Ceramic structure
By introducing intermediate layers and metallized layers with different ceramic materials into the ceramic structure, the problem of insufficient adhesion between the ceramic matrix and the metallized layer is solved, the adhesion and mechanical properties of the ceramic structure are improved, and the thermal expansion is reduced peeling phenomenon.
Patent Information
- Application Number
- CN202380027366.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-28
- Filing Date
- 2023-03-28
- Publication Date
- 2024-11-01
AI Technical Summary
In the existing ceramic structure, the adhesion between the ceramic matrix and the metallized layer is insufficient, and it is difficult to further improve.
An intermediate layer is introduced into the ceramic structure, which is composed of ceramic materials different from the ceramic substrate and forms a metallization layer on its surface. By adjusting the thickness and constituent elements of the intermediate layer, it increases the between the ceramic substrate and the metallization layer by adjusting the thickness and constituent elements of the intermediate layer. The adhesion of
By increasing the concave and convex structure of the intermediate layer, the anchoring effect and adhesion between the ceramic matrix and the metallized layer are improved, the bonding strength is enhanced, and the peeling phenomenon caused by thermal expansion is reduced, thereby achieving high adhesion and excellent ceramic structure. Mechanical properties.
Smart Images

Figure CN118891240A_ABST
Abstract
Description
Technical Field
[0001] Embodiments of the invention relate to ceramic structures. Background Art
[0002] Among the structures, ceramics are widely used from the viewpoints of strength, insulation, heat resistance, etc. In addition, as the ceramic structure, there is known a structure in which a metallized layer is provided on the surface of a base body formed of ceramics. For example, refer to Patent Document 1.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent No. 4348112 Summary of the invention
[0006] The ceramic structure of the present invention comprises a substrate, a first layer, and a second layer. The substrate comprises ceramic. The first layer is provided in contact with the surface of the substrate and comprises ceramic having a composition different from that of the substrate. The second layer is provided in contact with the surface of the first layer and comprises metal. In addition, in a cross section intersecting the surface of the substrate, the average grain size of the main crystal of the substrate is denoted by D B , the respective measured values when the thickness of the first layer is measured at 1 μm intervals are D1 to D n , the D1~D n The average value is D AVE When the first layer has |D n -D AVE | Greater than D B / 2 bump. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] Figure 1 It is a perspective view showing an example of the structure of the ceramic structure according to the embodiment.
[0008] Figure 2 It is an enlarged cross-sectional view showing an example of the structure of the ceramic structure according to the embodiment.
[0009] Figure 3 This is a diagram showing a SEM observation photograph of the surface of the base of the ceramic structure of Example 1.
[0010] Figure 4 This is a diagram showing a SEM observation photograph of the substrate surface of the ceramic structure of Reference Example 1.
[0011] Figure 5 This is a diagram showing a SEM observation photograph of a cross section of the surface vicinity of the ceramic structure of Example 1.
[0012] Figure 6This is a diagram showing Al distribution in a cross-sectional view near the surface of the ceramic structure of Example 1.
[0013] Figure 7 This is a diagram showing the Mn distribution in a cross-sectional view near the surface of the ceramic structure of Example 1.
[0014] Figure 8 This is a diagram showing the Mg distribution in a cross-sectional view near the surface of the ceramic structure of Example 1.
[0015] Fig. 9 This is a diagram showing a SEM observation photograph of a cross section of the surface vicinity of the ceramic structure of Reference Example 1.
[0016] Fig.10 This is a diagram showing Al distribution in a cross-sectional view near the surface of the ceramic structure of Reference Example 1.
[0017] Fig.11 This is a diagram showing the Mn distribution in a cross-sectional view near the surface of the ceramic structure of Reference Example 1.
[0018] Fig.12 This is a diagram showing the Mg distribution in a cross-sectional view near the surface of the ceramic structure of Reference Example 1. DETAILED DESCRIPTION
[0019] Hereinafter, with reference to the accompanying drawings, the embodiments of the ceramic structure disclosed in the present application are described. In addition, the present invention is not limited to the embodiments shown below. In addition, each embodiment can be appropriately combined within the scope that does not conflict with the processing content. In addition, in each of the following embodiments, the same symbols are added to the same parts, and repeated descriptions are omitted.
