiency of the light detection unit × the external quantum efficiency of the light-emitting unit. The maximum external quantum efficiency of the light detection unit is 100%, and the external quantum efficiency of the light-emitting unit has been reported to be close to 25%. Therefore, when the external circuit gain is not used, the theoretical maximum value of the photon conversion efficiency of the up-conversion device is about 25%.
[0053] The compounds involved in this application can all be obtained by purchasing commodities, and their chemical structures are as follows:
[0054]
[0055]
[0056] In this application, FS-31 is DuPont capstone FS-31 water-based solvent-based fluorocarbon surfactant;
[0057] PEDOT:PSS is poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonic acid).
[0058] Example 1
[0059] This embodiment provides a high-efficiency up-conversion device, which is composed of a detection unit and a light-emitting unit layer, including a transparent conductive electrode layer, an electron transport layer, a light-emitting layer, a hole transport layer, a photosensitive layer and a metal electrode layer arranged in sequence from bottom to top.
[0060] In this embodiment, the transparent conductive electrode layer is indium tin oxide ITO; the electron transport layer is a ZnO layer and a PEIE layer, the light-emitting layer is a mixed layer of PVK, TCTA, 26DCzppy and Ir(ppy)3; the hole transport layer is modified PEDOT:PSS; the photosensitive layer is a mixed layer of PTB7-Th, IEICO-4F and TCNQ, wherein the mass ratio of PTB7-Th and IEICO-4F is 1:1.5, and the amount of TCNQ is 1% of the amount of IEICO-4F; the metal electrode layer is aluminum.
[0061] Among them, the thickness of the ZnO layer is 30nm, the thickness of the PEIE layer is 10nm; the thickness of the light-emitting layer is 70nm; the thickness of the hole transport layer is 30nm, the thickness of the photosensitive layer is 200nm, and the thickness of the metal electrode layer is 100nm.
[0062] The high-efficiency up-conversion device of this embodiment is prepared by a method comprising:
[0063] Dissolve 1000 mg of zinc acetate dihydrate and 280 μL of ethanolamine in 10 mL of 2-methoxyethanol and stir overnight to obtain a zinc oxide precursor solution;
[0064] The PEIE aqueous solution was diluted to 0.4 mg / mL with 2-methoxyethanol to obtain a PEIE precursor solution.
[0065] PVK:TCTA:26DCzppy:Ir(ppy)3 was dissolved in tetrahydrofuran at a mass ratio of 5:2:2:1 to a total concentration of 10 mg / mL to obtain a luminescent layer stock solution.
[0066] Dissolve PTB7-Th and IEICO-4F in chlorobenzene, add TCNQ to prepare an active solution; in the active solution, the concentration of PTB7-Th is 8 mg / mL, the concentration of IEICO-4F is 12 mg / mL, and the concentration of TCNQ is 0.12 mg / mL;
[0067] PEDOT:PSS, isopropanol, and FS-31 were mixed in a mass ratio of 1:1:0.003 and stirred overnight to obtain a modified PEDOT:PSS solution;
[0068] The zinc oxide precursor solution was spin-coated on the surface of the clean ITO substrate and annealed at 180°C for 20 minutes in a hot plate to obtain a zinc oxide layer; the PEIE precursor solution was spin-coated on the surface of the zinc oxide layer and annealed at 100°C for 10 minutes to obtain a PEIE layer. The zinc oxide layer and the PEIE layer constitute an electron transport layer.
[0069] The light-emitting layer solution was spin-coated on the surface of the electron transport layer at a rotation speed of 2500 r / min, and annealed at 120° C. for 10 minutes to obtain the light-emitting layer; the modified PEDOT:PSS solution was spin-coated on the light-emitting layer, and annealed at 80° C. for 10 minutes in a vacuum oven to form a hole transport layer;
[0070] The active solution was spin-coated on the surface of the hole transport layer at a speed of 2500 r / min and annealed at 100°C for 10 minutes to obtain a photosensitive layer with a thickness of 200 nm;
[0071] An Al layer with a thickness of 100 nm is evaporated on the surface of the photosensitive layer as an electrode to obtain a high-efficiency up-conversion device. The structure of the high-efficiency up-conversion device of this embodiment is:
[0072] ITO / ZnO / PEIE / PVK:TCTA:26DCzppy / PEDOT:PSS / PTB7-Th:IEICO-4F:1wt%TCNQ / Al.
[0073] Example 2
[0074] The difference between Example 2 and Example 1 is that the mass ratio of PTB7-Th and IEICO-4F is 1:1, the amount of TCNQ used is 2% of the amount of IEICO-4F used, and the rest is the same as Example 1.
[0075] Example 3
[0076] The difference between Example 3 and Example 1 is that the mass ratio of PTB7-Th to IEICO-4F is 1:2, the amount of TCNQ used is 3% of the amount of IEICO-4F used, and the rest is the same as Example 1.
[0077] Example 4
[0078] The difference between Example 4 and Example 1 is that the mass ratio of PVK:TCTA:26DCzppy:Ir(ppy)3 is changed to 4:3:1:0.5, and the rest is the same as Example 1.
[0079] Example 5
[0080] The difference between Example 5 and Example 1 is that the mass ratio of PVK:TCTA:26DCzppy:Ir(ppy)3 is changed to 6:1:3:1, and the rest is the same as Example 1.
