Solid electrolyte, method for producing solid electrolyte, and battery
By using the combination of Li, M, Si and F and mechanical ball milling treatment in the solid electrolyte, the lithium ion conductivity is improved, the problems of low output and safety of lithium ion batteries are solved, and efficient battery performance is achieved.
Patent Information
- Application Number
- CN202280093024.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-30
- Publication Date
- 2024-11-01
AI Technical Summary
The lithium ion conductivity of existing solid electrolytes is low, making it difficult to increase the battery output high current, and there are safety problems such as the generation of hydrogen sulfide gas.
The solid electrolyte containing lithium (Li), M (elements as cations, such as aluminum), Si and F is used to improve the lithium ion conductivity by mixing Li3AlF6 and Li2SiF6 and mechanical ball milling, and the lithium ion conductivity is improved, and measured by CuKα ray X-ray diffraction. Optimize the crystal structure.
A solid electrolyte with high lithium ion conductivity is achieved, ensuring the safety of the battery and high output performance, and avoiding the generation of hydrogen sulfide gas.
Smart Images

Figure CN118891685A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a solid electrolyte and a battery. Background Art
[0002] In recent years, along with the development of portable devices such as personal computers and mobile phones, the demand for batteries as their power sources has been greatly expanded. In batteries for such purposes, as a medium for moving ions, organic electrolytes obtained by dissolving electrolytes in organic solvents have been used in the past. In batteries comprising this organic electrolyte, problems related to safety may occur.
[0003] In order to eliminate the above problems and ensure intrinsic safety, all-solid batteries using solid electrolytes instead of organic electrolytes are being developed. Solid electrolytes are generally non-flammable, and therefore, lithium (Li) ion batteries with high safety can be realized.
[0004] In addition, it is well known that there are materials in solid electrolytes that react with water to produce hydrogen sulfide gas like sulfide systems. On the other hand, oxide-based solid electrolytes that do not produce gases like hydrogen sulfide are also being widely developed. However, the lithium ion conductivity of the material is lower than that of sulfides, so it is difficult to increase battery output (output large current). Therefore, "Unlocking the Potential of Fluoride-Based Solid Electrolytes for Solid-State Lithium Batteries" (ACS Appl. Energy Mater., 2019, Vol. 2, pp. 7196-7203) (Document 1) by Max Feinauer and four others gives the improvement of lithium ion conductivity by adding Al2O3 to Li3AlF6 (see Table S1 of Document 1).
[0005] However, the maximum lithium ion conductivity of the solid electrolyte in Document 1 at 100°C is 1.8×10 -5 S / cm, insufficient. Summary of the invention
[0006] The present invention relates to a solid electrolyte, and an object of the present invention is to provide a solid electrolyte having high lithium ion conductivity.
[0007] A solid electrolyte according to a preferred embodiment of the present invention contains Li, M, Si, and F, wherein M is an element that becomes a cation.
[0008] According to the present invention, a solid electrolyte having high lithium ion conductivity can be provided.
[0009] Preferably, M is an element that forms a trivalent cation.
[0010] Preferably, M is aluminum.
[0011] Preferably, M is an element that becomes a trivalent cation, and the solid electrolyte contains a composition formula of Li a M b Si c F d The composition represented by the formula satisfies 0.9(3-x)≤a≤1.1(3-x), 0.9(1-x)≤b≤1.1(1-x), 0.9x≤c≤1.1x, 5.4≤d≤6.6 and 0<x<1.
[0012] Preferably, M is an element other than Si that becomes a tetravalent cation, and the solid electrolyte contains a composition formula of Li a M b Si c F d The composition represented by the formula satisfies 1.8≤a≤2.2, 0.9(1-x)≤b≤1.1(1-x), 0.9x≤c≤1.1x, 5.4≤d≤6.6 and 0<x<1.
[0013] Preferably, in the composition formula, 0.05≤x≤0.6 is satisfied.
[0014] Preferably, an X-ray diffraction pattern obtained by X-ray diffraction measurement using CuKα rays for the solid electrolyte has peaks in both a diffraction angle 2θ range of 19 to 23° and a diffraction angle 2θ range of 40 to 44°.
