Electrode foil for electrolytic capacitor, electrolytic capacitor, and method for manufacturing electrode foil for electrolytic capacitor
By forming a second dielectric layer with a high dielectric constant on the anode body of the electrolytic capacitor and suppressing oxygen diffusion using the first dielectric layer, the problems of reducing insulating properties of the dielectric layer and increasing leakage current are solved, and large capacity and low leakage are achieved Electrical capacitors for current.
Patent Information
- Application Number
- CN202380019172.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-31
- Filing Date
- 2023-01-30
- Publication Date
- 2024-11-01
AI Technical Summary
In the process of increasing the capacity of the electrolytic capacitor, the formation of a metal oxide layer with a high dielectric constant causes oxygen to move to the anode body side, resulting in a decrease in insulation of the dielectric layer and an increase in leakage current.
The anode body containing a valve-acting metal is adopted, and the first dielectric layer and the second dielectric layer covering at least a portion of the anode body, wherein the dielectric constant of the second dielectric layer is higher than that of the first dielectric layer, and the thickness of the second dielectric layer is greater than that of the The first dielectric layer, the first dielectric layer serves as a layer for suppressing oxygen diffusion to maintain the insulating property of the second dielectric layer.
While increasing the capacity, suppress the increase of leakage current, maintain the withstand voltage, and realize electrolytic capacitors with large CV values and low leakage current.
Smart Images

Figure CN118891695A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electrode foil for an electrolytic capacitor, an electrolytic capacitor, and a method for producing the electrode foil for an electrolytic capacitor. Background Art
[0002] The electrode foil of the electrolytic capacitor includes an anode body and a dielectric layer covering at least a portion of the surface of the anode body. The anode body can use a metal foil containing a valve metal. In order to increase the capacity of the electrolytic capacitor, the surface of the metal foil is roughened by etching or the like.
[0003] The dielectric layer is formed, for example, by subjecting a metal foil having a roughened surface to a chemical conversion treatment. In addition, a method of forming a dielectric layer by atomic layer deposition is also being studied (for example, Patent Document 1).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2012-43960 Summary of the invention
[0007] Problems to be solved by the invention
[0008] When a layer of a metal oxide with a high dielectric constant (dielectric layer) is formed to increase the capacity, oxygen in the dielectric layer moves to the anode body when a high voltage is applied, and the insulation of the dielectric layer decreases, which may increase the leakage current.
[0009] Means for solving problems
[0010] One aspect of the present invention relates to an electrode foil for an electrolytic capacitor, comprising an anode body including a valve action metal, a first dielectric layer covering at least a portion of the anode body, and a second dielectric layer covering at least a portion of the first dielectric layer, wherein the second dielectric layer has a higher dielectric constant than the first dielectric layer, a thickness T2 of the second dielectric layer is greater than a thickness T1 of the first dielectric layer, and the first dielectric layer is a layer that suppresses diffusion of oxygen from the second dielectric layer to the anode body.
[0011] Another aspect of the present invention relates to an electrolytic capacitor including the above-described electrode foil for an electrolytic capacitor and a cathode portion covering at least a portion of the second dielectric layer.
[0012] Another aspect of the present invention relates to a method for manufacturing an electrode foil for an electrolytic capacitor, the manufacturing method comprising: a first step of preparing an anode body containing a valve-acting metal; a second step of forming a first dielectric layer covering at least a portion of the anode body; and a third step of, after the second step, forming a second dielectric layer covering at least a portion of the first dielectric layer, wherein the second dielectric layer has a higher dielectric constant than the first dielectric layer, a thickness T2 of the second dielectric layer is greater than a thickness T1 of the first dielectric layer, and the first dielectric layer is a layer for suppressing diffusion of oxygen from the second dielectric layer to the anode body.
[0013] Effects of the Invention
[0014] According to the present invention, in an electrolytic capacitor, it is possible to increase the capacitance while suppressing an increase in leakage current.
[0015] The novel features of the present invention are described in the scope of the appended claims, but the present invention in both structure and content together with other objects and features of the present invention should be more fully understood through the following detailed description with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a cross-sectional view schematically showing a surface portion of an electrode foil according to an embodiment of the present invention.
[0017] Figure 2 It is a cross-sectional view schematically showing an electrolytic capacitor according to an embodiment of the present invention.
[0018] Figure 3 This is a perspective view of a part of the rolled body unfolded.
[0019] Figure 4 It is a cross-sectional view schematically showing an electrolytic capacitor according to another embodiment of the present invention. DETAILED DESCRIPTION
[0020] Hereinafter, the embodiments of the present invention will be described with examples, but the present invention is not limited to the examples described below. In the following description, specific numerical values and materials are sometimes exemplified, but other numerical values and materials may also be applied as long as the effect of the present invention can be obtained. In this specification, the description of "numerical value A to numerical value B" includes numerical value A and numerical value B, and may be renamed as "numerical value A or more and numerical value B or less". In the following description, when the lower limit and upper limit of numerical values for specific physical properties, conditions, etc. are exemplified, as long as the lower limit is not above the upper limit, any one of the exemplified lower limits may be arbitrarily combined with any one of the exemplified upper limits. When multiple materials are exemplified, one may be selected and used alone, or two or more may be used in combination.
[0021] [Electrode foil for electrolytic capacitors]
[0022] An electrode foil for an electrolytic capacitor according to an embodiment of the present invention comprises an anode body including a valve action metal, a first dielectric layer covering at least a portion of the anode body, and a second dielectric layer covering at least a portion of the first dielectric layer. The second dielectric layer has a higher dielectric constant than the first dielectric layer, and a thickness T2 of the second dielectric layer is greater than a thickness T1 of the first dielectric layer. The first dielectric layer is a layer that suppresses diffusion of oxygen from the second dielectric layer to the anode body.
[0023] By providing the electrode foil with a second dielectric layer with a high dielectric constant, a large capacity can be achieved. By sandwiching a first dielectric layer with a low dielectric constant and excellent insulation between the anode body and the second dielectric layer, the movement of oxygen from the second dielectric layer to the anode body is suppressed, the insulation of the second dielectric layer is maintained, and the increase of the leakage current (LC) is suppressed. In addition, the reduction of the withstand voltage is also suppressed. As a result, an electrolytic capacitor with a large CV value and a small LC can be obtained.
[0024] Assuming that the first dielectric layer is not interposed between the anode body and the second dielectric layer, the oxygen in the second dielectric layer decreases due to the movement of oxygen from the second dielectric layer to the anode body, and the insulation of the second dielectric layer decreases. In addition, due to the oxygen moving from the second dielectric layer to the anode body, an oxide film (film of the oxide of the valve metal) of the anode body is formed on the surface of the anode body. This oxide film cannot make up for the insufficient withstand voltage of the second dielectric layer. As a result, the leakage current increases.
