Method for producing glass article, glass article, and laminate
By performing water treatment and chemical strengthening processes on alkali aluminosilicate glass, a compressive stress layer is formed, which solves the problem of insufficient impact resistance of glass items, and improves high pencil strength and bending strength. It is suitable for foldable equipment.
Patent Information
- Application Number
- CN202380027744.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-23
- Filing Date
- 2023-03-09
- Publication Date
- 2024-11-01
AI Technical Summary
Existing glass items are insufficiently impact-resistant when facing stylus input, especially when used in foldable devices, and it is difficult to meet the demand for high pen strength.
By performing a water treatment process on the alkali aluminosilicate glass, it is brought into contact with the treated water for more than 0.5 hours and less than 15 hours, a compressive stress layer is formed in combination with the chemical strengthening process, and the temperature and conductivity of the treated water are controlled in the water treatment process. , optimize the thickness and composition of the glass to improve the pen strength of the glass.
The pen-down strength and bending strength of the glass are significantly improved, making it more efficient to withstand stylus input, and are suitable for foldable devices.
Smart Images

Figure CN118891235A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a glass article, a glass article, and a laminate including the glass article. Background Art
[0002] Chemically strengthened glass is often used as the cover glass of various electronic terminals, display devices, etc. In such devices, so-called foldable devices that can fold the display surface of the display have also been developed, and chemically strengthened glass is sometimes used as the cover glass of such foldable devices.
[0003] For chemically strengthened glass, by having a compressive stress layer formed by ion exchange treatment on the surface, the formation and development of surface cracks can be suppressed, and high strength can be obtained. It is believed that the strength of strengthened glass can be improved by adjusting the formation method of such a compressive stress layer (for example, Patent Document 1).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2013 / 088856 Summary of the invention
[0007] Problems to be solved by the invention
[0008] However, there is still room for improvement in glass articles used for protecting glass and the like to obtain higher impact resistance. In particular, in the case of devices corresponding to pen input using a stylus pen (original Japanese: タイラスペン), local impacts are easily applied to glass articles. Therefore, it is required to develop glass articles with high pen-fall strength that can fully withstand such pen input.
[0009] An object of the present invention is to provide a glass article having high pen-fall strength.
[0010] Means for solving problems
[0011] (1) The method for manufacturing a glass article of the present invention invented in order to solve the above-mentioned problems is characterized by comprising: a preparation step of preparing a treatment glass composed of an alkali-aluminosilicate glass containing an alkali metal oxide as a glass composition; and a water treatment step of contacting the treatment glass with treatment water for 0.5 hour or more and less than 15 hours.
[0012] The inventors of the present invention have conducted in-depth research and found that, when the treatment glass is alkali-aluminosilicate glass, the pen-falling strength of the treatment glass is greatly improved by performing a water treatment process in which the treatment glass is in contact with treatment water for the prescribed time. Moreover, such an effect of improving the pen-falling strength is maintained even after the water treatment process, that is, after the contact between the treatment glass and the treatment water is released. Therefore, a glass article with high pen-falling strength can be provided.
[0013] (2) In the configuration of (1) above, it is preferred that the treatment glass be immersed in treatment water at 46 to 100° C. in the water treatment step.
[0014] If the temperature of the treatment water is increased like this, the pen-fall strength of the treatment glass can be efficiently increased in a short time. That is, the treatment time (contact time of the treatment glass and the treatment water) until the desired pen-fall strength is obtained can be relatively shortened. Therefore, glass articles with high pen-fall strength can be efficiently manufactured.
[0015] (3) In the configuration of (1) above, in the water treatment step, the treatment glass may be immersed in treatment water adjusted to 100° C. or higher under a pressurized atmosphere.
[0016] If the temperature of the treatment water is increased in this way, the pen-fall strength of the treated glass can be efficiently increased in a short time. That is, the treatment time until the desired pen-fall strength is obtained can be relatively shortened. Therefore, glass articles with high pen-fall strength can be efficiently manufactured.
[0017] (4) In any one of the above configurations (1) to (3), preferably, in the water treatment step, the conductivity of the treated water is 3 mS / m or less.
[0018] If the treated water with low conductivity is used as described above, the pen-holding strength of the treated glass can be further improved. Therefore, the pen-holding strength of the glass article manufactured from the treated glass can also be further improved.
[0019] (5) In any one of the above structures (1) to (4), the processing glass is preferably in the form of a plate or sheet with a thickness of 0.005 to 0.1 mm.
[0020] If the processing glass is thinned like this, the glass article made of the processing glass can also be applied to foldable devices. On the other hand, the impact resistance of the glass article is inevitably reduced, and the improvement of the pen-falling strength becomes more important. Therefore, the pen-falling strength improvement effect of the present invention becomes more useful.
[0021] (6) In the configuration of (5) above, a thinning step may be further provided before the water treatment step, wherein the processing glass is thinned by etching to a thickness within the above range (0.005 to 0.1 mm).
[0022] (7) In the above-mentioned configuration (5), the process glass may be preformed into the above-mentioned thickness range (0.005 to 0.1 mm) by an overflow down-draw method.
[0023] (8) In any of the above structures (1) to (7), it is preferred that a chemical strengthening step is further provided before the water treatment step, in which the treatment glass is brought into contact with an alkali metal nitrate to form a compressive stress layer having a maximum compressive stress of 100 MPa or more on the surface.
[0024] In this way, the processing glass and glass articles become chemically strengthened glass having a compressive stress layer on the surface. Therefore, the writing strength of the glass articles can be improved, and the bending strength can be improved. If the glass articles with improved bending strength are thus suitable for foldable devices.
[0025] (9) In the configuration of (8) above, preferably, in the water treatment step, the temperature of the treated water is 50 to 95° C., and the contact time between the treatment glass and the treated water is 0.5 to 10 hours.
[0026] This provides water treatment conditions that are particularly suitable when the treatment glass is chemically strengthened glass, and can effectively improve the pen-fall strength of a glass article made of chemically strengthened glass.
[0027] (10) In the above-mentioned structure of (8) or (9), the processing glass preferably contains 50-80% SiO2, 5-25% Al2O3, 0-35% B2O3, 0-20% Li2O, 1-20% Na2O, and 0-10% K2O as the glass composition in mol%, and in the chemical strengthening process, the alkali metal nitrate is a molten salt containing potassium nitrate.
[0028] In this way, even when the processing glass is thin, it is easy to improve the writing strength and bending strength of the glass article at the same time.
[0029] (11) In any one of the above structures (8) to (10), it is preferred that a surface etching step is further provided after the ion exchange step and before the water treatment step, and in the surface etching step, the processing glass is etched in a range shallower than the compressive stress layer.
[0030] In this way, surface defects formed on the processing glass can be reduced in the ion exchange process or the like, and thus the pen-fall strength and / or bending strength of the glass article can be improved.
[0031] (12) The glass article of the present invention invented to solve the above-mentioned problems is characterized in that it is a plate-shaped or sheet-shaped glass article with a thickness of 0.005 to 0.1 mm, and in a pen drop test in which a 5.7 g ballpoint pen with a spherical tip with a diameter of 0.7 mm is dropped onto the main surface, the 60% destruction height is greater than 5 cm.
[0032] In this way, a glass article having high pen-fall strength can be obtained which is also able to sufficiently withstand pen input.
[0033] (13) In the configuration of (12) above, it is preferred that a compressive stress layer having a maximum compressive stress of 100 MPa or more is provided on the surface.
[0034] In this way, not only the writing strength is improved, but also the bending strength is improved, so it can also be suitable for use in foldable devices.
[0035] (14) The laminate of the present invention invented to solve the above-mentioned problems is characterized in that it comprises: a glass article having the structure of (12) or (13) above, and at least one main surface protection layer or reinforcement layer laminated on the glass article.
[0036] In this way, the protective layer can be used to protect the glass article to achieve higher pen-fall strength, or the reinforcing layer can be used to reinforce the glass article to achieve higher bending strength.
[0037] Effects of the Invention
[0038] According to the present invention, a glass article having high pen-fall strength can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a schematic diagram showing a cross section of a glass article according to a first embodiment of the present invention.
[0040] Figure 2 This is a schematic diagram of stress distribution in the thickness direction of the glass article according to the first embodiment of the present invention.