[0015] Preferably, in an X-ray diffraction pattern obtained by X-ray diffraction measurement using CuKα rays for the solid electrolyte, the half-value width of the strongest peak is 0.4° or more.
[0016] The present invention also relates to a method for producing a solid electrolyte. A preferred embodiment of the present invention relates to a method for producing a solid electrolyte, comprising the following steps: a) mixing a compound composed of Li, M and F (wherein M is an element that becomes a cation) and Li2SiF6 to obtain a mixture, or mixing a compound composed of M and F, LiF and Li2SiF6 to obtain a mixture, and b) subjecting the mixture to mechanical ball milling.
[0017] Preferably, M is an element that becomes a trivalent cation. The compound composed of Li, M and F is Li3MF6, or the compound composed of M and F is MF3.
[0018] Preferably, M is an element that becomes a tetravalent cation other than Si. The compound composed of Li, M and F is Li2MF6, or the compound composed of M and F is MF4.
[0019] The present invention also relates to a battery. A preferred embodiment of the present invention relates to a battery comprising: a positive electrode; a negative electrode; and an electrolyte layer, the electrolyte layer being provided between the positive electrode and the negative electrode. The solid electrolyte is contained in at least one of the positive electrode, the negative electrode, and the electrolyte layer.
[0020] The above-mentioned object and other objects, features, aspects and advantages will become more apparent from the following detailed description of the present invention with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is a longitudinal cross-sectional view showing an all-solid secondary battery.
[0022] Figure 2 It is a diagram showing the production flow of a solid electrolyte.
[0023] Figure 3 This is a diagram showing an X-ray diffraction pattern obtained from a solid electrolyte.
[0024] Figure 4 It is a graph showing the relationship between the composition of the solid electrolyte and the lithium ion conductivity. DETAILED DESCRIPTION
[0025] Figure 1 1 is a longitudinal cross-sectional view showing an all-solid lithium ion secondary battery 1 (hereinafter referred to as "all-solid secondary battery 1"). Figure 1 The positive electrode 11, the electrolyte layer 13 and the negative electrode 12 are sequentially provided from the top. That is, the electrolyte layer 13 is provided between the positive electrode 11 and the negative electrode 12. The electrolyte layer 13 is a solid electrolyte layer and also serves as a separator layer. The positive electrode 11 includes a current collector 111 and a positive electrode layer 112. The positive electrode layer 112 contains a positive electrode active material. The negative electrode 12 includes a current collector 121 and a negative electrode layer 122. The negative electrode layer 122 contains a negative electrode active material.
[0026] The positive electrode active material of the positive electrode layer 112 preferably includes a lithium composite oxide. The preferred positive electrode active material is a lithium composite oxide having a layered rock salt structure, such as NCM (Li(Ni, Co, Mn)O2). The positive electrode active material may also be other lithium composite oxides, such as NCA (Li(Ni, Co, Al)O2) having a layered rock salt structure, LCO (LiCoO2), LNMO (LiNi) having a spinel structure, or NCM (Li(Ni, Co, Mn)O2). 0.5 Mn 1.5O4), LFP (LiFePO4) with an olivine structure, etc. The positive electrode layer 112 includes, in addition to the positive electrode active material, a solid electrolyte and an electron conduction aid (carbon black, etc.) described later. The positive electrode layer 112 in this embodiment is obtained by integrating these materials by pressurizing or heating.
[0027] Examples of the negative electrode active material of the negative electrode layer 122 include LTO (Li4Ti5O 12 ), NTO (Nb2TiO7), TiO2 (titanium oxide), graphite, SiO (silicon monoxide) and other compounds. In addition to the negative electrode active material, the negative electrode layer 122 also includes a solid electrolyte described later. The negative electrode layer 122 may further include an electron conduction aid (carbon black, etc.). The negative electrode layer 122 in this embodiment is obtained by integrating these substances by pressurizing or heating.
[0028] The configuration and material of the positive electrode 11 and the negative electrode 12 of the all-solid secondary battery 1 are not limited to the configuration and material described above, and other various configurations and materials may be adopted.