[0025] This oxygen migration occurs, for example, when the cut surface of the electrode foil after forming the winding body is subjected to a formation treatment to form a formation film, or when the assembled electrolytic capacitor is subjected to a reflow treatment. This oxygen migration is easy to occur when a high voltage or a high temperature load is applied. For example, when the above-mentioned formation treatment is performed at a formation voltage of 15V or more, or when the reflow treatment is performed at 200°C or more, this oxygen migration is easy to occur. In this case, the effect of suppressing the increase of LC brought about by the first dielectric layer can be significantly obtained.
[0026] (1st dielectric layer)
[0027] The first dielectric layer is a layer that inhibits the diffusion of oxygen from the second dielectric layer to the anode body (hereinafter also referred to as the inhibition layer). The first dielectric layer contains a first metal oxide (hereinafter also referred to as the first oxide). The first oxide contains a first metal. From the viewpoint of low LC, the first metal is preferably at least one selected from silicon (Si) and aluminum (Al). In the first dielectric layer, for example, SiO2, Al2O3, etc. may be contained alone, or two or more may be contained. In the case where the first dielectric layer contains two or more oxides of the first metal, the oxides may be mixed or may be arranged in layers.
[0028] The first dielectric layer contains the first metal and substantially does not contain the second metal. The phrase “substantially does not contain the second metal” means that the second metal is less than the detection limit in energy dispersive X-ray spectroscopy (EDX) analysis.
[0029] (Second dielectric layer)
[0030] The second dielectric layer includes a second metal oxide (hereinafter also referred to as the second oxide) having a higher dielectric constant than the first metal oxide. The second oxide includes a second metal different from the first metal. The oxide of the second metal has a higher dielectric constant than the oxide of the first metal. From the viewpoint of large capacity, the second metal is preferably at least one selected from tantalum (Ta), titanium (Ti), zirconium (Zr), niobium (Nb) and hafnium (Hf). In the second dielectric layer, for example, Ta2O5, TiO2, ZrO2, Nb2O5, HfO2, etc. may be included alone, or two or more may be included. In the case where the second dielectric layer includes two or more oxides of the second metal, the two or more oxides may be mixed or may be configured in layers respectively.
[0031] The second oxide may also contain the first metal (for example, at least one selected from silicon and aluminum) while containing the second metal. That is, the second oxide may be a composite oxide in which the oxide of the first metal is mixed with the oxide of the second metal. In the case where the oxide of the second metal is easily crystallized and has a tendency to increase LC, crystallization can be suppressed by making it into a composite oxide, and the effect of suppressing the increase of LC can be easily obtained. In the case where the second metal is Ti, the effect brought by making it into a composite oxide is particularly significant. For example, in the case where the second dielectric layer is a composite oxide layer mixed with TiO2 and Al2O3, the molar ratio of Ti / Al in the composite oxide layer can be, for example, greater than 2 and less than 6.
[0032] The first dielectric layer and the second dielectric layer can be confirmed as follows.
[0033] A cross-sectional image (including a cross-sectional image of a porous portion) in the thickness direction of the electrode foil is obtained by using a scanning electron microscope (SEM) or a transmission electron microscope (TEM), and an element mapping based on energy dispersive X-ray spectroscopy (EDX) analysis is performed using the image to obtain a mapping diagram of the first metal and the second metal in the metal oxide layer covering the surface of the anode body. The above image is used to distinguish between the region of the metal structure constituting the anode body and the region of the metal oxide constituting the first dielectric layer and the second dielectric layer. For example, the above two regions can be distinguished by binarization processing of the image. In the element mapping, the region in which the second metal is distributed among the regions of the metal oxide is confirmed to be the second dielectric layer. Among the regions of the metal oxide, the region in which the first metal is confirmed to be distributed and the second metal is not distributed (less than the detection limit of the second metal) between the anode body and the second dielectric layer is confirmed to be the first dielectric layer.
[0034] The thickness T2 of the second dielectric layer is greater than the thickness T1 of the first dielectric layer. T1 / T2 can be, for example, less than 0.6, less than 0.3, or less than 0.1. Thus, the second dielectric layer with a high dielectric constant is fully ensured, and a large capacity can be achieved. It should be noted that the thickness T1 of the first dielectric layer can be obtained by measuring the thickness of any 10 points of the first dielectric layer confirmed by element mapping of the cross-sectional image in the thickness direction of the above-mentioned electrode foil, and calculating their average value. The thickness T2 of the second dielectric layer can also be obtained in the same way as the thickness T1 of the first dielectric layer.
[0035] From the viewpoint of sufficiently suppressing the movement of oxygen from the second dielectric layer to the anode body, the thickness T1 of the first dielectric layer may be 0.3 nm or more.
[0036] From the viewpoint of being easy to simultaneously realize the low LC brought about by the first dielectric layer and the large capacity brought about by the second dielectric layer, when the first metal includes Si, the ratio of the thickness T1 of the first dielectric layer to the thickness T2 of the second dielectric layer: T1 / T2 can be less than 0.45, less than 0.2, or less than 0.1. From the same viewpoint, when the first metal includes Al, T1 / T2 can be less than 0.6, less than 0.25, or less than 0.1. When T1 / T2 is within the above range, it is easy to obtain an electrolytic capacitor with a large CV value and low LC.
[0037] Below, in reference Figure 1 At the same time, an example of the electrode foil according to the embodiment of the present invention is described. Figure 1 This is a cross-sectional view schematically showing a surface portion of an electrode foil according to an embodiment of the present invention.
[0038] Anode foil 10 (electrode foil) includes an anode body 110 and a dielectric layer 120 covering at least a portion of anode body 110. Dielectric layer 120 includes a first dielectric layer 121 covering at least a portion of anode body 110 and a second dielectric layer 122 covering at least a portion of first dielectric layer 121. Second dielectric layer 122 has a higher dielectric constant than first dielectric layer 121. Thickness T2 of second dielectric layer 122 is greater than thickness T1 of first dielectric layer 121.
[0039] The anode body 110 is a metal foil containing a valve action metal having a surface roughened by etching or the like, and has a core portion 111 and a porous portion 112. The porous portion 112 has a plurality of pits P. The dielectric layer 120 (the first dielectric layer 121 and the second dielectric layer 122) covers the outer surface of the porous portion 112 and the inner wall surface of the pit P.