[0041] Figure 3 This is a flowchart of the method for producing a glass article according to the first embodiment of the present invention.
[0042] Figure 4 This is a cross-sectional view showing an embodiment of a water treatment step included in the method for producing a glass article according to the first embodiment of the present invention.
[0043] Figure 5 It is a schematic diagram showing a cross section of a laminated body according to a second embodiment of the present invention.
[0044] Figure 6This is a flowchart of a method for producing a glass article according to a third embodiment of the present invention.
[0045] Figure 7 This is a flowchart of a method for producing a glass article according to a fourth embodiment of the present invention.
[0046] Figure 8 This is a flowchart of a method for producing a glass article according to a fifth embodiment of the present invention.
[0047] Fig. 9 It is a side view showing an embodiment of the pen drop test.
[0048] Fig.10 It is a side view showing an embodiment of a bending failure test. DETAILED DESCRIPTION
[0049] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. It should be noted that in each embodiment, sometimes the same symbols are marked on the corresponding constituent elements, thereby omitting repeated descriptions. In each embodiment, when only a part of the composition is described, the composition of other embodiments previously described can be applied to the other parts of the composition. In addition, not only the combination of the compositions clearly described in the description of each embodiment can be adopted, but also the compositions of multiple embodiments can be partially combined with each other even if not clearly described, as long as there is no particular obstacle to the combination.
[0050] (First Embodiment)
[0051] <Glass Items>
[0052] like Figure 1 As shown, the glass article 1 of the first embodiment is in the form of a plate or sheet. The thickness t of the glass article 1 is not particularly limited, but is preferably 0.005 to 0.1 mm. The present invention is particularly useful for such thin glass.
[0053] The glass article 1 preferably has a 60% destruction height of 5 cm or more in a pen drop test in which a 5.7 g pen having a spherical tip with a diameter of 0.7 mm is dropped on the main surface. The 60% destruction height of the glass article 1 is more preferably 7 cm or more, 10 cm or more, or 15 cm or more.
[0054] In the present embodiment, the glass article 1 is a chemically strengthened glass that has been chemically strengthened by ion exchange, and includes a compressive stress layer 2 and a tensile stress layer 3. This can improve not only the pen-fall strength but also the bending strength.
[0055] When the glass article 1 is chemically strengthened glass, the two-point bending strength of the glass article 1 is preferably 900 MPa or more. The two-point bending strength of the glass article 1 is more preferably 1000 MPa or more, 1100 MPa or more, or 1200 MPa or more.
[0056] The compressive stress layer 2 is formed on the surface layer including the main surface 1a and the end surface 1b of the glass article 1. The tensile stress layer 3 is formed inside the glass article 1, that is, at a position deeper than the compressive stress layer 2. Here, the main surface refers to the surface of the entire plate-shaped or sheet-shaped glass surface except the end surface and the back surface.
[0057] An example of stress distribution of the glass article 1 is shown in FIG. Figure 2 .exist Figure 2 In the figure, the vertical axis represents the stress value and the horizontal axis represents the depth from the surface. Figure 2 The stress distribution is schematically represented by a straight line approximation, but the stress distribution can also be approximated by other functions (for example, a single curve function or a combination of multiple curve functions). In addition, in this specification, unless otherwise specified, the magnitude of each stress is expressed in absolute value. The stress distribution of the glass article 1 is not limited to Figure 2 The method shown.
[0058] Figure 2 The stress distribution shown in the figure illustrates the case where the glass article 1 is a tempered glass subjected to one stage of ion exchange treatment. In the stress distribution of the glass article 1, the compressive stress reaches the maximum (maximum compressive stress CS) at the surface, and the stress gradually decreases as the depth from the surface increases, and the stress reaches zero at the depth DOC. That is, DOC has the same meaning as the depth of the compressive stress. The tensile stress layer 3 having tensile stress extends in a region deeper than the depth DOC. For the stress distribution of the glass article 1, it is preferred that the stress distribution be as follows: Figure 2 The front and back surfaces are symmetrical as shown.
[0059] The tensile stress layer 3 includes a first region A1 where the tensile stress varies in the thickness direction of the glass article 1 and a second region A2 where the tensile stress is constant in the thickness direction. More specifically, the first region A1 extends from the depth DOC of the compressive stress layer 2 to the tensile stress convergence depth DCT, and the absolute value of the tensile stress gradually increases as the depth increases (in Figure 2 The negative number marks shown are areas where the stress gradually decreases. The second area A2 extends in an area deeper than the tensile stress convergence depth DCT, and is an area where the tensile stress is constant in the thickness direction. It should be noted that "constant tensile stress" means that the change in stress in the depth direction is less than 0.5 MPa / μm, and the change can be calculated, for example, by the differential value of the stress obtained by sampling at intervals of 0.1 μm in depth.
[0060] The depth DOC of the compressive stress layer 2 of the glass article 1 is preferably 20 μm or less, 1 μm or more and 19 μm or less, 2 μm or more and 18 μm or less, 3 μm or more and 17.5 μm or less, or 4 μm or more and 17 μm or less. The inventors have conducted various studies on the compressive stress value of the surface that does not become a dangerous failure form when broken and the threshold value of the depth of the compressive stress layer. As a result, it is found that, for example, for thin glass of 0.1 mm or less, it is effective to set the depth of the compressive stress layer to 20 μm or less. Thus, it has sufficient strength for bending and can also ensure safety.
[0061] The maximum compressive stress CS of the compressive stress layer 2 of the glass article 1 is preferably 100 MPa or more, 200 MPa or more and 1000 MPa or less, 300 MPa or more and 900 MPa or less, 400 MPa or more and 870 MPa or less, 430 MPa or more and 850 MPa or less, or 450 MPa or more and 800 MPa or less. By setting CS to such a range, high bending strength can be obtained.
[0062] The depth DOC of the compressive stress layer 2 and the thickness t of the glass article 1 satisfy the following formula (2).
[0063] DOC / t≤0.25(2)
[0064] By limiting the ratio of DOC to t to the above range, sufficient strength for bending can be obtained and safety can be ensured. The upper limit of DOC / t is preferably 0.23 or less. The lower limit of DOC / t is preferably 0.03 or more and 0.10 or more.
[0065] Regarding the tensile stress convergence depth DCT, the tensile stress can be calculated by the following formula (3).
[0066] DCT=(CS+CT) / (CS / DOC)(3)
[0067] The upper limit range of the maximum tensile stress CT of the second area A2 is preferably 1000MPa or less, 500MPa or less, 400MPa or less, 285MPa or less, 250MPa or less, 240MPa or less, 230MPa or less, 220MPa or less, 210MPa or less, 200MPa or less, 190MPa or less, 180MPa or less, 170MPa or less, 160MPa or less, 150MPa or less, 145MPa or less, 140MPa or less, 130MPa or less, 120MPa or less, 110MPa or less, 100MPa or less, 95MPa or less, 85MPa or less, or 70MPa or less. The lower limit range of the maximum tensile stress CT is preferably 10MPa or more, 20MPa or more, 35MPa or more, 50MPa or more, 55MPa or more, or 60MPa or more. By limiting CT as described above, it is possible to ensure safety so that the structure does not enter a dangerous state of destruction at the time of destruction, and to ensure strength against bending.
[0068] It should be noted that numerical values related to stress, such as CS, DOC, DCT, and CT, can be derived by measuring the stress distribution of glass using a measuring device such as FSM-6000 and SLP-1000 manufactured by Orihara Seisakusho, Ltd.
[0069] The lower limit range of the Young's modulus of the glass article 1 is preferably 55 GPa or more, 57 GPa or more, 60 GPa or more, or 62 GPa or more. The upper limit range of the Young's modulus of the glass article 1 is preferably 90 GPa or less.
[0070] As a method for forming the glass article 1 into a sheet, the overflow down-draw method is suitable from the viewpoint of cost and production volume, but there is a tendency that the thinner the sheet is, the more rapidly the glass is cooled, the lower the CS becomes, and the deeper the DOC becomes. In addition, it is known that when ion exchange is performed on thin glass, there is less glass inside to suppress the volume expansion of the ion exchange part, so it is difficult to obtain a high CS compared to thick glass. Therefore, for thin glass, it is not easy to achieve high CS and shallow DOC at a high level at the same time beyond simple conventional design (Japanese original text: design matters). That is, it is necessary to appropriately select the glass composition, the glass forming method, and the strengthening conditions. Therefore, for the glass article 1, an alkali aluminosilicate glass suitable for chemical strengthening is suitable, and among the alkali aluminosilicate glasses, a composition that can obtain a particularly high surface compressive stress value is suitable. In addition, in order to be able to form using the overflow down-draw method, a composition balance that achieves a high liquidus viscosity is preferred.