[0029] The electrolyte layer 13 is composed of the solid electrolyte involved in the present invention (hereinafter also referred to as "the present solid electrolyte"), or contains the solid electrolyte. The solid electrolyte is a lithium (Li) ion conductive material. The solid electrolyte contains lithium element (Li), an element that becomes a cation (M), silicon element (Si) and fluorine element (F). M is typically a metal element. As described later, the solid electrolyte achieves high lithium ion conductivity. In addition, the solid electrolyte is non-flammable and chemically stable, and does not produce hydrogen sulfide gas, so an inherently safe all-solid secondary battery 1 can be provided.
[0030] The present solid electrolyte is a substance obtained by mixing a compound containing Li, M and F with Li2SiF6. In one example, M is an element that becomes a trivalent cation, and the solid electrolyte is obtained by mixing Li3MF6 and Li2SiF6. When Li3MF6 and Li2SiF6 are mixed in a mass ratio of (1-x):x (where 0<x<1), the composition formula of the present solid electrolyte is Li 3-x M 1-x Si x F6 represents. If the measurement error is taken into account, the components whose mass ratios of Li, M, Si, and F a:b:c:d satisfy 0.9(3-x)≤a≤1.1(3-x), 0.9(1-x)≤b≤1.1(1-x), 0.9x≤c≤1.1x, and 5.4≤d≤6.6 can be regarded as the components represented by the above composition formula. In the above composition formula, it is preferred to satisfy 0.05≤x≤0.8, and it is more preferred to satisfy 0.05≤x≤0.6. In this way, the lithium ion conductivity can be further improved.
[0031] Preferably, M is aluminum (Al), and Li3MF6 is Li3AlF6 (hereinafter also referred to as "LAF"). The lithium ion conductivity of the solid electrolyte containing LAF and Li2SiF6 (hereinafter also referred to as "LSF") is higher than that of LAF alone. The reason for this is not necessarily clear, but one of the reasons is that Al and Si are mixed together in the crystal structure containing Li (for example, Si 4+ Solid solution in Al 3+ ) The same also applies when M is an element that becomes a trivalent cation other than Al.
[0032] As described later, the X-ray diffraction pattern obtained by X-ray diffraction measurement using CuKα rays for the present solid electrolyte preferably has peaks in the range of diffraction angles 2θ of 19 to 23° and in the range of diffraction angles 2θ of 40 to 44°. In addition, the half-value width of the strongest peak in the X-ray diffraction pattern is preferably 0.4° or more. In such a solid electrolyte, the crystallinity is moderately reduced to achieve high lithium ion conductivity. It should be noted that the present solid electrolyte can be amorphized.
[0033] Figure 2 : is a diagram showing the manufacturing process of the present solid electrolyte. In the following description, the process of mixing LAF and LSF to manufacture the present solid electrolyte is described. First, prepare the powder of LAF. In the preparation of the powder of LAF, for example, commercially available LiF (lithium fluoride) powder and commercially available AlF3 (aluminum fluoride) powder are weighed and mixed at a ratio of 3:1 (mass ratio). Next, the obtained mixture is subjected to a heat treatment (for example, 900°C), and then pulverized to obtain the powder of LAF. The powder of LAF can also be generated by other methods.
[0034] In addition, prepare the powder of LSF. The powder of LSF is a commercial product. Of course, the powder of LSF can also be generated by a well-known method. Then, the powder of LAF and the powder of LSF are mixed to obtain a mixture (step S11). In the mixture, the ratio of the amount of LSF in the total amount of LAF and the amount of LSF is greater than 0% and less than 100%. The ratio is preferably greater than 5% and less than 80%, and more preferably greater than 5% and less than 60%.
[0035] Next, the mixture is subjected to mechanical ball milling (step S12). Here, in one example of mechanical ball milling, a planetary ball mill is used. In the planetary ball mill, the tank rotates and the table carrying the tank revolves, so that very high impact energy can be generated. Mechanical ball milling can be performed using other types of pulverizers. Through the above-mentioned mechanical ball milling, a powder of the present solid electrolyte for the positive electrode layer 112, the negative electrode layer 122 or the electrolyte layer 13 is obtained. In this treatment example, the mechanical ball milling is performed at room temperature, but conditions such as temperature can be appropriately changed.