[0040] [Method for producing electrode foil for electrolytic capacitor]
[0041] The manufacturing method of the electrode foil for electrolytic capacitors according to the embodiment of the present invention includes: a first step of preparing an anode body including a valve metal; a second step of forming a first dielectric layer covering at least a portion of the anode body; and a third step of forming a second dielectric layer covering at least a portion of the first dielectric layer after the second step. The second dielectric layer has a higher dielectric constant than the first dielectric layer. The thickness T2 of the second dielectric layer is greater than the thickness T1 of the first dielectric layer. The first dielectric layer is a layer that suppresses the diffusion of oxygen from the second dielectric layer to the anode body.
[0042] Hereinafter, each step will be described in detail.
[0043] (1st step)
[0044] The anode body includes a valve-acting metal such as tantalum, niobium, titanium, or aluminum. The anode body may be, for example, a metal foil whose surface has been roughened by etching or the like. The thickness of the metal foil is, for example, not less than 15 μm and not more than 300 μm.
[0045] The metal foil with a roughened surface has a porous portion and a core connected to the porous portion. The porous portion has a plurality of pits. The most frequent pore size of the pits in the porous portion is not particularly limited, but from the perspective of easily obtaining a large surface area and easily forming a dielectric layer to the deep part of the pit, it is, for example, more than 50nm and less than 2000nm. It should be noted that the most frequent pore size of the pit is the most frequent pore size in the volume-based pore size distribution measured by a mercury porosimeter. The thickness D of each side of the porous portion is not particularly limited, but from the perspective of ensuring a large surface area and maintaining the strength of the electrode foil, it is, for example, more than 1 / 10 and less than 4 / 10 of the total thickness of the metal foil. The thickness D of each side of the porous portion can be obtained by measuring the thickness of any 10 points using a cross-sectional image of the metal foil based on SEM or TEM and calculating their average value.
[0046] (Second step)
[0047] In the second step, the first dielectric layer can be formed by atomic layer deposition (ALD) or chemical formation. In the case of chemical formation, a layer of valve metal oxide is formed as the first dielectric layer, and the valve metal becomes the first metal. In the case of the ALD method, the first metal can be appropriately selected without depending on the valve metal contained in the anode body. The chemical formation can be performed, for example, by immersing the anode body in a chemical formation liquid such as an ammonium adipate solution and applying a predetermined chemical formation voltage (anodization). In the case of chemical formation, the thickness T1 of the first dielectric layer can be controlled by using a chemical formation voltage, etc.
[0048] In the case of the ALD method, a raw material gas containing a first metal and an oxidant can be alternately supplied to a reaction chamber in which an object is arranged, and a first dielectric layer can be formed on the surface of the object. In the ALD method, due to the self-limiting effect, the first metal is deposited on the surface of the object in atomic layer units. Therefore, the thickness T1 of the first dielectric layer can be easily controlled by using the number of cycles of supply of raw material gas → exhaust (purge) of raw material gas → supply of oxidant → exhaust (purge) of oxidant as one cycle.
[0049] Examples of the oxidant include water, oxygen, ozone, etc. The oxidant may be supplied to the reaction chamber in the form of plasma, and the plasma may contain the oxidant as a raw material.
[0050] The first metal is supplied to the reaction chamber in the form of a gas (raw material gas) containing a precursor of the first metal. The precursor is, for example, an organic metal compound containing the first metal, whereby the first metal is easily chemically adsorbed on the object. Various organic metal compounds conventionally used in the ALD method can be used as precursors.
[0051] Examples of the precursor containing the first metal include a precursor containing Al and a precursor containing Si. Examples of the precursor containing Al include trimethylaluminum ((CH 3 ) 3 Al).
[0052] Examples of the precursor containing Si include N-sec-butyl(trimethylsilyl)amine (C7H 19 NSi), 1,3-diethyl-1,1,3,3-tetramethyldisilazane (C8H 23 NSi2), 2,4,6,8,10-pentamethylcyclopentasiloxane ((CH3SiHO)5), pentamethyldisilane ((CH3)3SiSi(CH3)2H), tri(dimethylamino)silane ([(CH3)2N]3SiH), tri(isopropoxy)silanol ([(H3C)2CHO]3SiOH), chloropentanemethyldisilane ((CH3)3SiSi(CH3)2Cl), dichlorosilane (SiH2Cl2), tri(dimethylamino)silane (Si[N(CH3)2]4), tetraethylsilane (Si(C2H5)4), tetramethylsilane (Si(CH3)4), tetraethoxysilane (Si(OC2H5)4), dodecamethylcyclohexasilane ((Si(CH3)2)6), silicon tetrachloride (SiCl4), silicon tetrabromide (SiBr4), etc.
[0053] The first metal may be used alone or in combination of two or more. When two or more first metals are used in combination, a precursor containing two or more first metals may be used. In addition, in this case, the type of precursor supplied to the reaction chamber may be changed corresponding to the cycle, thereby changing the type of the first metal deposited in atomic layer units. In this case, a first dielectric layer (composite oxide layer) mixed with oxides of two or more first metals may be formed.
[0054] (Step 3)
[0055] In the third step, it is preferred to form the second dielectric layer in the same manner as described above using the ALD method. The second metal can be appropriately selected relative to the first metal, and the thickness T2 of the second dielectric layer can be easily controlled using the number of cycles. In the formation step of the second dielectric layer based on the ALD method, the second metal is supplied to the reaction chamber in the form of a gas (raw material gas) containing a precursor of the second metal. Examples of the precursor containing the second metal include a precursor containing Ta, a precursor containing Ti, a precursor containing Zr, a precursor containing Nb, a precursor containing Hf, and the like.
[0056] Examples of the precursor containing Ta include tris(ethylmethylamide)(tert-butylamide)tantalum(V) (C 13 H33 N4Ta), ethoxytantalum (V) (Ta(OC2H5)5), tris(diethylamide)(tert-butylimide)tantalum (V) ((CH3)3CNTa(N(C2H5)2)3), penta(dimethylamino)tantalum (V) (Ta(N(CH3)2)5), etc.
[0057] Examples of the precursor containing Ti include bis(tert-butylcyclopentadienyl)titanium(IV) dichloride (C 18 H 26 C 12 Ti), tetrakis(dimethylamino)titanium(IV)([(CH3)2N]4Ti), tetrakis(diethylamino)titanium(IV)([(C2H5)2N]4Ti), tetrakis(ethylmethylamino)titanium(IV)(Ti[N(C2H5)(CH3)]4), diisopropoxybis(2,2,6,6-tetramethyl-3,5-heptanedione)titanium(IV)(Ti[OCC(CH3)3CHCOC(CH3)3]2(OC3H7)2), titanium tetrachloride (TiCl4), isopropoxytitanium(IV)(Ti[OCH(CH3)2]4), ethoxytitanium(IV)(Ti[O(C2H5)]4), etc.