[0071] The glass article 1 preferably contains, for example, in mol % 50 to 80% SiO 2 , 5 to 25% Al 2 O 3 , 0 to 35% B 2 O 3 , 0 to 20% Li 2 O, 1 to 20% Na 2 O, and 0 to 10% K 2 O as a glass composition.
[0072] SiO2 is a component that forms a glass network. If the content of SiO2 is too little, it is difficult to vitrify. In addition, the thermal expansion coefficient becomes too high, and the thermal shock resistance is easily reduced. Therefore, the suitable lower limit range of SiO2 is 50% or more, 55% or more, 57% or more, 59% or more, and especially 61% or more in mole %. On the other hand, if the content of SiO2 is too much, the meltability and formability are easily reduced. In addition, the thermal expansion coefficient becomes too low, and it is difficult to match the thermal expansion coefficient of the surrounding materials. Therefore, the suitable upper limit range of SiO2 is 80% or less, 70% or less, 68% or less, 66% or less, 65% or less, and especially 64.5% or less.
[0073] Al2O3 is a component that improves ion exchange performance, and is a component that improves strain point, Young's modulus, fracture toughness, and Vickers hardness. Therefore, the suitable lower limit range of A12O3 is more than 5%, more than 8%, more than 10%, more than 11%, and more than 11.2% in mole %. On the other hand, if the content of Al2O3 is too much, the high-temperature viscosity rises, and the melting property and formability are easily reduced. In addition, it is easy to separate out devitrified crystals in glass, and it is difficult to utilize overflow down-drawing method etc. to be formed into a plate shape. In particular, when using alumina-based refractory as a forming body refractory, when utilizing overflow down-drawing method to form a glass sheet, at the interface with alumina-based refractory, it is easy to separate out devitrified crystals of spinel. In addition, acid resistance is also reduced, and it is difficult to be applied to the acid treatment process. Therefore, the upper limit range of Al2O3 is preferably 25% or less, 21% or less, 20.5% or less, 20% or less, 19.9% or less, 19.5% or less, 19.0% or less, and particularly 18.9% or less. If the content of Al2O3, which has a great influence on ion exchange performance, is set to a suitable range, it is easy to design CS / DOC to a high value even in thin glass.
[0074] B2O3 is a component that reduces high temperature viscosity and density, stabilizes glass, makes crystals difficult to precipitate, and reduces liquidus temperature. In addition, it is a component that suppresses Young's modulus, improves bending strength and crack resistance. However, if the content of B2O3 is too much, there is a tendency for surface coloring (Japanese original: ヤケ) called weathering (original Japanese: ヤケ) to occur due to ion exchange treatment, or water resistance is reduced, or the compressive stress value of the compressive stress layer is reduced. Therefore, the suitable lower limit range of B2O3 is 0% or more, 0.01% or more, 0.02% or more, 0.1% or more, and 0.3% or more in mole %, and the suitable upper limit range is 35% or less, 30% or less, 25% or less, 22% or less, 20% or less, and especially 15% or less. It should be noted that from the viewpoint of giving priority to improving CS, the content of B2O3 is further preferably 0.2-5%, 0.3-1%. In addition, from the viewpoint of improving chemical durability for the purpose of suppressing defects during etching, the upper limit of the content of B2O3 may be preferably 1% or more, 1.5% or more, or 2% or more, and the lower limit may be 5% or less, 4.5% or less, 4% or less, or 3% or less. On the other hand, from the viewpoint of preferentially suppressing Young's modulus, the content of B2O3 may be further preferably 10 to 25%, 15 to 23%, or 18 to 22%.
[0075] Li2O is an ion exchange component, in particular, a component that makes the Li ions contained in the glass exchange ions with the K ions in the molten salt to obtain a high surface compressive stress value. In addition, Li2O is a component that reduces high temperature viscosity and improves solubility and formability. Therefore, the suitable lower limit range of Li2O is 0% or more, 3% or more, 4% or more, 4.2% or more, 5% or more, 5.5% or more, 6.5% or more, 7% or more, 7.3% or more, 7.5% or more, 7.8% or more, and especially 8% or more in mole %. Therefore, the suitable upper limit range of Li2O is 20% or less, 15% or less, 13% or less, 12% or less, 11.5% or less, 11% or less, 10.5% or less, less than 10%, especially 9.9% or less, 9% or less, and 8.9% or less.
[0076] Na2O is an ion exchange component, and is a component that reduces high temperature viscosity, improves solubility and formability. In addition, Na2O is also a component that improves devitrification resistance and reaction devitrification with formed body refractory, especially alumina refractory. If the content of Na2O is too little, the solubility is reduced, or the thermal expansion coefficient is excessively reduced, or the ion exchange rate is easily reduced. Therefore, the suitable lower limit range of Na2O is 1% or more, 5% or more, 7% or more, 8% or more, 8.5% or more, 9% or more, 9.5% or more, 10% or more, 11% or more, 12% or more, and especially 12.5% or more in mole %. On the other hand, if the content of Na2O is too much, the viscosity is easily reduced due to phase separation. In addition, sometimes the acid resistance is reduced, or the component balance of the glass composition is lacking, and the devitrification resistance is reduced instead. Therefore, the suitable upper limit range of Na2O is 20% or less, 19.5% or less, 19% or less, 18% or less, 17% or less, 16.5% or less, 16% or less, 15.5% or less, and particularly 15% or less.
[0077] K2O is a component that reduces high temperature viscosity and improves solubility and formability. In addition, it is also a component that improves resistance to devitrification or increases Vickers hardness. However, if the content of K2O is too much, the viscosity is easily reduced due to phase separation. In addition, there is a tendency for reduced acid resistance or lack of component balance in the glass composition, which in turn reduces resistance to devitrification. Therefore, the suitable lower limit range of K2O is 0% or more, 0.01% or more, 0.02% or more, 0.1% or more, 0.5% or more, 1% or more, 1.5% or more, 2% or more, 2.5% or more, 3% or more, and especially 3.5% or more, and the suitable upper limit range is 10% or less, 5.5% or less, 5% or less, and especially less than 4.5%.
[0078] Li2O and Na2O are both components that exchange ions with K ions in molten salt to obtain high surface compressive stress values, and are components that require any one of them in the present invention. Therefore, the suitable lower limit range of Li2O+Na2O is 1% or more, 3% or more, 4% or more, 5% or more, 6% or more, 7% or more, 8% or more, 9% or more, 10% or more, 11% or more, 12% or more, 13% or more, 14% or more, 15% or more, 16% or more, 17% or more, 18% or more, and especially 18.5% or more in terms of mole %. On the other hand, if the content of Li2O+Na2O is too much, the thermal expansion coefficient becomes too high, and the thermal shock resistance is easily reduced. In addition, sometimes the components of the glass composition are unbalanced, but the resistance to devitrification is reduced. Therefore, the suitable upper limit range of Li2O+Na2O is less than 20%, especially less than 19%.
[0079] In addition to the above-mentioned components, the glass article 1 may contain, for example, the following components as a glass composition.
[0080] MgO is a component that reduces high temperature viscosity, improves solubility and formability, or increases strain point and Young's modulus. It is a component that has a great effect on improving ion exchange performance among alkaline earth metal oxides. However, if the content of MgO is too much, the density and thermal expansion coefficient are likely to increase, and the glass is prone to devitrification. Therefore, the upper limit range of MgO is less than 12%, less than 10%, less than 8%, less than 6%, and especially less than 5%. It should be noted that when MgO is introduced into the glass composition, the lower limit range of MgO is more than 0.1%, more than 0.5%, more than 1%, and especially more than 2% in mole%.
[0081] Compared with other components, CaO has a great effect of reducing high temperature viscosity, improving solubility and formability, or improving strain point and Young's modulus without reducing devitrification resistance. The content of CaO is preferably 0 to 10%. However, if the content of CaO is too much, the density and thermal expansion coefficient become high, and the component balance of the glass composition is lacking, and the glass is prone to devitrification and the ion exchange performance is prone to decrease. Therefore, the suitable content of CaO is 0 to 5%, 0.01 to 4%, 0.1 to 3%, and particularly 1 to 2.5% in mole %.