[0020] In the embodiments shown below, expressions such as "certain", "orthogonal", "perpendicular" or "parallel" are sometimes used, but these expressions do not need to be "certain", "orthogonal", "perpendicular" or "parallel" in a strict sense. That is, the above expressions allow for deviations in manufacturing accuracy, setting accuracy, etc.
[0021] Among the structures, ceramics are widely used from the viewpoints of strength, insulation, heat resistance, etc. Also, as the ceramic structure, there is known a structure in which a metallized layer is provided on the surface of a base body formed of ceramics.
[0022] However, in the prior art, there is room for further improvement in terms of improving the adhesion between the ceramic substrate and the metallization layer. Therefore, it is desired to realize a technology that can overcome the above-mentioned problems and improve the adhesion between the ceramic substrate and the metallization layer in a ceramic structure.
[0023] Figure 1is a schematic perspective view of a ceramic structure 1 according to an embodiment, Figure 2 1 is an enlarged cross-sectional view showing an example of the structure of the ceramic structure 1 according to the embodiment. Figure 2 yes Figure 1 The AA line cross-sectional view is shown.
[0024] like Figure 1 and Figure 2 As shown, the ceramic structure 1 of the embodiment includes a substrate 2, a first layer 3, and a second layer 4. The substrate 2 is, for example, a rectangular parallelepiped and has a surface 2a. In the present invention, the shape of the substrate 2 is not limited to Figure 2 Examples include plate-shaped, frame-shaped, column-shaped, and any other shapes.
[0025] The substrate 2 is composed of a sintered body of ceramics. Examples of the ceramics constituting the substrate 2 include ceramics having aluminum oxide (Al2O3), silicon carbide (SiC), silicon carbonitride (SiCN), titanium carbide (TiC), titanium carbonitride (TiCN), etc. as main components.
[0026] In addition, the so-called "main component" in the present invention refers to a component that occupies 80% by mass or more of the total 100% by mass of the components constituting the ceramic. The determination of each component contained in the ceramic is carried out by an X-ray diffraction device using CuKα rays, and the content of each component can be obtained by, for example, an ICP (Inductively Coupled Plasma) emission spectrometer or an X-ray fluorescence analyzer.
[0027] When the main component of the substrate 2 is alumina, it is relatively cheap in terms of both raw material price and production cost among ceramics, yet has excellent mechanical properties.
[0028] When the main component of the substrate 2 is aluminum oxide, the substrate 2 may further contain oxides of magnesium (Mg), calcium (Ca), and silicon (Si), for example.
[0029] like Figure 2 As shown, the first layer 3 is provided in contact with the surface 2a of the substrate 2. The first layer 3 contains ceramics having a composition different from that of the substrate 2. The constituent elements of the first layer 3 may include, for example, one or more elements of the substrate 2 and one or more elements of the second layer 4.
[0030] The second layer 4 is provided in contact with the surface 3a of the first layer 3. The second layer 4 contains a metal and is also referred to as a metallization layer. The second layer 4 can be formed of a metal material such as molybdenum (Mo), manganese (Mn), tungsten (W), copper (Cu), silver (Ag), palladium (Pd), gold (Au), platinum (Pt), or an alloy of these metal materials.
[0031] The second layer 4 may contain, for example, molybdenum and manganese. Thereby, the second layer 4 can be formed as a metal layer having good adhesion to the base body 2 made of ceramics.
[0032] The second layer 4 can be formed by, for example, kneading the powder of the above-mentioned metal material with an organic solvent and a binder to make a metal paste, applying the metal paste on a ceramic green sheet as the substrate 2, and sintering them simultaneously under a reducing atmosphere. In addition, at this time, the first layer 3 as an intermediate layer is formed at the interface between the substrate 2 and the second layer 4.
[0033] Also, in Figure 1 and Figure 2 In the example shown, an example in which the second layer 4 is exposed is shown, but the present invention is not limited to such an example, and other layers such as a nickel (Ni) plating layer may also be provided on the surface of the second layer 4.
[0034] Here, in the embodiment, in the cross section intersecting with the surface 2a of the base 2, that is, Figure 2 In the cross section shown, the average grain size of the main crystals (not shown) of the substrate 2 is D B , the respective measured values when the thickness of the first layer 3 is measured at 1 μm intervals are D1 to D n , such D1~D n The average value is D AVE . And, D n Here, n is an integer. The so-called main crystal refers to the crystal that occupies 50% or more of the area in the matrix.