[0058] Examples of the precursor containing Zr include bis(methyl-η 5 -cyclopentadienyl) methoxymethyl zirconium (Zr(CH3C5H4)2CH3OCH3), tetrakis(dimethylamide) zirconium (IV) ([(CH3)2N]4Zr), tetrakis(ethylmethylamide) zirconium (IV) (Zr(NCH3C2H5)4), tert-butoxy zirconium (IV) (Zr[OC(CH3)3]4), etc.
[0059] Examples of the precursor containing Nb include niobium (V) ethoxide (Nb(OCH2CH3)5, tris(diethylamide)(tert-butylimide)niobium (V) (C 16 H 39 N4Nb) etc.
[0060] As precursors containing Hf, for example, hafnium tetrachloride (HfCl4), tetrakis(dimethylamino)hafnium (Hf[N(CH3)2]4), tetrakis(ethylmethylamino)hafnium (Hf[N(C2H5)(CH3)]4), tetrakis(diethylamino)hafnium (Hf[N(C2H5)2]4), tert-butoxyhafnium (Hf[OC(CH3)3]4), etc. can be mentioned.
[0061] The second metal may be used alone or in combination of two or more. When two or more second metals are used in combination, a precursor containing two or more second metals may be used. In addition, in this case, the type of precursor supplied to the reaction chamber may be changed corresponding to the cycle, thereby changing the type of the second metal deposited in atomic layer units. In this case, a second dielectric layer (composite oxide layer) mixed with oxides of two or more second metals may be formed.
[0062] In addition, the first metal may be used together with the second metal. In this case, a precursor containing the first metal and the second metal may be used. In addition, in this case, the type of precursor supplied to the reaction chamber may be changed corresponding to the cycle, thereby changing the type of metal deposited in atomic layer units. In this case, a second dielectric layer (composite oxide layer) mixed with an oxide of the first metal and an oxide of the second metal may be formed. In the case of the ALD method, it is easy to control the mixing ratio of the oxide of the first metal and the oxide of the second metal in the composite oxide layer.
[0063] The step of forming the second dielectric layer (the third step) is performed after the step of forming the first dielectric layer (the second step). In this case, the first dielectric layer functions as an inhibitory layer for the second dielectric layer. When the first dielectric layer having a thickness of T1 functions as an inhibitory layer for the second dielectric layer having a thickness of T2, the LC value can be reduced to, for example, 1 / 2 or less, compared to the case where the dielectric layer having a thickness equal to the sum of T1 and T2 is formed only by the second dielectric layer.
[0064] If a chemical film is formed as a first dielectric layer between the anode body and the second dielectric layer by performing a chemical treatment after forming the second dielectric layer, the first dielectric layer does not function as an inhibitory layer. In this case, the insulating property of the second dielectric layer is reduced by the chemical treatment performed to form the first dielectric layer, and the LC value increases.
[0065] [Electrolytic capacitors]
[0066] The electrolytic capacitor of the embodiment of the present invention comprises the above-mentioned electrode foil for electrolytic capacitor and the cathode portion covering at least a portion of the second dielectric layer. Hereinafter, the above-mentioned electrode foil for electrolytic capacitor and the cathode portion are also collectively referred to as capacitor element. The cathode portion includes an electrolyte. The electrolyte covers at least a portion of the second dielectric layer. The electrolyte includes at least one of a solid electrolyte and an electrolyte. The cathode portion may include a solid electrolyte and an electrolyte, or may include a solid electrolyte and a solvent (e.g., a polyol compound).
[0067] The solid electrolyte includes a conductive polymer. As the conductive polymer, for example, a π-conjugated polymer can be cited. As the conductive polymer, polypyrrole, polythiophene, polyfuran, polyaniline, etc. can be cited. The conductive polymer can be used alone, or two or more kinds can be used in combination, or it can be a copolymer of two or more monomers. The weight average molecular weight of the conductive polymer is, for example, 1000 to 100000.
[0068] It should be noted that, in this specification, polypyrrole, polythiophene, polyfuran, polyaniline, etc. respectively refer to polymers having polypyrrole, polythiophene, polyfuran, polyaniline, etc. as basic skeletons. Therefore, polypyrrole, polythiophene, polyfuran, polyaniline, etc. may also include their respective derivatives. For example, polythiophene includes poly(3,4-ethylenedioxythiophene) (PEDOT), etc.
[0069] The conductive polymer may be doped with a dopant. Examples of the dopant include polystyrene sulfonic acid (PSS) and the like. The solid electrolyte may further contain an additive as required.
[0070] The electrolyte contains a solvent and an ionic substance (solute (e.g., an organic salt)) dissolved therein. The solvent may be an organic solvent or an ionic liquid. As the solvent, a high boiling point solvent is preferred. For example, polyol compounds such as ethylene glycol, sulfone compounds such as cyclopentane sulfone, lactone compounds such as γ-butyrolactone, ester compounds such as methyl acetate, carbonate compounds such as propylene carbonate, ether compounds such as 1,4-dioxane, ketone compounds such as methyl ethyl ketone, etc. may be used. The solvent may be used alone or in combination of two or more.
[0071] The so-called organic salt is a salt in which at least one of the anion and the cation contains an organic substance. As the organic salt, for example, trimethylamine maleate, triethylamine borodisalicylate, ethyldimethylamine phthalate, 1,2,3,4-tetramethylimidazolinium phthalate, 1,3-dimethyl-2-ethylimidazolinium phthalate, etc. can be used. One organic salt can be used alone, or two or more can be used in combination.
[0072] Here, Figure 2 It is a cross-sectional view schematically showing an electrolytic capacitor according to one embodiment of the present invention. Figure 3 This is a perspective view of a part of the rolled body unfolded.
[0073] The wound electrolytic capacitor 200 includes a capacitor element. The capacitor element includes a wound body 100 and an electrolyte (not shown). The wound body 100 is formed by winding an anode foil 10 and a cathode foil 20 with a separator 30 interposed therebetween. The anode foil 10 is an electrode foil for an electrolytic capacitor of the present invention. There is no particular limitation on the separator 30, and for example, a nonwoven fabric containing fibers of cellulose, polyethylene terephthalate, vinylon, or polyamide can be used.