[0082] SrO is a component that reduces high temperature viscosity, improves solubility and formability, or increases strain point and Young's modulus without reducing devitrification resistance. However, if the SrO content is too high, the density and thermal expansion coefficient become higher, or the ion exchange performance is reduced, or the glass composition lacks a component balance, and the glass is prone to devitrification. The suitable content range of SrO is 0 to 5%, 0 to 3%, 0 to 1%, and particularly 0 to less than 0.1% in mole %.
[0083] BaO is a component that reduces high temperature viscosity, improves solubility and formability, or increases strain point and Young's modulus without reducing devitrification resistance. However, if the content of BaO is too much, the density and thermal expansion coefficient become higher, or the ion exchange performance is reduced, or the component balance of the glass composition is lacking, and the glass is prone to devitrification. The suitable content range of BaO is 0 to 5%, 0 to 3%, 0 to 1%, and particularly 0 to less than 0.1% in mole %.
[0084] ZnO is a component that improves ion exchange performance, and is particularly effective in increasing the compressive stress value. In addition, it is a component that does not reduce low-temperature viscosity but reduces high-temperature viscosity. However, if the ZnO content is too much, there is a tendency for glass phase separation, reduced devitrification resistance, increased density, or reduced stress depth of the compressive stress layer. Therefore, the ZnO content is preferably 0 to 6%, 0 to 5%, 0 to 1%, 0 to 0.5%, and particularly 0 to less than 0.1% in terms of mole %.
[0085] ZrO2 is a component that significantly improves ion exchange performance, and is a component that improves viscosity and strain points near liquidus viscosity, but if its content is too much, the resistance to devitrification may be significantly reduced, and the density may become too high. Therefore, the upper limit range of ZrO2 is 10% or less, 8% or less, 6% or less, and especially 5% or less in terms of mole %. It should be noted that when it is desired to improve ion exchange performance, it is preferred to introduce ZrO2 into the glass composition. In this case, the lower limit range of ZrO2 is 0.001% or more, 0.01% or more, 0.5%, and especially 1% or more.
[0086] P2O5 is a component that improves ion exchange performance, and in particular, increases the stress depth of the compressive stress layer. In addition, it is a component that suppresses the Young's modulus to a low level. However, if the content of P2O5 is too much, the glass is prone to phase separation. Therefore, the suitable upper limit range of P2O5 is, in terms of mole %, less than 10%, less than 8%, less than 6%, less than 4%, less than 2%, less than 1%, and in particular less than 0.1%.
[0087] As a clarifier, 0 to 30,000 ppm (3%) of one or more selected from the group consisting of As2O3, Sb2O3, SnO2, F, Cl, and SO3 (preferably the group consisting of SnO2, Cl, and SO3) may be introduced. From the viewpoint of reliably enjoying the clarification effect, the content of SnO2+SO3+Cl is preferably 0 to 10,000 ppm, 50 to 5,000 ppm, 80 to 4,000 ppm, 100 to 3,000 ppm, and particularly 300 to 3,000 ppm. Here, "SnO2+SO3+Cl" refers to the total amount of SnO2, SO3, and Cl.
[0088] The suitable content range of SnO2 is 0 to 10000 ppm, 0 to 7000 ppm, and particularly 50 to 6000 ppm. The suitable content range of Cl is 0 to 1500 ppm, 0 to 1200 ppm, 0 to 800 ppm, 0 to 500 ppm, and particularly 50 to 300 ppm. The suitable content range of SO3 is 0 to 1000 ppm, 0 to 800 ppm, and particularly 10 to 500 ppm.
[0089] Rare earth oxides such as Nd2O3 and La2O3 are components that increase the Young's modulus. In addition, if a complementary color is added, the color is reduced and the color tone of the glass can be controlled. However, the cost of the raw materials themselves is high, and if a large amount is introduced, the resistance to devitrification is easily reduced. Therefore, the content of rare earth oxides is preferably 4% or less, 3% or less, 2% or less, 1% or less, and particularly 0.5% or less.
[0090] From the perspective of environmental considerations, the glass article 1 preferably does not substantially contain As2O3, F, PbO, and Bi2O3. Here, "substantially does not contain As2O3" means that although As2O3 is not actively added as a glass component, it is allowed to be mixed at an impurity level. Specifically, it means that the content of As2O3 is less than 500ppm. "Substantially does not contain F" means that although F is not actively added as a glass component, it is allowed to be mixed at an impurity level. Specifically, it means that the content of F is less than 500ppm. "Substantially does not contain PbO" means that although PbO is not actively added as a glass component, it is allowed to be mixed at an impurity level. Specifically, it means that the content of PbO is less than 500ppm. "Substantially does not contain Bi2O3" means that although Bi2O3 is not actively added as a glass component, it is allowed to be mixed at an impurity level. Specifically, it means that the content of Bi2O3 is less than 500ppm.
[0091] As an example, the glass article 1 may not contain B2O3 as a glass composition, or the content of B2O3 may be limited to a very small amount. That is, the glass article 1 may contain 50 to 80% SiO2, 5 to 25% Al2O3, 0 to 1% B2O3, 0 to 20% Li2O, 1 to 20% Na2O, and 0 to 10% K2O as a glass composition in terms of mol%.
[0092] As another example, the glass article 1 may contain B2O3 as an essential component as a glass composition. That is, the glass article 1 may contain 50 to 80% of SiO2, 5 to 25% of Al2O3, 1 to 5% of B2O3, 0 to 20% of Li2O, 1 to 20% of Na2O, and 0 to 10% of K2O as a glass composition in terms of mol%.
[0093] It should be noted that, when the glass article 1 contains B2O3 as an essential component as a glass composition, there is a concern that the formability of the glass may be reduced, so in order to achieve a balance, for example, the content of other components such as A12O3 may be limited. That is, the glass article 1 may contain 50 to 80% of SiO2, 5 to 10% of A12O3, 1 to 5% of B2O3, 0 to 20% of Li2O, 1 to 20% of Na2O, and 0 to 10% of K2O as a glass composition in terms of mol%.
[0094] <Method for manufacturing glass article>
[0095] like Figure 3 As shown, the method for producing a glass article according to the first embodiment includes a preparation step S1 , a chemical strengthening step S2 , and a water treatment step S3 in this order.
[0096] In the preparation step S1, glass (hereinafter referred to as process glass) serving as a base of the glass article 1 is prepared. The process glass is glass having the same shape, size and glass composition as the glass article 1.
[0097] The process glass is obtained, for example, by cutting and processing a plate-shaped or sheet-shaped mother glass obtained by a forming method such as an overflow down-draw method, a flow hole down-draw method, a float method, a re-draw method, etc. into small pieces of glass. In order to obtain a smooth surface, the overflow down-draw method is preferably used as a forming method. In addition, if the overflow down-draw method is used, even if grinding (including mechanical grinding and etching) is not performed after forming, it is easy to form a process glass with a thickness of 0.005 to 0.1 mm. It should be noted that when forming by the overflow down-draw method, the process glass has a forming confluence surface inside.
[0098] The end face of the processing glass is preferably chamfered or treated to improve strength by grinding, heat treatment, etching, etc. The main surface of the processing glass can be ground, but when the main surface is pre-formed smoothly by the overflow down-draw method, or when the thickness is uniform and the shape is formed with good precision, the main surface may not be ground, that is, the non-ground surface is directly used. It should be noted that when the main surface is formed by the overflow down-draw method and is not ground, the main surface of the processing glass becomes a fire-polished surface.
[0099] In the chemical strengthening step S2, the processing glass is subjected to ion exchange treatment. In this embodiment, the processing glass is immersed in a molten salt for ion exchange treatment. By using ion exchange treatment to make the processing glass into chemically strengthened glass, the bending strength of the processing glass is improved.
[0100] Molten salt is a salt containing a component that can exchange ions with the components in the chemically strengthened glass, typically an alkali metal nitrate. As alkali metal nitrates, NaNO3, KNO3, LiNO3, etc. can be cited, and they can be used alone (100% by mass) or in a mixture of multiple types. The mixing ratio when mixing multiple alkali metal nitrates can be determined arbitrarily, for example, in terms of mass%, it can be 5-95% for NaNO3 and 5-95% for KNO3, preferably 30-80% for NaNO3 and 20-70% for KNO3, and more preferably 50-70% for NaNO3 and 30-50% for KNO3.