[0035] Thus, in an embodiment, the first layer 3 has |D n -D AVE | Greater than D B In this way, since the first layer 3 has a larger concavity than the value based on the grain size of the main crystal of the substrate 2, the anchoring effect of the first layer 3 to the surface 2a of the substrate 2 can be improved.
[0036] Therefore, according to the embodiment, the adhesion of the first layer 3 to the base 2 can be improved, so the adhesion between the base 2 and the second layer 4 can be improved. In addition, if the minimum width of the base 2 and the first layer 3 is greater than 1 mm, the adhesion is particularly high. In addition, from the viewpoint of adhesion, the minimum width is greater than 2 mm, and can also be greater than 3 mm.
[0037] In addition, in the embodiment, the main crystal of the substrate 2 may be alumina. That is, the substrate 2 may have alumina as a main component. Thus, the ceramic structure 1 is relatively cheap in terms of both raw material price and production cost, but can have excellent mechanical properties.
[0038] In addition, in the embodiment, the constituent elements of the first layer 3 may include one or more elements included in the substrate 2, and may include one or more elements included in the second layer 4. For example, when the substrate 2 includes Al, Mg, Ca, Si, and oxygen (O), and the second layer 4 includes Mo and Mn, the first layer 3 may include Mg, Al, Mn, and O.
[0039] Thus, the first layer 3 as the intermediate layer has both the elements contained in the base 2 and the elements contained in the second layer 4 , thereby improving the adhesion between the base 2 and the first layer 3 and the adhesion between the first layer 3 and the second layer 4 .
[0040] Therefore, according to the embodiment, the adhesion between the base 2 and the second layer 4 can be further improved.
[0041] In addition, in an embodiment, the first layer 3 may have crystals having a spinel crystal structure. For example, when the substrate 2 contains Al, Mg, Ca, Si, and O, and the second layer 4 contains Mo and Mn, the first layer 3 may contain at least one of MgO·Al2O3 spinel crystals and MnO·Al2O3 spinel crystals.
[0042] This allows the thermal expansion coefficient of the substrate 2 containing aluminum oxide as a main component to be close to the thermal expansion coefficient of the first layer 3 containing the spinel crystals. Therefore, according to the embodiment, the peeling between the substrate 2 and the second layer 4 caused by the thermal cycle can be reduced.
[0043] In addition, in the embodiment, if Figure 1 As shown, the thickness t of the base 2 when the second layer 4 is disposed on the upper surface can be 2.0 mm or more. This can realize a ceramic structure 1 having high insulation properties with respect to the second layer 4 as a metallized layer.
[0044] Example
[0045] Hereinafter, an embodiment of the present invention will be described in detail. In the embodiment described below, a substrate 2 having aluminum oxide as a main crystal is shown, but the present invention is not limited to the following embodiment.
[0046] <Examples 1 to 3>
[0047] First, alumina powder as the main component of the substrate 2 and powders of silicon oxide (SiO2), magnesium oxide (MgO) and calcium oxide (CaO) as sintering aids are prepared. Then, the alumina powder and the sintering aid powder are mixed in a manner of Al2O3: 90 mass%, SiO2: 7 mass%, MgO: 2 mass%, and CaO: 1 mass%, and water and a dispersant are added, and the mixture is mixed for a predetermined time using a ball mill or a bead mill to form a primary slurry.
[0048] Next, an organic binder is added to the obtained primary slurry and mixed to obtain a secondary slurry. Then, the obtained secondary slurry is spray-dried to obtain particles whose main component is aluminum oxide.
[0049] Next, the obtained pellets are filled into a predetermined molding die and molded into a predetermined shape, for example, a rectangular parallelepiped shape, at an appropriately set pressure, to obtain a resulting body serving as the substrate 2 .
[0050] In parallel with the preparation of the generated body as the base 2, a metal paste is prepared as the second layer 4. Specifically, first, powders of molybdenum and manganese constituting the second layer 4 and powder of titanium oxide (TiO2) as a sintering aid are prepared.
[0051] Then, molybdenum and manganese powders and sintering aid powders were mixed in such a manner that Mo: 85 mass %, Mn: 10 mass %, and TiO2: 5 mass %, and an organic binder was added and mixed to obtain a metal paste.