[0074] One end of lead tabs 50A and 50B is connected to anode foil 10 and cathode foil 20, respectively, and lead tabs 50A and 50B are wound to form winding body 100. Leads 60A and 60B are connected to the other ends of lead tabs 50A and 50B, respectively.
[0075] A winding fixing tape 40 is disposed on the outer surface of the cathode foil 20 located at the outermost layer of the wound body 100, and the end of the cathode foil 20 is fixed by the winding fixing tape 40. It should be noted that when the anode foil 10 is prepared by cutting from a large-sized foil, the wound body 100 may be further subjected to a chemical treatment in order to provide a dielectric layer on the cut surface.
[0076] The electrolyte is contained in the wound body 100 and sandwiched between the anode foil 10 and the cathode foil 20 of the wound body 100. For example, the wound body can be impregnated with a treatment solution (or electrolyte solution) containing a conductive polymer. The impregnation can be performed under reduced pressure, for example, in an atmosphere of 10 kPa to 100 kPa.
[0077] The wound body 100 is housed in the bottomed case 211 so that the leads 60A and 60B are located on the opening side of the bottomed case 211. As the material of the bottomed case 211, metals such as aluminum, stainless steel, copper, iron, and brass, or alloys thereof can be used.
[0078] A sealing member 212 is arranged at the opening of a bottomed casing 211 accommodating the wound body 100 , the open end of the bottomed casing 211 is riveted to the sealing member 212 and curled, and a seat plate 213 is arranged at the curled portion, thereby sealing the wound body 100 in the bottomed casing 211 .
[0079] The sealing member 212 is formed so as to allow the lead wires 60A and 60B to pass through. The sealing member 212 may be made of any insulating material, and is preferably an elastomer. Among them, silicone rubber, fluororubber, ethylene-propylene rubber, Hypalon rubber, butyl rubber, isoprene rubber, etc. having high heat resistance are preferred.
[0080] in addition, Figure 4 It is a cross-sectional view schematically showing an electrolytic capacitor according to another embodiment of the present invention.
[0081] The stacked electrolytic capacitor 400 includes a capacitor element 402, an anode lead terminal 404 and a cathode lead terminal 405 electrically connected to the capacitor element 402, and a resin outer package 403 that seals the capacitor element 402. Anode lead terminal 404 and cathode lead terminal 405 are partially covered by outer package 403. Outer package 403 has an approximately rectangular parallelepiped shape, and electrolytic capacitor 400 also has an approximately rectangular parallelepiped shape.
[0082] The capacitor element 402 includes an anode body (metal foil containing a valve action metal) having a cathode forming portion 406a and an anode lead portion 406b, a dielectric layer 407 covering the cathode forming portion 406a, and a cathode portion 408 covering the dielectric layer 407. The anode body has a porous portion on the surface, and the dielectric layer 407 is formed so as to cover the surface of the porous portion of the cathode forming portion 406. The anode foil 460 includes the cathode forming portion 406a of the anode body and the dielectric layer 407. The anode foil 460 is an electrode foil for an electrolytic capacitor of the present invention.
[0083] An insulating separation layer 413 is formed in a portion of the anode lead portion 406b adjacent to the cathode portion 408 to limit contact between the cathode portion 408 and the anode foil 460. The anode lead portion 406b is electrically connected to the anode lead terminal 404 by welding. The cathode lead terminal 405 is electrically connected to the cathode portion 408 via an adhesive layer 414 formed of a conductive adhesive.
[0084] The cathode portion 408 includes a solid electrolyte layer 409 covering the dielectric layer 407 and a cathode extraction layer 410 covering the solid electrolyte layer 409. The solid electrolyte layer 409 includes a conductive polymer and may include a dopant, etc. as required. The solid electrolyte layer 409 can be formed, for example, by impregnating the anode foil 460 with a treatment solution containing a conductive polymer.
[0085] The cathode lead layer 410 includes a carbon layer 411 and a silver paste layer 412. The carbon layer 411 includes, for example, carbon particles and silver. The silver paste layer 412 includes, for example, silver particles and a binder. The binder is not particularly limited, but a cured product of a curable resin is preferred. As the curable resin, for example, a thermosetting resin such as an epoxy resin can be cited.
[0086] The outer package 403 preferably contains a cured product of a curable resin composition, and may contain a thermoplastic resin or a composition containing the thermoplastic resin. Examples of the curable resin include thermosetting resins such as epoxy resins.
[0087] As the anode body, a porous sintered body obtained by sintering particles containing a valve acting metal may be used instead of the metal foil containing a valve acting metal whose surface is roughened. A part of a metal lead member is embedded in the porous sintered body.
[0088] Example
[0089] Hereinafter, the present invention will be described in more detail based on examples, but the present invention is not limited to the examples.
[0090] 《Examples 1 to 3, Comparative Example 7》
[0091] A wound electrolytic capacitor (diameter Φ6.3 mm×length L9.9 mm) was produced with a rated voltage of 2.0 V. A specific method for producing the electrolytic capacitor will be described below.
[0092] (Manufacturing of anode foil)
[0093] (Step 1: Preparation of anode body)
[0094] An Al foil having a thickness of 120 μm was prepared, and the surface of the Al foil was roughened by etching to form a porous portion (thickness of 40 μm per surface, pore diameter of pits of 100 to 200 nm).
[0095] (Second step: formation of first dielectric layer)
[0096] The first dielectric layer (first metal oxide layer) was formed on the surface of the anode body by the ALD method (temperature: 150°C, precursor: precursor containing Si, oxidant: O3, pressure: 1 Pa). Tris(dimethylamino)silane was used as a precursor containing Si to form Si oxide (SiO x The number of cycles was appropriately adjusted to set the thickness T1 of the first dielectric layer to the value shown in Table 1.
[0097] (Third Step: Formation of Second Dielectric Layer)
[0098] The second dielectric layer (second metal oxide layer) was formed on the surface of the first dielectric layer by the ALD method (temperature: 150° C., precursor: a precursor containing Ti and a precursor containing Al, oxidant: H 2 O, pressure: 1 Pa).
[0099] Tetrakis(dimethylamino)titanium(IV) was used as a precursor containing Ti, and trimethylaluminum was used as a precursor containing Al. Six cycles were set as one group, and in each group, the precursor containing Ti was supplied for 5 cycles and the precursor containing Al was supplied for 1 cycle. In this way, a composite oxide layer (Ti-Al-O) in which TiO2 and Al2O3 were mixed in a molar ratio of 5:1 was formed.x ). The number of cycles (number of groups) was appropriately adjusted to set the thickness T2 of the second dielectric layer to the value shown in Table 1.