[0101] The temperature of the molten salt is, for example, 350° C. to 500° C., preferably 355° C. to 470° C., 360° C. to 450° C., 365° C. to 430° C., or 370° C. to 410° C. In addition, the immersion time is, for example, 3 to 300 minutes, preferably 5 to 120 minutes, or 7 to 100 minutes. Of course, the conditions such as the temperature and immersion time of the molten salt can be appropriately changed according to the glass composition, etc. within the range of obtaining the above-mentioned stress characteristics.
[0102] In the water treatment process S3, the treatment glass is contacted with the treatment water for more than 0.5 hours and less than 15 hours. By contacting the treatment glass with the treatment water in this way, the pen-falling strength of the treatment glass is improved. In addition, since the pen-falling strength of the treatment glass is also maintained after the water treatment process S3, the pen-falling strength of the glass article 1 manufactured by the treatment glass is also improved. It should be noted that the contact time between the treatment glass and the treatment water (hereinafter referred to as the water treatment time) is too short or too long to fully enjoy the pen-falling strength improvement effect. Therefore, it is important that the water treatment time is set within the above-mentioned numerical range.
[0103] The lower limit of the water treatment time is preferably 0.75 hours or more, 1 hour or more, 1.25 hours or more, or 1.5 hours or more, and the upper limit of the water treatment time is preferably 14 hours or less, 13 hours or less, 12 hours or less, or 11 hours or less.
[0104] The temperature of the treated water is, for example, 10 to 100° C. The lower limit of the temperature of the treated water is preferably 20° C. or higher, 30° C. or higher, 40° C. or higher, or 46° C. or higher. The upper limit of the temperature of the treated water is preferably 95° C. or lower, 90° C. or lower, or 85° C. or lower. As the temperature of the treated water increases, the treatment time until the desired pen-fall strength is obtained tends to be shorter.
[0105] When the treatment glass is chemically strengthened glass, in the water treatment step S3, the temperature of the treatment water is preferably 50 to 95°C and the water treatment time is preferably 0.5 to 10 hours.
[0106] The conductivity of the treated water is preferably 3 mS / m or less. The conductivity of the treated water is more preferably 1 mS / m or less, 0.1 mS / m or less, or 0.01 mS / m or less. As the conductivity of the treated water decreases, the pen-fall strength of the treated glass is easily improved. The treated water preferably does not contain lotions and their materials (e.g., surfactants, water softeners, metal chelating agents (Japanese original text: metal blockers), pH adjusters, stabilizers), etc.
[0107] An example of an embodiment of the water treatment step S3 is shown in Figure 4 .like Figure 4As shown, the treatment glass 6 is immersed in the treatment water 5 stored in the container 4. In the treatment water 5, for example, a plurality of treatment glasses 6 are supported by a support table 7 at predetermined intervals in the thickness direction in a vertical posture. Then, the container 4 containing the treatment glass 6 and the treatment water 5 is placed in a constant temperature device (temperature adjustment device) 8 maintained at a predetermined temperature for a predetermined time, and the treatment glass 6 is subjected to water treatment.
[0108] The method of contacting the treatment water with the treatment glass is not particularly limited, and it is preferred to adopt the method of immersing the treatment glass in the treatment water stored in the container as described above. At this time, it is preferred not to give the treatment water external vibrations such as ultrasound, and to leave the treatment glass still in the treatment water. If immersed in the treatment water like this, the entire treatment glass can be efficiently contacted with the treatment water, and it is easy to enjoy the effect of improving the pen-falling strength. It should be noted that, for the treatment water, the treatment glass can be sprayed from a nozzle, etc., or running water can be made to flow over the entire surface of the treatment glass.
[0109] The treatment glass can be moved relative to the treatment water. Specifically, for example, the treatment glass immersed in the treatment water can be moved in the treatment water, or the treatment glass can be moved in an area where the treatment water is sprayed and supplied by a nozzle or the like.
[0110] (Second Embodiment)
[0111] <Laminate>
[0112] like Figure 5 As shown, the laminated body 9 of the second embodiment includes: the above-mentioned glass article 1; a protective layer 10a laminated on one main surface 1a (e.g., the surface) of the glass article 1; and a reinforcing layer 10b laminated on the other main surface 1a (e.g., the back surface) of the glass article. In this way, the glass article 1 is protected by the protective layer 10a, so that a higher pen-falling strength can be achieved. In addition, the reinforcing layer 10b can improve the bending strength of the glass article 1 and suppress breakage during bending. It is preferred that the protective layer 10a is provided on the surface side of the glass article 1 that is in contact with a pen or the like, and the reinforcing layer 10b is provided on the back side of the glass article 1 that is not in contact with a pen or the like. It should be noted that only one of the protective layer 10a and the reinforcing layer 10b may be provided.
[0113] As the protective layer 10a and the reinforcing layer 10b, plate-shaped or sheet-shaped resins, metals, glass, etc. can be cited, and they can be formed as a single layer or a combination of multiple layers. However, when the laminate 9 is applied to a foldable device, the protective layer 10a and the reinforcing layer 10b are preferably resins that are easy to impart flexibility.
[0114] The thickness of the resin contained in the protective layer 10a and the reinforcing layer 10b is preferably 0.5 to 200 μm, 1 to 150 μm, or 2 to 100 μm. Examples of the material of the resin contained in the protective layer 10 include polycarbonate (PC), acrylic resin, polyethylene terephthalate (PET), polyetheretherketone (PEEK), polyamide (PA), polyvinyl chloride (PVC), polyethylene (PE), polypropylene (PP), polyethylene naphthalate (PEN), polyimide (PI), cycloolefin polymer (COP), and epoxy resin.
[0115] The protective layer 10a and the reinforcing layer 10b are laminated on the main surface 1a of the glass article 1, for example, by means of an adhesive layer 11. The thickness of the adhesive layer 11 is preferably 0.1 to 100 μm, 0.2 to 90 μm, or 0.3 to 80 μm. As the material of the adhesive layer 11, for example, acrylic adhesives, silicone adhesives, rubber adhesives, UV-curable acrylic adhesives, UV-curable epoxy adhesives, thermosetting epoxy adhesives, thermosetting melamine adhesives, thermosetting phenol adhesives, ethylene vinyl acetate (EVA), polyvinyl butyral (PVB), cycloolefin polymer (COP), etc. It should be noted that the protective layer 10 can also be directly formed on the main surface 1a of the glass article 1 by any method such as coating without the aid of the adhesive layer 11.
[0116] (Third Embodiment)
[0117] <Method for manufacturing glass article>
[0118] like Figure 6 As shown, the manufacturing method of the glass article of the third embodiment sequentially comprises a preparation step S11, a chemical strengthening step S12, a surface etching step S13 and a water treatment step S14. Among them, the steps other than the surface etching step S13 are the same as the corresponding steps of the above-mentioned embodiment, so detailed description is omitted.
[0119] The surface etching step S13 is a step of etching the processing glass in a range shallower than the compressive stress layer after the chemical strengthening step S12 and before the water treatment step S14. By performing the surface etching step S13 in this way, surface defects formed on the processing glass in the chemical strengthening step S12 and the like can be reduced. Therefore, the pen-falling strength and / or bending strength of the processing glass and the glass article can be improved.
[0120] In the surface etching step S13, for example, the entire processing glass is immersed in a liquid etching medium, and the entire surface of the processing glass is wet-etched. By such a treatment, the entire processing glass can be etched uniformly, so the thickness deviation caused by the etching treatment can be suppressed. When such an etching treatment is performed, the surface of the processing glass is composed of an etched surface.
[0121] As the etching medium, an acidic or alkaline aqueous solution capable of etching glass can be used.
[0122] As the acidic etching medium, for example, an acidic aqueous solution containing HF can be used. When an aqueous solution containing HF is used, the etching rate of glass is high and the production efficiency is good.