[0052] Next, a metal paste is printed on the surface of the generated body by screen printing, and sintered for a predetermined time in a reducing atmosphere, for example, an atmosphere of 20% hydrogen + 80% nitrogen, to obtain three samples as Examples 1 to 3. The sintering temperature of the sintering step is, for example, 1420°C.
[0053] <Reference Examples 1 to 3>
[0054] First, alumina powder as a main component of the substrate 2 and powders of silicon oxide (SiO2), magnesium oxide (MgO) and calcium oxide (CaO) as sintering aids are prepared. Then, the alumina powder and the sintering aid powder are mixed in a manner of Al2O3: 90 mass%, SiO2: 7 mass%, MgO: 2 mass%, and CaO: 1 mass%, and water and a dispersant are added, and the mixture is mixed for a predetermined time using a ball mill or a bead mill to prepare a primary slurry.
[0055] Next, an organic binder is added to the obtained primary slurry and mixed to obtain a secondary slurry. Then, the obtained secondary slurry is spray-dried to obtain particles whose main component is aluminum oxide.
[0056] Next, the obtained pellets are filled into a predetermined forming mold and extruded into a predetermined shape, such as a rectangular parallelepiped, at an appropriately set pressure. Then, the obtained molded body is subjected to a primary firing in air to obtain a primary fired body as the substrate 2. The sintering temperature of the primary firing step is, for example, 1420°C.
[0057] In parallel with the preparation of the primary fired body as the base 2, a metal paste as the second layer 4 is prepared. Specifically, first, powders of molybdenum and manganese constituting the second layer 4 and powder of titanium oxide (TiO2) as a sintering aid are prepared.
[0058] Then, powders of molybdenum and manganese and powders of a sintering aid are mixed in such a manner that Mo: 85 mass %, Mn: 10 mass %, and TiO2: 5 mass %, and an organic binder is added and mixed to obtain a metal paste.
[0059] Next, a metal paste is printed on the surface of the primary fired body by screen printing, and secondary firing is performed for a predetermined time in a reducing atmosphere, for example, an atmosphere of 20% hydrogen + 80% nitrogen, to obtain three samples as reference examples 1 to 3. The sintering temperature of such a secondary firing step is, for example, 1350°C.
[0060] <Various Reviews>
[0061] Next, in the ceramic structures 1 of Examples 1 to 3 and Reference Examples 1 to 3 obtained above, the surface of the base 2 exposed at the side surface or the like was observed by SEM (scanning electron microscope). Figure 3 : is a figure which shows the SEM observation photograph of the base surface of the ceramic structure 1 of Example 1, Figure 4 This is a diagram showing a SEM observation photograph of the surface of the base body of the ceramic structure 1 of Reference Example 1.
[0062] Then, using the obtained SEM observation photographs, the average particle size D of aluminum oxide as the main crystal of the substrate 2 of Examples 1 to 3 and Reference Examples 1 to 3 was measured by the code method. B Specifically, first, lines are drawn so as to divide the measured SEM image into five or more equal parts in the longitudinal and lateral directions, and then the number of particles connected to each line is counted.
[0063] Next, the particle size is calculated based on the number of particles counted and the scale of the line. Finally, the average value of all the calculated particle sizes is taken as the average particle size D of the main crystal. B In addition, particles whose entire particles are not shown in the photograph are excluded from the objects of measurement.
[0064] In addition, in the ceramic structures 1 of Examples 1 to 3 and Reference Examples 1 to 3 obtained above, the bonding strength of the second layer 4 to the substrate 2 was measured by a peel strength measurement method. First, a sample for measurement was prepared. Specifically, nickel plating was formed on the surface of the second layer 4, and Kovar (nickel-iron-cobalt alloy) was brazed on the nickel-plated surface with Ag solder.
[0065] Next, the brazed sample was placed on a fixture and the fixture was clamped at one end of the Kovar cover. Then, the second layer 4 was peeled off from one end, and the bonding strength was measured at 5 points at 1mm intervals from any distance during the peeling process, and the values were taken. In addition, the bonding strength was measured using a load cell at 98N and a crosshead speed of 10mm / min.
[0066] Then, the measured values are averaged at 5 points as the bonding strength of the first measurement. This measurement is repeated 5 to 10 times, and the average bonding strength is taken as the bonding strength of the sample. The unit of bonding strength is N.