[0100] The anode foil is obtained as described above. Thereafter, the anode foil is cut into a given size.
[0101] The first dielectric layer and the second dielectric layer were confirmed by the above-mentioned method. The thickness T1 of the first dielectric layer and the thickness T2 of the second dielectric layer shown in Table 1 were determined by the above-mentioned method.
[0102] (Manufacturing of cathode foil)
[0103] An Al foil having a thickness of 50 μm was etched to roughen the surface of the Al foil to obtain a cathode foil. Thereafter, the cathode foil was cut into a predetermined size.
[0104] (Production of wound body)
[0105] Anode lead tabs and cathode lead tabs are connected to the anode foil and cathode foil, and the anode foil and cathode foil are wound with separators interposed therebetween while being wound into the lead tabs. Anode leads and cathode leads are connected to the ends of the lead tabs protruding from the wound body.
[0106] Thereafter, the produced winding body was subjected to a chemical conversion treatment to form a chemical conversion film (dielectric layer) on the cut end of the anode foil. An ammonium adipate solution (concentration 7 mass %, temperature 70° C.) was used as a chemical conversion solution and the chemical conversion treatment was performed at a chemical conversion voltage Vf of 8.5 V. Then, the end of the outer surface of the winding body was fixed with a winding fixing tape.
[0107] (Preparation of Conductive Polymer Dispersion)
[0108] A mixed solution was prepared by dissolving 3,4-ethylenedioxythiophene and polystyrene sulfonic acid as a dopant in ion exchange water. While stirring the obtained mixed solution, iron (III) sulfate (oxidant) dissolved in ion exchange water was added to carry out a polymerization reaction. After the reaction, the obtained reaction solution was dialyzed to remove unreacted monomers and excess oxidant, thereby obtaining a conductive polymer dispersion containing polyethylenedioxythiophene doped with about 5% by mass of polystyrene sulfonic acid.
[0109] (Formation of Solid Electrolyte Layer)
[0110] In a reduced pressure atmosphere (40 kPa), the winding body is immersed in a conductive polymer dispersion contained in a predetermined container for 5 minutes, and then the winding body is lifted from the conductive polymer dispersion. Then, the winding body impregnated with the conductive polymer dispersion is dried in a drying oven at 150° C. for 20 minutes to form a solid electrolyte layer containing a conductive polymer between the anode foil and the cathode foil. A capacitor element is obtained as described above.
[0111] (Sealing of capacitor elements)
[0112] The capacitor element is placed in a bottom housing, and the capacitor element is sealed using a sealing member and a seat plate to complete the electrolytic capacitor. Thereafter, the rated voltage is applied and the aging treatment is performed at 130°C for 2 hours. It should be noted that A1 to A3 in Table 1 are electrolytic capacitors of Examples 1 to 3, respectively. X7 in Table 1 is the electrolytic capacitor of Comparative Example 7.
[0113] 《Examples 4-5, Comparative Example 8》
[0114] (Formation of the First Dielectric Layer)
[0115] The first dielectric layer (first metal oxide layer) was formed on the surface of the anode body by the ALD method (temperature: 150°C, precursor: precursor containing Al, oxidant: H2O, pressure: 1 Pa). Trimethylaluminum was used as a precursor containing Al to form Al oxide (AlO x The number of cycles was appropriately adjusted to set the thickness T1 of the first dielectric layer to the value shown in Table 1.
[0116] (Formation of Second Dielectric Layer)
[0117] The second dielectric layer (second metal oxide layer) was formed on the surface of the first dielectric layer by the ALD method (temperature: 150° C., precursor: a precursor containing Ti and a precursor containing Al, oxidant: H 2 O, pressure: 1 Pa).
[0118] Tetrakis(dimethylamino)titanium(IV) was used as a precursor containing Ti, and trimethylaluminum was used as a precursor containing Al. Six cycles were set as one group, and in each group, the precursor containing Ti was supplied for 5 cycles and the precursor containing Al was supplied for 1 cycle. In this way, a composite oxide layer (Ti-Al-O) in which TiO2 and Al2O3 were mixed in a molar ratio of 5:1 was formed. x ). The number of cycles (number of groups) was appropriately adjusted to set the thickness T2 of the second dielectric layer to the value shown in Table 1.
[0119] Except for the above, electrolytic capacitors B1 and B2 of Examples 4 and 5 and an electrolytic capacitor X8 of Comparative Example 8 were produced by the same method as the electrolytic capacitor A1 of Example 1.
[0120] Comparative Example 1
[0121] The second dielectric layer was formed on the surface of the anode body without forming the first dielectric layer. The second dielectric layer was formed by ALD (temperature: 150°C, precursor: tetrakis(dimethylamino)titanium(IV), oxidant: H2O, pressure: 1Pa) to form Ti oxide (TiO x The number of cycles was appropriately adjusted to set the thickness of the second dielectric layer to the value shown in Table 1.
[0122] An electrolytic capacitor X1 was produced by the same method as the electrolytic capacitor A1 of Example 1 except for the above.
[0123] Comparative Example 2
[0124] The second dielectric layer was formed on the surface of the anode body without forming the first dielectric layer. The number of cycles was appropriately adjusted so that the thickness of the second dielectric layer was set to the value shown in Table 1.
[0125] An electrolytic capacitor X2 was produced by the same method as the electrolytic capacitor A1 of Example 1 except for the above.
[0126] Comparative Example 3
[0127] (Formation of Second Dielectric Layer)
[0128] The second dielectric layer was formed on the surface of the anode body by the ALD method (temperature: 150° C., precursor: a precursor containing Ti and a precursor containing Al, oxidant: H 2 O, pressure: 1 Pa).
[0129] Tetrakis(dimethylamino)titanium(IV) was used as a precursor containing Ti, and trimethylaluminum was used as a precursor containing Al. 12 cycles were set as one group, and in each group, 11 cycles were performed to supply the precursor containing Ti, and 1 cycle was performed to supply the precursor containing Al. In this way, a composite oxide layer (Ti-Al-O) in which TiO2 and Al2O3 were mixed in a molar ratio of 11:1 was formed. x ) as the second dielectric layer. The number of cycles (number of groups) was appropriately adjusted to set the thickness T2 of the second dielectric layer to the value shown in Table 1.
[0130] (Formation of the First Dielectric Layer)
[0131] The anode body having the second dielectric layer on the surface is subjected to a chemical conversion treatment to form a chemical conversion film (AlO x) as the first dielectric layer. An ammonium adipate solution (concentration 7 mass %, temperature 70° C.) was used as the chemical conversion solution. The chemical conversion voltage Vf was appropriately adjusted to set the thickness T1 of the first dielectric layer (chemical conversion film) to the value shown in Table 1.