[0123] The aqueous solution containing HF is, for example, an aqueous solution containing only HF, or containing HF and HCl, HF and HNO3, HF and H2SO4, HF and NH4F in combination. The concentration of each compound of HF, HCl, HNO3, H2SO4, and NH4F is preferably 0.1 to 30 mol / L. In etching using an aqueous solution containing HF, fluoride containing glass components is generated as a by-product, which may become an important cause of a decrease in etching rate and defects, but as described above, by making a mixed acid with other acids such as HCl, HNO3 or H2SO4, the by-product can be decomposed to suppress a decrease in productivity. When etching is performed using an acidic aqueous solution, it is preferred that the temperature of the acidic aqueous solution is, for example, 10 to 30°C, and the time for immersing the glass for treatment is, for example, 0.1 to 60 minutes.
[0124] As an alkaline etching medium, an alkaline aqueous solution containing NaOH or KOH can be used. Compared with the above-mentioned etching medium containing HF, the alkaline aqueous solution has a lower etching rate for glass, so it has the advantage of being easy to precisely control the etching amount. It is particularly suitable when it is necessary to control the thickness of the glass, DOC, etc. in units of several μm.
[0125] In the aqueous solution containing NaOH or KOH, the concentration of the alkali component is preferably 1 to 20 mol / L. When etching is performed using an aqueous alkali solution, the temperature of the aqueous alkali solution is preferably, for example, 10 to 130°C, and the time for immersing the glass for treatment is, for example, 0.5 to 120 minutes. It should be noted that in the case of increasing the etching rate to increase productivity, it is preferred to heat the temperature of the aqueous alkali solution to above 80°C. On the contrary, in the case of wanting to control the etching amount with higher precision, it is preferred to limit the temperature of the aqueous alkali solution to below 70°C. In addition, in the case where more attention is paid to the size of the etching rate, it is preferred to use an aqueous solution of NaOH.
[0126] The thickness of the surface layer of the processing glass removed in the surface etching step S13 is preferably 0.25 μm to 3 μm. The thickness of the surface layer of the processing glass removed is more preferably 0.4 μm to 2.7 μm, 0.6 μm to 2.5 μm, or 0.8 μm to 2.3 μm. By setting the etching amount to such a range, the maximum compressive stress before and after etching and the variation of the compressive stress depth can be reduced.
[0127] The glass article manufactured by the surface etching step S13 preferably has the entire surface, that is, the two main surfaces and the end surfaces of the front and back surfaces, all composed of etching surfaces. Thus, defects are reduced on the entire surface of the glass article, and high strength, especially high pen-holding strength, can be achieved.
[0128] (Fourth Embodiment)
[0129] <Method for manufacturing glass article>
[0130] like Figure 7 As shown, the manufacturing method of the glass article of the fourth embodiment sequentially comprises a preparation step S21, a thinning step S22, a chemical strengthening step S23, a surface etching step S24 and a water treatment step S25. Among them, the steps other than the thinning step S22 are the same as the corresponding steps of the above-mentioned embodiment, so the detailed description is omitted. It should be noted that the surface etching step S24 may not be provided.
[0131] The thinning step S22 is a step of thinning the thickness of the process glass to a range of 0.005 to 0.1 mm by etching. By performing the thinning step S22 in this way, even if a thick process glass is prepared in the preparation step S21, the thickness of the process glass can be thinned to an appropriate range.
[0132] In the thinning step S22, for example, the entire surface of the processing glass is wet-etched by immersing the entire processing glass in a liquid etching medium. As the etching medium, the same etching medium as used in the surface etching step S24 can be used.
[0133] The thickness of the surface layer of the processing glass removed in the thinning step S22 depends on the original thickness (initial thickness) of the processing glass before the thinning step S22, so it is not specifically limited, but sometimes it is greater than the thickness of the surface layer of the processing glass removed in the surface etching step S24.
[0134] (Fifth Embodiment)
[0135] <Method for manufacturing glass article>
[0136] like Figure 8As shown, the manufacturing method of the glass article of the fifth embodiment sequentially comprises a preparation step S31, a thinning step S32 and a water treatment step S33. Each step is the same as the corresponding step of the above embodiment, except that the present embodiment does not comprise a chemical strengthening step.
[0137] By such a manufacturing method, in the water treatment process S33, the unreinforced treatment glass is in contact with the treatment water. In this case, compared with the case where the chemically strengthened treatment glass is in contact with the treatment water, the pen-fall strength of the treatment glass tends to be higher. Therefore, even in the glass article manufactured by the water treatment process S33 in which the unreinforced treatment glass is in contact with the treatment water, a high pen-fall strength can be obtained. That is, in the present invention, the glass article is not limited to chemically strengthened glass. However, with respect to bending strength, there is a tendency for chemically strengthened glass articles to become higher. Therefore, from the viewpoint of taking into account both pen-fall strength and bending strength, the glass article is preferably chemically strengthened glass.
[0138] In the present embodiment, the case where the thinning step S32 is provided is exemplified, but in the preparation step S31, when the process glass preformed to a thickness of 0.005 to 0.1 mm by the overflow down-draw method or the like can be prepared, the thinning step S32 may not be provided.
[0139] (Sixth Embodiment)
[0140] <Method for manufacturing glass article>
[0141] In the sixth embodiment, a method for producing a glass article shows a modification of the water treatment step in the above embodiment. In the above embodiment, the temperature of the treated water in the water treatment step is 100° C. or less, but in this embodiment, the temperature of the treated water is set to 100° C. or more.
[0142] As an example of the water treatment process of this embodiment, the treatment glass is immersed in treatment water reaching 100°C or above under a pressurized atmosphere. Specifically, the treatment glass is immersed in treatment water stored in a container. Then, while the container is stored in a pressurizing device, the pressurizing device is pressurized to heat the treatment water to 100°C or above. By setting the treatment water to 100°C or above, it is expected that the water treatment time until the desired pen-fall strength is obtained can be shortened.
[0143] The temperature of the treated water is preferably higher than 100° C. and lower than 200° C. The lower limit of the treated water temperature is more preferably higher than 105° C., higher than 110° C., or higher than 120° C. The upper limit of the treated water temperature is more preferably lower than 190° C., lower than 180° C., or lower than 170° C.
[0144] The pressure of the pressurized atmosphere is preferably 0.15 to 2.0 MPa. The lower limit of the pressure of the pressurized atmosphere is more preferably 0.17 MPa or more, 0.2 MPa or more, or 0.25 MPa or more. The upper limit of the pressure of the pressurized atmosphere is more preferably 1.9 MPa or less, 1.8 MPa or less, or 1.7 MPa or less.
[0145] The lower limit of the water treatment time is preferably 0.6 hours or more, 0.75 hours or more, or 1 hour or more, and the upper limit of the water treatment time is preferably 12 hours or less, 11 hours or less, or 10 hours or less.
[0146] Instead of immersing the treatment glass in treatment water at 100° C. or higher, the treatment water may be sprayed onto the treatment glass in the form of superheated water vapor at 100° C. or higher.
[0147] It should be noted that although the embodiments of the present invention have been described, the embodiments of the present invention are not limited thereto, and various modifications can be made without departing from the gist of the present invention.
[0148] In the above-mentioned embodiment, the shape of the glass article is not particularly limited. The shape of the glass article can be, for example, square, rectangular, circular, oval, etc. in a plan view.
[0149] In the above-mentioned embodiment, the glass article can be three-dimensionally bent as needed. Specifically, by preliminarily performing three-dimensional bending on the entire or part of the treatment glass, a three-dimensional curved shape can be given to the finally manufactured glass article.
[0150] In the above-mentioned embodiment, the case of performing one chemical strengthening process (ion exchange treatment) is illustrated, but the chemical strengthening process can also be performed 2 or 3 times or more. In addition, heat treatment can also be performed before and after the ion exchange. By heat treatment, stress relaxation, ion diffusion promotion and control of the depth of the compressive stress layer can be performed. In the case of performing a chemical strengthening process, it is preferred to clean and dry the treatment glass after the chemical strengthening process and before the water treatment process. It should be noted that, in the case of implementing multiple chemical strengthening as described above, for the stress distribution of the strengthened glass article, in the region of the compressive stress layer 2, there can be at least one of more than one bending point (Japanese original: buckling point), maximum value, minimum value or inflection point (Japanese original: inflection point).