[0067] The ceramic structures 1 of Examples 1 to 3 and Reference Examples 1 to 3 obtained above were cut, the cut surfaces were mirror-polished, and the cross sections of the substrate 2, the first layer 3, and the second layer 4 were observed by SEM. In addition, the field of view observed by SEM was mapped by EPMA (Electron Probe Micro Analyzer) for various elements.
[0068] Figure 5 : is a figure which shows the SEM observation photograph of the cross section of the surface vicinity of the ceramic structure 1 of Example 1. In addition, Figure 6 to Figure 8 It is a diagram showing Al distribution, Mn distribution, and Mg distribution in a cross-section near the surface of the ceramic structure 1 of Example 1.
[0069] in addition, Fig. 9 : is a diagram showing a SEM observation photograph of a cross section of the surface vicinity of the ceramic structure 1 of Reference Example 1. Figure 10 to Figure 12 1 is a diagram showing Al distribution, Mn distribution, and Mg distribution in a cross-section near the surface of the ceramic structure 1 of Reference Example 1.
[0070] like Figure 6 to Figure 8 As shown, it can be seen that in the ceramic structures 1 of Examples 1 to 3, the first layer 3 as an intermediate layer is formed between the substrate 2 and the second layer 4 , and the first layer 3 has Al and Mg contained in the substrate 2 and Mn contained in the second layer 4 .
[0071] In addition, if Figure 6 to Figure 8 As shown, it can be seen that in the ceramic structures 1 of Examples 1 to 3, Figure 10 to Figure 12 Compared with the ceramic structures 1 of Reference Examples 1 to 3 shown, the first layer 3 as the intermediate layer is formed with a large film thickness.
[0072] In addition, if Figure 6 to Figure 8 As shown, it can be seen that in the ceramic structures 1 of Examples 1 to 3, compared with the ceramic structures 1 of Reference Examples 1 to 3, the first layer 3 as the intermediate layer has a complex shape, that is, a shape having large irregularities.
[0073] This can be speculated to be because by applying metal paste to the surface of the generated body and firing such a generated body and the metal paste at the same time, the movement of elements in the interface between the substrate 2 and the second layer 4 becomes easier than in the case where the metal paste is applied to the surface of the fired body and the metal paste is fired separately.
[0074] In the ceramic structures 1 of Examples 1 to 3 and Reference Examples 1 to 3, the mapping images of Al distribution, Mn distribution, and Mg distribution were used to regard the portion where these three elements existed as the first layer 3, and the thicknesses D1 to D2 of the first layer 3 were measured at intervals of 1 μm. n Measurements were made at 20 points.
[0075] In addition, in the mapping images of Al distribution, Mn distribution and Mg distribution, it is not necessary to Figure 6 to Figure 8 and Figure 10 to Figure 12 Instead of the gray images shown, color images directly acquired by the analysis device are used.
[0076] Then, using the obtained thicknesses D1 to D n , find the average value D of the thickness of the first layer 3 AVE In addition, the thicknesses D1 to D n With the average value D AVE The absolute value of the difference |D n -D AVE |.
[0077] Here, regarding Examples 1 to 3 and Reference Examples 1 to 3, the bonding strength of the samples, the average particle size D of the main crystals B , the thickness D of the first layer 3 at 20 points n and |D n -D AVE |、D n and |D n -D AVE The mean, maximum, minimum and standard deviation σ of |D n -D AVE | Larger than the average particle size D B The number of measurement points of / 2 is shown in Table 1. In addition, the results in Table 1 are the thicknesses D1 to D2 measured manually based on the color image obtained by the analysis device. n In addition, in Table 1, the bold frame encloses |D n -D AVE | Larger than the average particle size D B / 2 is the value of the measurement point.
[0078]
Table 1
[0079]
[0080] Comparison between Examples 1 to 3 and Reference Examples 1 to 3 shows that in Examples 1 to 3, the bonding strength of the second layer 4 to the substrate 2 is improved compared to Reference Examples 1 to 3.
[0081] In addition, according to the comparison between Examples 1 to 3 and Reference Examples 1 to 3, in Examples 1 to 3, the first layer 3 has |D n -D AVE | Greater than D B / 2 has a large number of bumps and depressions.