[0132] An electrolytic capacitor X3 of Comparative Example 3 was produced by the same method as the electrolytic capacitor A1 of Example 1 except for the above.
[0133] 《Comparative Example 4》
[0134] (Formation of Second Dielectric Layer)
[0135] The second dielectric layer was formed on the surface of the anode body by the ALD method (temperature: 150° C., precursor: a precursor containing Ti and a precursor containing Al, oxidant: H 2 O, pressure: 1 Pa).
[0136] Tetrakis(dimethylamino)titanium(IV) was used as a precursor containing Ti, and trimethylaluminum was used as a precursor containing Al. Six cycles were set as one group, and in each group, the precursor containing Ti was supplied for 5 cycles and the precursor containing Al was supplied for 1 cycle. In this way, a composite oxide layer (Ti-Al-O) in which TiO2 and Al2O3 were mixed in a molar ratio of 5:1 was formed. x ) as the second dielectric layer. The number of cycles (number of groups) was appropriately adjusted to set the thickness T2 of the second dielectric layer to the value shown in Table 1.
[0137] (Formation of the First Dielectric Layer)
[0138] The anode body having the second dielectric layer on the surface was subjected to a chemical treatment to form a layer of a chemical film (AlOx) between the anode body and the second dielectric layer as the first dielectric layer. An ammonium adipate solution (concentration 7 mass %, temperature 70° C.) was used as the chemical solution. The chemical voltage Vf was appropriately adjusted to set the thickness T1 of the first dielectric layer (chemical film) to the value shown in Table 1.
[0139] An electrolytic capacitor X4 of Comparative Example 4 was produced by the same method as the electrolytic capacitor A1 of Example 1 except for the above.
[0140] 《Comparative Example 5》
[0141] (Formation of the First Dielectric Layer)
[0142] The first dielectric layer was formed on the surface of the anode body by the ALD method (temperature: 150° C., precursor: a precursor containing Ti and a precursor containing Al, oxidant: H 2 O, pressure: 1 Pa).
[0143] Tetrakis(dimethylamino)titanium(IV) was used as a precursor containing Ti, and trimethylaluminum was used as a precursor containing Al. Six cycles were set as one group, and in each group, the precursor containing Ti was supplied for 5 cycles and the precursor containing Al was supplied for 1 cycle. In this way, a composite oxide layer (Ti-Al-O) in which TiO2 and Al2O3 were mixed in a molar ratio of 5:1 was formed. x ) as the first dielectric layer. The number of cycles (number of groups) was appropriately adjusted to set the thickness T1 of the first dielectric layer to the value shown in Table 1.
[0144] (Formation of Second Dielectric Layer)
[0145] By using the ALD method (temperature: 150° C., precursor: precursor containing Si, oxidant: O 3 , pressure: 1 Pa), Si oxide (SiO x ) as the second dielectric layer. Tris(dimethylamino)silane was used as a precursor containing Si. The number of cycles was appropriately adjusted to set the thickness T2 of the second dielectric layer to the value shown in Table 1.
[0146] An electrolytic capacitor X5 of Comparative Example 5 was produced by the same method as the electrolytic capacitor A1 of Example 1 except for the above.
[0147] 《Comparative Example 6》
[0148] The anode body is subjected to chemical treatment to form a chemical film (AlO x ) as the first dielectric layer. The anode body is immersed in an ammonium adipate solution and a forming voltage Vf is applied to the anode body to perform a forming treatment. The forming voltage Vf is appropriately adjusted to set the thickness T1 of the first dielectric layer (formed film) to the value shown in Table 1. Thereafter, the second dielectric layer is not formed.
[0149] An electrolytic capacitor X6 of Comparative Example 6 was produced by the same method as the electrolytic capacitor A1 of Example 1 except for the above.
[0150] [evaluate]
[0151] For each electrolytic capacitor of the embodiment and the comparative example, the breakdown voltage, electrostatic capacitance and leakage current were measured at 20°C. Specifically, the voltage was applied while increasing the voltage at a rate of 1.0V / second, and the breakdown voltage of an overcurrent of 0.5A was measured. The electrostatic capacitance at a frequency of 120Hz was measured using a 4-terminal LCR tester. The current flowing through the electrolytic capacitor when the rated voltage was maintained for 40 seconds was measured, and the current value was set as the leakage current.
[0152] The electrostatic capacitance is expressed as an index (capacitance index C) with the electrostatic capacitance of the electrolytic capacitor X6 of Comparative Example 6 being 100. The breakdown voltage is expressed as an index (voltage withstand index V) with the breakdown voltage of the electrolytic capacitor X6 of Comparative Example 6 being 100. The leakage current is expressed as an index (LC index) with the leakage current of the electrolytic capacitor X6 of Comparative Example 6 being 100.
[0153] The evaluation results are shown in Table 1. Table 1 also shows the CV value. The CV value is a value obtained by multiplying the electrostatic capacitance by the breakdown voltage, and indicates the amount of electricity that can be stored in the electrolytic capacitor. The CV value is expressed in the form of an index (CV index) with the CV value of the electrolytic capacitor X6 of Comparative Example 6 being 100.
[0154] [Table 1]
[0155]
[0156] In electrolytic capacitors A1 to A3 and B1 to B2, it is possible to suppress the increase of LC while increasing the capacity, thereby achieving large capacity and low LC at the same time. In electrolytic capacitors A1 to A3 and B1 to B2, the decrease of withstand voltage index V is also suppressed. In electrolytic capacitors X1 to X8, it is not possible to achieve large capacity and low LC at the same time.
[0157] In the electrolytic capacitors X1 and X2, since the first dielectric layer is not formed, the insulation of the second dielectric layer is reduced by the chemical conversion treatment of the wound body, the LC index increases, and the withstand voltage index V decreases.
[0158] In the electrolytic capacitors X3 and X4, since the first dielectric layer is formed by chemical formation after the second dielectric layer is formed, the first dielectric layer does not function as an inhibitory layer, and the insulation of the second dielectric layer is reduced by the chemical formation performed for the formation of the first dielectric layer, the LC index increases, and the withstand voltage index V decreases. In the electrolytic capacitor X3, the molar ratio of Ti / Al in the second dielectric layer is larger than that of the electrolytic capacitor X4, and the LC index is further increased.