[0036] Figure 3 This is a diagram showing an X-ray diffraction (XRD) pattern obtained by measuring the present solid electrolyte by a powder X-ray diffraction method. In this measurement, CuKα rays are used as a radiation source of the X-ray diffraction device. Figure 3 In the figure, the X-ray diffraction pattern of the solid electrolyte obtained by setting the mass ratio of LSF to 20% (Experimental Example 3 described later) is marked with the symbol L11, the X-ray diffraction pattern of the solid electrolyte obtained by setting the ratio to 50% (Experimental Example 4 described later) is marked with the symbol L12, and the X-ray diffraction pattern of the solid electrolyte obtained by setting the ratio to 80% (Experimental Example 5 described later) is marked with the symbol L13. In addition, the X-ray diffraction pattern of the solid electrolyte of the comparative example obtained by mechanically milling only LAF is marked with the symbol L21. In addition, the X-ray diffraction pattern of the powder of LAF that has not been mechanically milled is marked with the symbol L31, and the X-ray diffraction pattern of the powder of LSF that has not been mechanically milled is marked with the symbol L32. It should be noted that in the X-ray diffraction patterns of lines L11 to L13 and L21, the changes in the vertical axis direction (intensity) are magnified compared with lines L31 and L32.
[0037] picture Figure 3 Thus, the X-ray diffraction pattern of the solid electrolyte produced by mechanical ball milling has broad peaks in both the diffraction angle 2θ range of 19 to 23° and the diffraction angle 2θ range of 40 to 44°. Figure 3It can be seen that due to the very high impact energy brought by the mechanical ball milling treatment, the LAF and LSF particles are miniaturized or partially amorphized. In addition, the crystal structure is disordered due to deformation and dislocation within the crystal, especially at the particle interface. This phenomenon occurs significantly, and it is believed that the lithium ion conductivity of the solid electrolyte is increased. Accordingly, the solid electrolyte can be further amorphized or completely amorphized. In order to more reliably improve the lithium ion conductivity of the solid electrolyte, the half-value width of the strongest peak in the X-ray diffraction pattern (for example, a peak in the range of 19 to 23°) is preferably above 0.4°, and more preferably above 0.6°. In the X-ray diffraction pattern of line L11, the half-value width of the strongest peak is 1.08°. The upper limit of the half-value width is not particularly limited, for example, 3.0°. It should be noted that the half-value width of the peak is solved as follows: For the X-ray diffraction pattern, the data analysis software Origin Pro 2020b is used to fit the pseudo-Voigt peak function (type 1).
[0038] In addition, if Figure 3 As shown by the arrow A1 in the figure, the peak in the range of 40 to 44° moves toward the high angle side as the mass ratio of LSF increases. Therefore, for the present solid electrolyte, it is considered that: in the crystal structure of LAF, the ion radius is Si 4+ Solid solution in ions with a radius of Al 3+ , the unit lattice becomes smaller. It should be noted that the present solid electrolyte can be made amorphous by the solid electrolyte production method and the like.
[0039] Next, an experimental example of a solid electrolyte is described. The following experiments were performed in a glove box or a dry room with a dew point of -40°C or less.
[0040] (Experimental Example 1)
[0041] As raw materials, commercially available LiF (lithium fluoride) powder and commercially available AlF3 (aluminum fluoride) powder were prepared. Each raw material was weighed and mixed according to a LiF:AlF3 ratio of 3:1 (mass ratio). The obtained mixture was heated at 900°C and then crushed in a mortar to obtain Li3AlF6 (i.e., LAF) powder. Thus, a solid electrolyte powder containing only LAF powder was obtained.
[0042] (Experimental Example 2)
[0043] In addition to the above LAF powder, commercially available Li2SiF6 (ie, LSF) powder was prepared, LAF:LSF was weighed to 90:10 (mass ratio), and mechanically milled using a planetary ball mill to obtain a solid electrolyte powder containing LAF and LSF.