[0082] That is, in the embodiment, the first layer 3 has a large amount of |D n -D AVE | Greater than D B The unevenness of / 2 can improve the anchoring effect of the first layer 3 relative to the surface 2a of the substrate 2, thereby improving the adhesion between the substrate 2 and the second layer 4, that is, improving the bonding strength.
[0083] In addition, according to the comparison between Examples 1 to 3 and Reference Examples 1 to 3, by using |D n -D AVE | Greater than D B When the concavity / convexity of 3 / 2 is 3 or more, the anchoring effect of the first layer 3 relative to the surface 2a of the substrate 2 can be further improved, so the adhesion between the substrate 2 and the second layer 4 can be further improved, that is, the bonding strength can be further improved.
[0084] In addition, for the ceramic structures 1 of Examples 1 to 3 and Reference Examples 1 to 3, the thicknesses D1 to D2 of the first layer 3 were analyzed at intervals of 1 μm using the image analysis software Image Pro ver. 10 manufactured by MEDIACYBERNETICS. n Measurement is performed at 40 points, and the minimum value y1 and the maximum value y2 are measured.
[0085] The minimum value y1 is the minimum value of the coordinate position in the stacking direction of the interface between the substrate 2 and the first layer 3, in this case the vertical direction of the SEM image. The maximum value y2 is the maximum value of the coordinate position in the stacking direction of the interface between the first layer 3 and the second layer 4.
[0086] In this case, an SEM image of a different field of view from the SEM image used to obtain the measurement results shown in Table 1 was used. The specific procedure is as follows.
[0087] First, open the image to be analyzed. Next, calibrate the image scale using "Create Calibration Data" on the "Home" tab. The image scale can be 1000 to 5000 times the SEM image, depending on the state of the interface. In the current example, a 3000-times scale SEM image is used.
[0088] Next, the function of "Measurement Figure - Automatic Tracking of Free Curve" on the "Measurement" tab is used to create the contour line of the boundary between the first layer 3 and the second layer 4. Also, the function of "Measurement Figure - Automatic Tracking of Free Curve" on the "Measurement" tab is used to create the contour line of the boundary between the first layer 3 and the substrate 2.
[0089] Next, select the two created contour lines by clicking "Select" on the "Measurement" tab. Then, measure the two selected contour lines by clicking "Continuous Interval Measurement" on the "Measurement" tab. At this time, the interval of the continuous interval measurement is 1 μm.
[0090] Next, select "Measurement Items" on the "Measurement" tab and add "Line Segment Length", "Line Start Point y", and "Line End Point y" to the measurement items. Then, select "Collect" on the "Measurement" tab to create a data collection table.
[0091] Finally, according to the data recorded in the data collection table, the "average value D AVE ”, “D n The maximum value of "D n The minimum value of "D n In addition, the minimum value of the “starting point y of the line” is taken as the minimum value y1, the maximum value of the “end point y of the line” is taken as the maximum value y2, and the difference between the maximum value y2 and the minimum value y1 is taken as the difference D R That is, D R =y2-y1.
[0092] Here, regarding Examples 1 to 3 and Reference Examples 1 to 3, the bonding strength and thickness D of the samples n The average value, maximum value, minimum value and standard deviation σ, difference D R Shown in Table 2.
[0093] In addition, regarding Examples 1 to 3 and Reference Examples 1 to 3, the bonding strength of the samples and the average particle size D of the main crystals measured using the image analysis software Image Pro ver. 10 manufactured by MEDIACYBERNETICS were B , the thickness D of 40 points of the first layer 3 n and |D n -D AVE |、D n and |D n -D AVE The mean, maximum, minimum and standard deviation σ of |D n -D AVE | Larger than the average particle size D B The number of measurement points of / 2 is shown in Table 3. In Table 3, the bold frame encloses |Dn -D AVE | Larger than the average particle size D B / 2 is the value of the measurement point.
[0094]
Table 2
[0095]
[0096]
Table 3
[0097]
[0098] According to the comparison between Examples 1 to 3 and Reference Examples 1 to 3, by making the difference D R When the value is 4 μm or more, the anchoring effect of the first layer 3 with respect to the surface 2 a of the substrate 2 can be enhanced, thereby improving the adhesion between the substrate 2 and the second layer 4 , that is, the bonding strength can be improved.