[0081] Comparative Example 1
[0082] The comparative example provides an up-conversion device without electron trap assistance, which differs from Example 1 in that TCNQ is not added to the photosensitive layer, and the rest is the same as Example 1. The device structure of Comparative Example 1 is:
[0083] ITO / ZnO / PEIE / PVK:TCTA:26DCzppy / PEDOT:PSS / PTB7-Th:IEICO-4F / Al.
[0084] The high efficiency up-conversion device prepared in Example 1 was tested for performance. The test results are as follows: Figure 3 and Figure 4 shown.
[0085] The test results of its absorption spectrum and luminescence spectrum are as follows: Figure 3 As shown. Figure 3 It can be seen that the absorption peak is 935nm, which is in the near-infrared region that is difficult to distinguish with the naked eye; the luminescence spectrum peak is at 520nm, which is the green color that the human eye is sensitive to.
[0086] Figure 4 It is a response time diagram. It can be seen that under the excitation of infrared light with a wavelength of 808nm, the rise time is 40μs and the fall time is 237μs. Compared with the rise time, the fall time is significantly increased. This is due to the longer response time of the phosphorescent luminescence system.
[0087] The up-conversion devices of Example 1 and Comparative Example 1 were tested for light-to-light conversion efficiency. The results are as follows: Figure 5 As shown. Figure 5 It can be seen that when the optical power density is set to 0.1mW / cm -2 Under the irradiation of an infrared laser with a wavelength of 808nm, the amplified infrared high-efficiency up-conversion device of Example 1 emits a dazzling green light of 520nm, and the light-to-light conversion efficiency is 69.14%, while the light-to-light conversion efficiency of the non-amplified up-conversion device in Comparative Example 1 is only 10.4%.
[0088] The up-conversion devices prepared in Examples 2-5 were tested to have photoelectric performances close to that of the high-efficiency up-conversion device prepared in Example 1.
[0089] Although the present application has been described in detail in general terms and in specific embodiments in this specification, it is obvious to those skilled in the art that some modifications or improvements may be made to the present application. Therefore, these modifications or improvements made without departing from the spirit of the present application are within the scope of protection claimed in the present application.
Claims
1. A high-efficiency up-conversion device, characterized in that: It includes a transparent conductive electrode layer, an electron transport layer, a light-emitting layer, a hole transport layer, a photosensitive layer and a metal electrode layer arranged in sequence from bottom to top; The photosensitive layer comprises an electron donor material, an electron acceptor material and an electron trap material, wherein the LUMO energy level of the electron trap material is lower than the LUMO energy level of the electron acceptor material; The electron donor material is PTB7-Th, the electron acceptor material is IEICO-4F; the electron trap material is TCNQ or its derivatives; The hole transport layer is modified PEDOT:PSS.
2. The high-efficiency up-conversion device according to claim 1, characterized in that: The mass ratio of the PTB7-Th to the IEICO-4F is 1:(1-2); the mass of the TCNQ is 1-3wt% of the mass of the IEICO-4F.
3. The high-efficiency up-conversion device according to claim 1, characterized in that: The modified PEDOT:PSS is prepared by the following method: PEDOT:PSS, isopropanol and FS-31 were mixed and stirred, and allowed to stand to obtain modified PEDOT:PSS.
4. The high-efficiency up-conversion device according to claim 3, characterized in that: The mass ratio of PEDOT:PSS, isopropanol, and FS-31 is 1:1:(0.002-0.005).
5. The high-efficiency up-conversion device according to claim 1, characterized in that: The electron transport layer includes a zinc oxide layer disposed on the transparent conductive electrode layer and a PEIE layer disposed on the zinc oxide layer.
6. The high-efficiency up-conversion device according to claim 1, characterized in that: The light-emitting layer includes a polymer-based hole transport material, a small molecule hole transport material, a bipolar carrier transport material and a phosphorescent light-emitting material.
7. The high-efficiency up-conversion device according to claim 6, characterized in that: The polymer-based hole transport material is PVK, the small molecule hole transport material is TCTA, the bipolar carrier transport material is 26DCzppy, and the phosphorescent luminescent material is Ir(ppy)3.
8. The high-efficiency up-conversion device according to claim 7, characterized in that: The mass ratio of the PVK, TCTA, 26DCzppy and Ir(ppy)3 is (4-6):(1-3):(1-3):(0.5-1).
9. The high-efficiency up-conversion device according to claim 1, characterized in that: The transparent conductive electrode layer is ITO; the metal electrode layer is Al.
10. The method for preparing a high-efficiency up-conversion device according to claim 5, characterized in that: include: S1, take an ITO substrate, spin-coat a layer of zinc oxide precursor solution, and anneal at 170-190° C.; spin-coat a PEIE precursor solution on the zinc oxide layer, and anneal at 80-120° C. to obtain an electron transport layer; S2, spin coating a light-emitting layer on the electron transport layer and annealing at 110-130° C.; S3, spin coating a hole transport layer on the light-emitting layer, and annealing at 70-90° C. in vacuum; S4, spin coating a photosensitive layer on the hole transport layer and annealing at 100-120° C.; S5, evaporating a metal electrode layer on the photosensitive layer.