[0044] (Experimental Example 3)
[0045] The same treatment as in Experimental Example 2 was carried out except that the weight was adjusted so that LAF:LSF was 80:20 (mass ratio) to obtain a solid electrolyte powder.
[0046] (Experimental Example 4)
[0047] The same treatment as in Experimental Example 2 was carried out except that the LAF:LSF was weighed to be 50:50 (mass ratio), thereby obtaining a solid electrolyte powder.
[0048] (Experimental Example 5)
[0049] The same treatment as in Experimental Example 2 was carried out except that the weight was adjusted so that LAF:LSF was 20:80 (mass ratio) to obtain a solid electrolyte powder.
[0050] <Measurement of lithium ion conductivity>
[0051] The solid electrolyte powder was placed in a mold consisting of a resin sleeve and upper and lower punches made of SUS (stainless steel) and uniaxially pressed at 150 MPa. Lead wires were connected to the upper and lower punches, and impedance was measured at room temperature to 100°C to calculate the lithium ion conductivity.
[0052] Table 1 shows the composition formula of the solid electrolytes of Experimental Examples 1 to 5, the lithium ion conductivity at 100° C., and the half-value width of each peak calculated by the above method for the XRD pattern. 3-x Al 1-x Si x F6 is a composition formula when Li3AlF6 as LAF and Li2SiF6 as LSF are mixed at a mass ratio of (1-x):x. Experimental Examples 2 to 5 are embodiments of the present invention satisfying 0<x<1, and Experimental Example 1 is a comparative example of x=0. In addition, Figure 4 The composition formula is shown as Li 3-x Al 1-x Si x The relationship between the value of x in F6 (that is, the ratio of the amount of substance of LSF) and the lithium ion conductivity at 100°C.
[0053] [Table 1]
[0054]
[0055] The solid electrolyte powders of Experimental Examples 2 to 5 containing LSF had higher lithium ion conductivity at 100°C than the solid electrolyte powder of Experimental Example 1 not containing LSF. Specifically, as the mass ratio of LSF approaches 20% from 0%, the lithium ion conductivity increases. If the ratio of LSF increases further, the lithium ion conductivity decreases. In Experimental Example 5, where the ratio of LSF is 80%, the lithium ion conductivity reaches 2.4×10 -5 S / cm, compared with the lithium ion conductivity of Experiment 1 without LSF of 7.6×10 -6 Therefore, it is considered that the lithium ion conductivity higher than that of the solid electrolyte powder of Experimental Example 1 is ensured by the LSF ratio being greater than 0% and less than 100% (ie, 0<x<1).
[0056] In Experimental Example 2, where the mass ratio of LSF was 10%, the lithium ion conductivity was 8.9×10 -5 S / cm, therefore, it is believed that if the ratio of LSF is 5% or more, the lithium ion conductivity is sufficiently increased. The upper limit of the ratio of LSF is preferably 80%, and more preferably 60%. Thus, sufficiently high lithium ion conductivity can be achieved more reliably.
[0057] Figure 2 In step S11, Li3AlF6 (i.e., LAF) generated from LiF and AlF3 is mixed with LSF, however, LiF and AlF3 may be directly mixed with LSF without generating Li3AlF6. In this case, a solid electrolyte with high lithium ion conductivity may be produced by mechanically milling the mixture in step S12. In addition, in step S11, the element that will become a trivalent cation may be set as M, and Li3MF6 other than Li3AlF6 may be mixed with LSF. Li3MF6 is, for example, Li3GaF6, Li3CrF6, Li3LaF6, etc. In addition, MF3 and LiF other than AlF3 may be directly mixed with LSF. MF3 is, for example, GaF3, CrF3, LaF3, BiF3, YF3, etc.
[0058] M in the present solid electrolyte may be an element other than Si that becomes a tetravalent cation. Such a solid electrolyte is obtained, for example, by mixing Li2MF6 and LSF (i.e., Li2SiF6). In this case, a solid electrolyte having high lithium ion conductivity can also be realized. Figure 2 In step S11, when Li2MF6 and Li2SiF6 are mixed in a mass ratio of (1-x):x (where 0<x<1), the composition formula of the solid electrolyte is Li2M 1-x Si x F6 indicates.