[0099] In addition, according to the comparison between Examples 1 to 3 and Reference Examples 1 to 3, by making the difference D R When the value is 7 μm or less, the anchoring effect of the first layer 3 with respect to the surface 2 a of the substrate 2 can be further improved, thereby further improving the adhesion between the substrate 2 and the second layer 4 , that is, the bonding strength can be further improved.
[0100] Furthermore, XRD (X-ray diffraction analysis) was performed on the mirror-polished cross-section samples of the ceramic structures 1 of Examples 1 to 3 and Reference Examples 1 to 3 obtained above to evaluate the crystal state of the first layer 3 and the substrate 2 .
[0101] This shows that in Examples 1 to 3 and Reference Examples 1 to 3, the substrate 2 contains 97.8 mass % of aluminum oxide as a main phase and contains 2.2 mass % of sapphire as a heterophase.
[0102] In Examples 1 to 3, 94.0 mass% of aluminum oxide and 6.0 mass% of spinel were contained near the first layer 3. On the other hand, in Reference Examples 1 to 3, 98.3 mass% of aluminum oxide and 1.7 mass% of sapphire were contained near the first layer 3.
[0103] That is, it is found that the first layer 3 has crystals having a spinel crystal structure in Examples 1 to 3. This can reduce the peeling between the base 2 and the second layer 4 caused by thermal expansion and thermal contraction.
[0104] As mentioned above, although embodiment of this invention was described, this invention is not limited to the said embodiment, Unless it deviates from the summary, various changes are possible.
[0105] Further effects and other aspects can be easily derived by those skilled in the art. Therefore, the broader aspects of the present invention are not limited to the specific details and representative embodiments expressed and described above. Therefore, various changes can be made without departing from the scope of the appended patent claims and the spirit or scope of the general inventive concept defined by their equivalents.
[0106] Explanation of symbols
[0107] 1 Ceramic structure
[0108] 2 Matrix
[0109] 2a Surface
[0110] 3First floor
[0111] 3a Surface
[0112] 4 Second floor
Claims
1. A ceramic structure comprising: a substrate comprising a ceramic; A first layer, the first layer is disposed in contact with the surface of the substrate and includes a ceramic having a composition different from that of the substrate; The second layer is disposed in contact with the surface of the first layer and comprises a metal, In a cross section intersecting the surface of the substrate, Assume that the average particle size of the main crystal of the matrix is D B , The respective measured values when the thickness of the first layer is measured at 1 μm intervals are D1 to D n , D1~D n The average value is D AVE hour, The first layer has |D n -D AVE | Greater than D B / 2 bump.
2. A ceramic structure, wherein: have: a substrate comprising a ceramic; A first layer, the first layer is disposed in contact with the surface of the substrate and includes a ceramic having a composition different from that of the substrate; The second layer is disposed in contact with the surface of the first layer and comprises a metal, In a cross section intersecting the surface of the substrate, Assuming that the minimum coordinate value of the stacking direction position at the interface between the substrate and the first layer is y1, The maximum value of the coordinate position in the stacking direction at the interface between the first layer and the second layer is y2, The difference between y2 and y1 is D R hour, The D R 4μm or more.
3. The ceramic structure according to claim 2, wherein: The D R It is 7μm or more.
4. The ceramic structure according to claim 2 or 3, wherein: Assume that the average particle size of the main crystal of the matrix is D B , The respective measured values when the thickness of the first layer is measured at 1 μm intervals are D1 to D n , D1~D n The average value is D AVE hour, The first layer has |D n -D AVE | Greater than D B / 2 bump.
5. The ceramic structure according to claim 1 or 4, wherein: In the measurement range of n=20, the number of the concavities and convexities is 3 or more.
6. The ceramic structure according to any one of claims 1 to 5, wherein The main crystal of the matrix is aluminum oxide.
7. The ceramic structure according to any one of claims 1 to 6, wherein The constituent elements of the first layer include one or more elements included in the matrix and one or more elements included in the second layer.
8. The ceramic structure according to any one of claims 1 to 7, wherein The first layer has crystals including a spinel type crystal structure.
Citation Information
Patent Citations
Powder for aluminum oxide ceramics nano metallized paste and preparation method thereof
CN102049514A
Porous ceramic heating body and preparation method thereof
CN110563466A
Ceramic surface metallization process
CN110563484A
Aluminous sintered body having metallized metallic layer
JP1991218992A
Production of ceramic substrate
JP1997124382A