[0151] In the above-mentioned embodiment, the tensile stress in the tensile stress layer 3 may be non-constant in the thickness direction. For example, when the DOC is set larger relative to the thickness t of the glass article (for example, when DOC≥0.20t), the stress distribution in the tensile stress layer 3 may be set to a distribution shape of a downwardly convex quadratic curve having a minimum value at the center of the thickness of the glass article.
[0152] In the above embodiment, the stress distribution of the glass article may be asymmetric between the front and back surfaces. The asymmetric stress distribution between the front and back surfaces is obtained by grinding one main surface side of the strengthened glass article more than the other surface, or chemically strengthening the glass article while providing a film that inhibits ion exchange on one main surface side.
[0153] [Example]
[0154] Hereinafter, the glass article of the present invention will be described based on Examples. It should be noted that the following Examples are merely illustrative, and the present invention is not limited to the following Examples at all.
[0155] The samples were prepared as follows: First, treatment glass having the glass composition shown in Table 1 was prepared. It should be noted that the Young's modulus shown in Table 1 is a value measured by a resonance method.
[0156] [Table 1]
[0157] (mol%) A B <![CDATA[SiO2]]> 66.4 69.9 <![CDATA[Al2O3]]> 11.5 8,67 MgO 4.8 4.7 CaO 0.1 0.1 <![CDATA[B2O3]]> 0.5 2.3 Zn-O - - <![CDATA[ZrO2]]> - - <![CDATA[Li2O]]> 0.02 0.03 <![CDATA[Na2O]]> 15.2 13.7 <![CDATA[K2O]]> 1.4 0.45 <![CDATA[P2O5]]> - - <![CDATA[SnO2]]> 0.1 0,15 Young's modulus(GPa) 72.1 70.1
[0158] Specifically, glass raw materials were blended to have the composition shown in Table 1 and melted in a test melting furnace. The obtained molten glass was then formed into a plate or sheet by an overflow down-draw method and cut into a predetermined size to obtain process glass.
[0159] Next, the plate-shaped or sheet-shaped processing glass is treated under the conditions described in Tables 2 to 8, thereby manufacturing plate-shaped or sheet-shaped glass articles. The thinning process and the surface etching process are performed by immersing the processing glass in an HF aqueous solution. The chemical strengthening process is performed by immersing the processing glass in a molten salt of 100% KNO3. The water treatment process is performed by immersing the processing glass in treated water. In Tables 2 to 8, No. 1 to 29 are embodiments of the present invention, and No. 30 to 45 are comparative examples.
[0160] [Table 2]
[0161]
[0162] [Table 3]
[0163]
[0164] [Table 4]
[0165]
[0166] [Table 5]
[0167]
[0168] [Table 6]
[0169]
[0170] [Table 7]
[0171]
[0172] [Table 8]
[0173]
[0174] <Method for producing glass article or laminate>
[0175] (1) In No. 1 to 6 in Table 2, the treatment glass was subjected to a water treatment process to manufacture glass articles. In No. 7 to 8 in Table 2, the treatment glass was subjected to a thinning process and a water treatment process in sequence to manufacture glass articles. That is, in No. 1 to 8 in Table 2, the treatment glass was not subjected to a chemical strengthening process. It should be noted that in No. 1 to 6, the initial thickness of the treatment glass was consistent with the thickness of the glass article, and in No. 7 to 8, the thickness of the treatment glass after the thinning process was consistent with the thickness of the glass article.
[0176] (2) In No. 9 to 14 in Table 3, the glass for treatment was subjected to a chemical strengthening step and a water treatment step in sequence to produce glass articles. In No. 15 to 16 in Table 3, the glass for treatment was subjected to a thinning step, a chemical strengthening step, and a water treatment step in sequence to produce glass articles. It should be noted that in No. 9 to 14, the initial thickness of the glass for treatment was consistent with the thickness of the glass article, and in No. 15 to 16, the thickness of the glass for treatment after the thinning step was consistent with the thickness of the glass article.
[0177] (3) In No. 17 to 24 in Table 4, the treatment glass was subjected to a chemical strengthening step, a surface etching step, and a water treatment step in order to produce a glass article. It should be noted that in No. 17 to 24, the thickness of the treatment glass after the surface etching step was consistent with the thickness of the glass article.
[0178] (4) In No. 25 to 26 of Table 5, the glass for treatment is subjected to a thinning process, a chemical strengthening process, a surface etching process, and a water treatment process in sequence to manufacture glass articles. In No. 27 to 29 of Table 5, the glass for treatment is subjected to a chemical strengthening process, a surface etching process, and a water treatment process in sequence to manufacture glass articles. In addition, in No. 27 to 29 of Table 5, a protective layer (PET film, PA film, PI coating layer) is laminated on one main surface of the glass article to manufacture a laminate. The PET film and the PA film are bonded to the glass article by means of a pressure-sensitive adhesive (PSA) sheet having a thickness of 5 μm. The PI coating layer is formed by coating PI on the main surface of the glass article. It should be noted that in No. 25 to 29, the thickness of the glass for treatment after the surface etching process is consistent with the thickness of the glass article.
[0179] (5) In No. 30 and 31 of Table 6, the treatment glass is directly used as a glass article in an untreated state. In No. 32 and 33 of Table 6, the treatment glass is subjected to a thinning process to manufacture glass articles. In No. 34 and 35 of Table 6, the treatment glass is subjected to a chemical strengthening process to manufacture glass articles. In No. 36 and 37 of Table 6, a thinning process and a chemical strengthening process are sequentially performed to manufacture glass articles. That is, in No. 30 to 33 of Table 6, the treatment glass is not subjected to a chemical strengthening process and a water treatment process. In No. 34 to 37 of Table 6, the treatment glass is not subjected to a water treatment process. It should be noted that in No. 30, 31, 34, and 35, the initial thickness of the treatment glass is consistent with the thickness of the glass article. In No. 32, 33, 36, and 37, the thickness of the treatment glass after the thinning process is consistent with the thickness of the glass article.
[0180] (6) In No. 38 to 39 of Table 7, the glass for treatment was subjected to a chemical strengthening step and a surface etching step in sequence to produce glass articles. In No. 40 to 41 of Table 7, the glass for treatment was subjected to a thinning step, a chemical strengthening step, and a surface etching step in sequence to produce glass articles. That is, in No. 38 to 41 of Table 7, the glass for treatment was not subjected to a water treatment step. It should be noted that in No. 38 to 41, the thickness of the glass for treatment after the surface etching step was consistent with the thickness of the glass article.
[0181] (7) In No. 42 to No. 45 of Table 8, the glass for treatment was subjected to a chemical strengthening step, a surface etching step, and a water treatment step in sequence to manufacture glass articles. It should be noted that in No. 42 to No. 45, the thickness of the glass for treatment after the surface etching step was consistent with the thickness of the glass article. It should be noted that in No. 42 to No. 45, the glass for treatment was subjected to a water treatment step, but the water treatment time was less than 0.5 hours or more than 15 hours.
[0182] In some examples and comparative examples in which a chemical strengthening process was performed, CS, DOC, and CT of the glass articles were measured. CS, DOC, and CT in Tables 1 to 8 are values obtained by measuring each glass article (sample) using a surface stress meter FSM-6000LE manufactured by Orihara Seisakusho.
[0183] <Pen drop test>
[0184] like Fig. 9 As shown, in the pen drop test, the tip of a ballpoint pen 18 is dropped onto a measurement sample 12 to evaluate the strength (pen drop strength) of a glass article 13 included in the measurement sample 12 .
[0185] In the pen-drop tests of No. 1 to 26 and 30 to 45, a sample in which a glass article 13, a PSA sheet 14, a PET plate 15, a PSA sheet 16, and a SUS plate 17 are stacked in this order is prepared as the measurement sample 12. On the other hand, in the pen-drop tests of No. 27 to 29, a protective layer (PET film, PA film, PI coating layer) is further provided on the upper surface of the glass article 13 in the above-mentioned measurement sample 12. That is, in the pen-drop tests of No. 1 to 26 and 30 to 45, the tip of the ballpoint pen 18 is in direct contact with the glass article 13, and in the pen-drop tests of No. 27 to 29, the tip of the ballpoint pen 18 is in direct contact with the protective layer.