[0059] If measurement errors are taken into account, the components whose mass ratios of Li, M, Si, and F a:b:c:d satisfy 1.8≤a≤2.2, 0.9(1-x)≤b≤1.1(1-x), 0.9x≤c≤1.1x, and 5.4≤d≤6.6 can be regarded as components represented by the above composition formula. In the above composition formula, it is preferred to satisfy 0.05≤x≤0.8, and it is more preferred to satisfy 0.05≤x≤0.6. In this way, the lithium ion conductivity can be further improved. Li2MF6 is, for example, Li2TiF6, Li2ZrF6, Li2GeF6, etc. In step S11, LiF and MF4 can be directly mixed with Li2SiF6 without generating Li2MF6. MF4 is, for example, TiF4, ZrF4, etc.
[0060] As described above, the present solid electrolyte contains Li, M, Si, and F, where M is an element that becomes a cation. Thus, a solid electrolyte having high lithium ion conductivity can be provided.
[0061] Preferably, M is an element that becomes a trivalent cation. In this case, the present solid electrolyte preferably contains a composition formula of Li a M b Si c F d The composition represented by the formula satisfies 0.9(3-x)≤a≤1.1(3-x), 0.9(1-x)≤b≤1.1(1-x), 0.9x≤c≤1.1x, 5.4≤d≤6.6, and 0<x<1. Thus, high lithium ion conductivity can be achieved more reliably.
[0062] M may be an element that forms a tetravalent cation other than Si. In this case, the present solid electrolyte preferably contains a composition formula of Li a M b Si c F d The composition represented by the formula satisfies 1.8≤a≤2.2, 0.9(1-x)≤b≤1.1(1-x), 0.9x≤c≤1.1x, 5.4≤d≤6.6, and 0<x<1. Thus, high lithium ion conductivity can be achieved more reliably.
[0063] When confirming whether the unknown solid electrolyte is the present solid electrolyte, the unknown solid electrolyte is subjected to chemical analysis to confirm whether the constituent elements are Li, M, Si, or F. In addition, when confirming whether the unknown solid electrolyte is the above composition formula, for example, for Li, Al, and Si, quantification can be performed using an ICP-emission spectrophotometer. For F, ion chromatography can be used for quantification. When the present solid electrolyte contains an element M other than Al, a determination method capable of quantifying the element M is appropriately selected.
[0064] The method for manufacturing the solid electrolyte includes the following steps: mixing a compound composed of Li, M and F (wherein M is an element that becomes a cation) and Li2SiF6 to obtain a mixture, or mixing a compound composed of M and F, LiF and Li2SiF6 to obtain a mixture (step S11); and mechanically milling the mixture (step S12). Thus, a solid electrolyte having high lithium ion conductivity can be easily provided.
[0065] Preferably, M is an element that becomes a trivalent cation. In this case, preferably, the compound composed of Li, M and F is Li3MF6, or the compound composed of M and F is MF3. Thus, a solid electrolyte having high lithium ion conductivity can be manufactured more reliably.
[0066] M may be an element that becomes a tetravalent cation other than Si. In this case, it is preferred that the compound composed of Li, M and F is Li2MF6, or the compound composed of M and F is MF4. Thus, a solid electrolyte having high lithium ion conductivity can be manufactured more reliably.
[0067] The present solid electrolyte, the method for producing the solid electrolyte, and the battery may be modified in various ways.
[0068] M contained in the present solid electrolyte may be an element that becomes a cation, and may be an element other than an element that becomes a trivalent cation and an element that becomes a tetravalent cation. In addition, the X-ray diffraction pattern obtained from the solid electrolyte may not have a peak in the range of a diffraction angle 2θ of 19 to 23° and / or a diffraction angle 2θ of 40 to 44°. In addition, the half-value width of the strongest peak in the X-ray diffraction pattern may be less than 0.4°.