[0159] In the electrolytic capacitor X5, since the second metal oxide layer is formed as the first dielectric layer and the first metal oxide layer is formed as the second dielectric layer, there is no inhibition layer between the second metal oxide layer and the anode body. The insulation of the second metal oxide layer is reduced due to the chemical treatment performed on the winding body, the LC index is increased, and the withstand voltage index V is reduced.
[0160] In the electrolytic capacitor X6, since the dielectric layer is constituted by only the first dielectric layer, the capacitance index C is reduced. In the electrolytic capacitors X7 and X8, T1 / T2 is greater than 1, and the capacitance index C is reduced.
[0161] Industrial Applicability
[0162] The electrode foil for electrolytic capacitors of the present invention can be suitably used in electrolytic capacitors that require large capacitance and low LC.
[0163] Although the present invention has been described with respect to the present preferred embodiments, such disclosure should not be construed in a limiting sense. Upon reading the above disclosure, various modifications and changes will undoubtedly be apparent to those skilled in the art in the technical field to which the present invention belongs. Therefore, the scope of the appended claims should be interpreted as including all modifications and changes without departing from the true spirit and scope of the present invention.
[0164] Description of Reference Numerals
[0165] 10 anode foil, 110 anode body, 111 core, 112 porous part, 120 dielectric layer, 121 first dielectric layer, 122 second dielectric layer, P pit, 20 cathode foil, 30 spacer, 40 winding fixing tape, 60A, 60B lead wires, 50A, 50B lead terminals, 100 winding body, 200 wound electrolytic capacitor, 211 bottom casing, 212 sealing member, 213 seat plate, 400 laminated electrolytic capacitor, 402 capacitor element, 403 outer packaging body, 404 anode lead terminal, 405 cathode lead terminal, 406a cathode forming part, 406b anode lead-out part, 407 dielectric layer, 408 cathode part, 409 solid electrolyte layer, 410 cathode lead-out layer, 411 carbon layer, 412 silver paste layer, 413 separation layer, 414 adhesive layer, 460 anode foil.
Claims
1. An electrode foil for an electrolytic capacitor, comprising: An anode body comprising a valve action metal, a first dielectric layer covering at least a portion of the anode body, and a second dielectric layer covering at least a portion of the first dielectric layer, The second dielectric layer has a higher dielectric constant than the first dielectric layer. The thickness T2 of the second dielectric layer is greater than the thickness T1 of the first dielectric layer. The first dielectric layer is a layer that suppresses diffusion of oxygen from the second dielectric layer into the anode body.
2. The electrode foil for electrolytic capacitor according to claim 1, wherein The first dielectric layer includes a first metal oxide. The second dielectric layer includes a second metal oxide having a higher dielectric constant than the first metal oxide.
3. The electrode foil for electrolytic capacitor according to claim 2, wherein: The second metal oxide includes at least one second metal selected from the group consisting of tantalum, titanium, zirconium, niobium, and hafnium.
4. The electrode foil for electrolytic capacitor according to claim 3, wherein The second metal oxide includes the second metal and at least one selected from silicon and aluminum.
5. The electrode foil for electrolytic capacitor according to any one of claims 2 to 4, wherein The first metal oxide includes at least one first metal selected from silicon and aluminum.
6. The electrode foil for electrolytic capacitor according to claim 5, wherein The first metal includes silicon, A ratio of a thickness T1 of the first dielectric layer to a thickness T2 of the second dielectric layer: T1 / T2 is 0.45 or less.
7. The electrode foil for electrolytic capacitor according to claim 5, wherein The first metal includes aluminum, A ratio of a thickness T1 of the first dielectric layer to a thickness T2 of the second dielectric layer: T1 / T2 is 0.6 or less.
8. The electrode foil for electrolytic capacitor according to any one of claims 1 to 7, wherein The thickness T1 of the first dielectric layer is greater than or equal to 0.3 nm. 9 . An electrolytic capacitor comprising: the electrode foil for an electrolytic capacitor according to claim 1 ; and a cathode portion covering at least a portion of the second dielectric layer.
10. The electrolytic capacitor according to claim 9, wherein: The cathode portion includes an electrolyte.
11. The electrolytic capacitor according to claim 9, wherein: The cathode portion includes a solid electrolyte.
12. A method for manufacturing an electrode foil for an electrolytic capacitor, the method comprising: In the first step, an anode body including a valve metal is prepared; A second step of forming a first dielectric layer covering at least a portion of the anode body; as well as a third step of forming a second dielectric layer covering at least a portion of the first dielectric layer after the second step; The second dielectric layer has a higher dielectric constant than the first dielectric layer. The thickness T2 of the second dielectric layer is greater than the thickness T1 of the first dielectric layer. The first dielectric layer is a layer that suppresses diffusion of oxygen from the second dielectric layer into the anode body.
13. The method for producing an electrode foil for an electrolytic capacitor according to claim 12, wherein: In the second step, the first dielectric layer is formed by atomic layer deposition or chemical conversion.
14. The method for producing an electrode foil for an electrolytic capacitor according to claim 12 or 13, wherein: In the third step, the second dielectric layer is formed by atomic layer deposition.
15. The method for producing an electrode foil for an electrolytic capacitor according to any one of claims 12 to 14, wherein: The first dielectric layer includes a first metal oxide, The second dielectric layer includes a second metal oxide having a higher dielectric constant than the first metal oxide.
16. The method for producing an electrode foil for an electrolytic capacitor according to claim 15, wherein: The second metal oxide includes at least one second metal selected from the group consisting of tantalum, titanium, zirconium, niobium, and hafnium.
17. The method for producing an electrode foil for an electrolytic capacitor according to claim 16, wherein: The second metal oxide includes the second metal and at least one selected from silicon and aluminum.
18. The method for producing an electrode foil for an electrolytic capacitor according to any one of claims 15 to 17, wherein: The first metal oxide includes at least one first metal selected from silicon and aluminum.
19. The method for producing an electrode foil for an electrolytic capacitor according to claim 18, wherein: The first metal includes silicon, A ratio of a thickness T1 of the first dielectric layer to a thickness T2 of the second dielectric layer: T1 / T2 is 0.45 or less.
20. The method for producing an electrode foil for an electrolytic capacitor according to claim 18, wherein: The first metal includes aluminum, A ratio of a thickness T1 of the first dielectric layer to a thickness T2 of the second dielectric layer: T1 / T2 is 0.6 or less.
21. The method for producing an electrode foil for an electrolytic capacitor according to any one of claims 12 to 20, wherein: The thickness T1 of the first dielectric layer is greater than or equal to 0.3 nm.
Citation Information
Patent Citations
Electrolytic capacitor manufacturing method and electrolytic capacitor
JP2012043960A