[0186] The top view dimensions of the glass article 13, PSA sheets 14, 16, PET plate 15 and protective layer are set to 50 mm × 50 mm, respectively. The top view dimensions of the SUS plate 17 are set to 55 mm × 55 mm. The thicknesses of the glass article 13 and the protective layer are as shown in Tables 2 to 8. The thickness of the PSA sheets 14, 16 is set to 50 μm. The thickness of the PET plate 15 is set to 125 μm. The thickness of the SUS plate 17 is set to 3 mm.
[0187] In the pen drop test, five samples 12 of No. 1 to 45 were prepared, and the tip of the ballpoint pen 18 was dropped to the center of each sample 12. At this time, the tip of the ballpoint pen 18 was dropped to the sample 12 through the inner hole of the vertically held guide tube 19 in such a manner that the tip of the ballpoint pen 18 dropped vertically relative to the sample 12. The ballpoint pen 18 was Orange EG0.7 manufactured by BIC, with a ball diameter of 0.7 mm and a mass of 5.7 g. The height of the tip of the pen before dropping based on the upper surface of the sample 12 was set as the drop height H, and the initial value was set to 1 cm before dropping. When the glass article 13 contained in the sample 12 was not broken by the drop of the ballpoint pen 18, the height was raised by 1 cm and dropped again. As described above, the increase and drop of the drop height H were repeated until the glass article 13 contained in the sample 12 was broken. Then, as the pen drop strength, the 60% breakage height (Japanese original text: breakage height さ) and the maximum breakage height are calculated. The 60% breakage height is the drop height H when the glass articles 13 included in three of the five measurement samples 12 are broken. The maximum breakage height is the drop height H when all the glass articles 13 included in the five measurement samples 12 are broken.
[0188] The results of the pen drop test confirmed that the Examples (Nos. 1 to 29) that performed an appropriate water treatment process had a 60% higher damage height than the Comparative Examples (Nos. 30 to 45) that did not perform any water treatment process or did not perform an appropriate water treatment process.
[0189] <Bending failure test>
[0190] like Fig.10 As shown, in the bending failure test, the test sample 20 composed of a glass article is clamped by two plate-like bodies 21, and the strength (two-point bending strength) is evaluated by so-called two-point bending in which the test sample 20 is bent in a U-shaped manner. The two-point bending strength is evaluated only for No. 2, 10, 18, 30, 34, and 38, and 30 test samples 20 corresponding to these glass articles are prepared respectively. The top view size of the test sample 20 is set to 140 mm × 70 mm. The thickness of the test sample 20 is set to 50 μm in No. 2, 10, 30, and 34, and to 47 μm in No. 18 and 38, as described in Tables 2 to 8. Then, the test sample 20 is arranged between the plate-like bodies 21 in a manner of bending into a U-shape along the long side (140 mm side).
[0191] For the two-point bending strength, the interval D between the two plate-like bodies 21 when the glass article 20 is broken by bending is used and calculated by the following formula (4). Then, as the two-point bending strength, the central value, maximum value, and minimum value are calculated. The central value of the two-point bending strength is the central value when the two-point bending strength data of 30 measured samples are arranged in order of size. The maximum value of the two-point bending strength is the maximum value among the two-point bending strengths of the 30 measured samples. The minimum value of the two-point bending strength is the minimum value among the two-point bending strengths of the 30 measured samples.
[0192] σ=1.198[E×t / (Dt)] (4)
[0193] Wherein, σ represents the two-point bending strength [MPa], E represents the Young's modulus of the glass article [MPa], and t represents the thickness of the glass article [mm].
[0194] According to the results of the bending failure test, it was confirmed that the two-point bending strength of the chemically strengthened glass articles (No. 10, 18, 34, 38) was improved compared with the glass articles (No. 2, 30) that were not chemically strengthened. In particular, in the glass articles (No. 18, 38) that were subjected to a surface etching process after chemical strengthening, it was confirmed that the two-point bending strength was greatly improved. Therefore, it can be seen that from the viewpoint of simultaneously improving the pen-fall strength and the two-point bending strength of the glass article, it is preferable to perform not only the chemical strengthening process but also an appropriate water treatment process thereafter.
[0195] Industrial Applicability
[0196] The glass article of the present invention can be used, for example, for smartphones, mobile phones, tablet computers, personal computers, digital cameras, touch panel displays, cover glasses of other display devices, vehicle-mounted display devices, vehicle-mounted panels, and the like.
[0197] Description of Reference Numerals
[0198] 1 Glass Item
[0199] 2 Compressive stress layer
[0200] 3 Tensile stress layer
[0201] 4 Container
[0202] 5. Treat water
[0203] 6. Processing glass
[0204] 7 Support table
[0205] 8 Constant temperature device
[0206] 9 Laminated body
[0207] 10a Protective layer
[0208] 10b Enhancement Layer
[0209] 11 Adhesive layer
[0210] 12 Measurement samples
[0211] 13 Glass objects
[0212] 14 PSA sheet
[0213] 15 PET board
[0214] 16 PSA sheet
[0215] 17 SUS plate
[0216] 18. Ballpoint pen
[0217] 19 Guide tube
[0218] 20 Measurement sample (glass object)
[0219] 21 plate-shaped body
Claims
1. A method for manufacturing a glass article, comprising: a preparation step of preparing a processing glass composed of an alkali-aluminosilicate glass containing an alkali metal oxide as a glass composition; and In the water treatment step, the treatment glass is brought into contact with treatment water for a period of 0.5 hours or more and less than 15 hours.
2. The method for manufacturing a glass article according to claim 1, wherein: In the water treatment step, the treatment glass is immersed in the treatment water at 46° C. to 100° C.
3. The method for manufacturing a glass article according to claim 1, wherein: In the water treatment step, the treatment glass is immersed in the treatment water adjusted to 100° C. or higher under a pressurized atmosphere.
4. The method for producing a glass article according to any one of claims 1 to 3, wherein: In the water treatment step, the conductivity of the treated water is 3 mS / m or less.
5. The method for producing a glass article according to any one of claims 1 to 4, wherein: The processing glass is in the form of a plate or sheet with a thickness of 0.005 mm to 0.1 mm.
6. The method for manufacturing a glass article according to claim 5, wherein: A thinning step is further provided before the water treatment step, and in the thinning step, the processing glass is thinned to be within the thickness range by etching.
7. The method for manufacturing a glass article according to claim 5, wherein: The process glass is preformed within the thickness range by an overflow down-draw method.
8. The method for producing a glass article according to any one of claims 1 to 7, wherein: A chemical strengthening step is further provided before the water treatment step. In the chemical strengthening step, the processing glass is brought into contact with an alkali metal nitrate to form a compressive stress layer having a maximum compressive stress of 100 MPa or more on the surface.
9. The method for manufacturing a glass article according to claim 8, wherein: In the water treatment step, the temperature of the treatment water is 50° C. to 95° C., and the contact time between the treatment glass and the treatment water is 0.5 hour to 10 hours.
10. The method for manufacturing a glass article according to claim 8 or 9, wherein: The treatment glass comprises, in mole percent, 50% to 80% SiO2, 5% to 25% Al2O3, 0% to 35% B2O3, 0% to 20% Li2O, 1% to 20% Na2O, and 0% to 10% K2O as a glass composition, In the chemical strengthening step, the alkali metal nitrate is a molten salt containing potassium nitrate.
11. The method for producing a glass article according to any one of claims 8 to 10, wherein: A surface etching step is further provided after the chemical strengthening step and before the water treatment step. In the surface etching step, the processing glass is etched in a range shallower than the compressive stress layer.
12. A glass article, which is a plate-shaped or sheet-shaped glass article with a thickness of 0.005 mm to 0.1 mm, In a pen drop test in which a 5.7 g ballpoint pen having a spherical tip with a diameter of 0.7 mm was dropped onto the main surface, the 60% destruction height was 5 cm or more. 13 . The glass article according to claim 12 , comprising a compressive stress layer having a maximum compressive stress of 100 MPa or more on the surface.
14. A laminate comprising: The glass article of claim 12 or 13; and A protective layer or a reinforcing layer laminated to at least one major surface of the glass article.
Citation Information
Patent Citations
Display cover glass and display cover glass fabrication method
WO2013088856A1
Aluminosilicate glass, antibacterial glass and preparation method thereof
CN107434354A
Method for manufacturing substrate for information recording medium, substrate for information recording medium and information recording medium
JP2003030828A
Method for producing chemical strengthened glass
JP2016216330A