[0069] The present solid electrolyte can be mixed with other substances (which may contain Li) and used as an electrolyte material. In this case, the present solid electrolyte is preferably the component with the largest mass ratio among the components contained in the electrolyte material, i.e., the main component. The mass ratio of the main component in the electrolyte material is preferably 50% by mass or more, more preferably 60% by mass or more, and further preferably 70% by mass or more.
[0070] The present solid electrolyte used in the all-solid secondary battery 1 does not necessarily need to be included in all of the positive electrode 11, the negative electrode 12 and the electrolyte layer 13, and can be included in at least one of the positive electrode 11, the negative electrode 12 and the electrolyte layer 13. In addition, the present solid electrolyte can be used in batteries other than all-solid secondary batteries, and can also be used for purposes other than batteries. The manufacture of the present solid electrolyte can be carried out by a treatment other than a mechanical ball milling treatment.
[0071] The configurations in the above-described embodiment and each modified example may be appropriately combined unless they are mutually contradictory.
[0072] Although the invention has been described and illustrated in detail, the above description is illustrative and not restrictive, and therefore, it can be understood that numerous modifications and variations may be employed without departing from the scope of the invention.
[0073] Explanation of symbols
[0074] 1All-solid lithium-ion secondary battery
[0075] 11 Positive electrode
[0076] 12 Negative electrode
[0077] 13 Electrolyte layer
[0078] Steps S11 and S12
Claims
1. A solid electrolyte, wherein: Contains Li, M, Si and F, where M is an element that becomes a cation.
2. The solid electrolyte according to claim 1, wherein M is an element which becomes a trivalent cation.
3. The solid electrolyte according to claim 1 or 2, wherein M is aluminum element.
4. The solid electrolyte according to any one of claims 1 to 3, wherein M is an element that becomes a trivalent cation, The solid electrolyte comprises a composition formula of Li a M b Si c F d Indicates the ingredients, It satisfies 0.9(3-x)≤a≤1.1(3-x), 0.9(1-x)≤b≤1.1(1-x), 0.9x≤c≤1.1x, 5.4≤d≤6.6 and 0<x<1.
5. The solid electrolyte according to claim 1, wherein M is an element other than Si that forms a tetravalent cation, The solid electrolyte comprises a composition formula of Li a M b Si c F d Indicates the ingredients, Satisfies 1.8≤a≤2.2, 0.9(1-x)≤b≤1.1(1-x), 0.9x≤c≤1.1x, 5.4≤d≤6.6 and 0<x<1.
6. The solid electrolyte according to claim 4 or 5, wherein In the composition formula, 0.05≤x≤0.6 is satisfied.
7. The solid electrolyte according to any one of claims 1 to 6, wherein The X-ray diffraction pattern obtained by X-ray diffraction measurement using CuKα rays has peaks in both the diffraction angle 2θ range of 19 to 23° and the diffraction angle 2θ range of 40 to 44°.
8. The solid electrolyte according to any one of claims 1 to 7, wherein In the X-ray diffraction pattern obtained by X-ray diffraction measurement using CuKα rays, the half-value width of the strongest peak is 0.4° or more.
9. A method for producing a solid electrolyte, wherein: Including the following processes: a) a mixture obtained by mixing a compound consisting of Li, M and F and Li2SiF6, or a mixture obtained by mixing a compound consisting of M and F, LiF and Li2SiF6, wherein M is an element that becomes a cation, b) subjecting the mixture to mechanical ball milling.
10. The method for producing a solid electrolyte according to claim 9, wherein: M is an element that becomes a trivalent cation, The compound composed of Li, M and F is Li3MF6, or the compound composed of M and F is MF3.
11. The method for producing a solid electrolyte according to claim 9, wherein: M is an element other than Si that forms a tetravalent cation, The compound composed of Li, M and F is Li2MF6, or the compound composed of M and F is MF4.
12. A battery, wherein: have: positive electrode; a negative electrode; and an electrolyte layer, the electrolyte layer being disposed between the positive electrode and the negative electrode, The solid electrolyte according to any one of claims 1 to 8 is contained in at least one of the positive electrode, the negative electrode, and the electrolyte layer.