Wafer bend compensation by patterned UV curing
By depositing stress-tunable films on semiconductor substrates and using patterned quartz windows for selective UV exposure, the problem of asymmetric bending in 3D-NAND manufacturing is solved, improving the precision and uniformity of photolithography etching and avoiding processing problems caused by warping.
Patent Information
- Application Number
- CN202380024044.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-28
- Filing Date
- 2023-02-10
- Publication Date
- 2024-11-01
AI Technical Summary
Existing technologies are insufficient to effectively alleviate the asymmetric bending problem of semiconductor wafers during 3D-NAND manufacturing, leading to mismatch in photolithography coverage and wafer warping exceeding the clamping limit of the electrostatic chuck, which affects the uniformity and accuracy of subsequent processing.
By depositing stress-tunable films on the front or back of a semiconductor substrate and selectively exposing them to UV light using patterned quartz windows, the local stress of the stress-tunable films can be adjusted to alleviate wafer bending.
It effectively regulates local stress in semiconductor substrates, reduces wafer bending, improves the precision and uniformity of photolithography etching, and avoids uneven processing and equipment jamming problems caused by warping.
Smart Images

Figure CN118891706A_ABST
Abstract
Description
Incorporation by Reference
[0001] The PCT application form is filed concurrently with this specification as a part of this application. Each application identified in the concurrently filed PCT application form to which this application claims the benefit or priority is incorporated herein by reference in its entirety and for all purposes. Background Art
[0002] Semiconductor manufacturing processes involve many deposition and etching operations, which can greatly change the wafer bow. For example, in 3D-NAND manufacturing, which is gradually replacing 2D-NAND chips due to lower cost and higher reliability in various applications, multi-layer stacked films with thick, highly stressed carbon-based hard masks and / or metallization lines may cause significant wafer warpage, leading to front-side lithography overlay mismatch, or even wafer bow beyond the clamping limit of the electrostatic chuck.
[0003] The background description provided here is for the purpose of generally presenting the background of the present disclosure. The work of the currently designated inventors within the scope described in this background section and aspects of the specification that could not be determined as prior art at the time of filing the application are neither explicitly nor implicitly admitted to be prior art against the present disclosure. Summary of the invention
[0004] Provided herein is a device for selective UV exposure. The device includes an ultraviolet (UV) light source and a processing chamber. The processing chamber includes a substrate support configured to support a semiconductor substrate, and one or more heating elements configured to control the temperature of the semiconductor substrate, wherein the semiconductor substrate includes a stress-adjustable film. The device further includes a window positioned between the substrate support and the UV light source, wherein the window is patterned to have one or more UV transparent regions for selectively exposing one or more first regions of the stress-adjustable film to UV light and one or more UV opaque regions for selectively blocking UV light for one or more second regions of the stress-adjustable film.
[0005] In some implementations, the window is patterned with a metal coating corresponding to one or more UV opaque areas. In some implementations, the metal coating comprises silver, aluminum, or a combination thereof. In some implementations, the window is patterned with a ceramic cover configured on the window and corresponding to one or more UV opaque areas. In some implementations, the ceramic cover comprises aluminum nitride or aluminum oxide. In some implementations, the window is patterned with a metal cover configured on the window and corresponding to one or more UV opaque areas. In some implementations, the window is further patterned with one or more transition zones lining an interface between one or more UV transparent areas and one or more UV opaque areas, wherein one or more transition zones are semi-transparent to UV light or contain a grid pattern of UV transparent and UV opaque materials. In some implementations, one or more transition zones contain a metal layer having a thickness of less than about 100nm. In some implementations, one or more transition zones are configured to provide a more graduated stress change at an interface between one or more first zones of the stress-adjustable film and one or more second zones of the stress-adjustable film. In some implementations, one or more UV transparent zones are configured to induce a stress shift in one or more first zones of the stress-adjustable film in an amount equal to or greater than about 50%. In some implementations, the UV light source is configured to direct UV light to the back side of a semiconductor substrate, wherein the stress-adjustable film is formed on the back side of the semiconductor substrate. In some implementations, the UV light source is configured to direct UV light to the front side of the semiconductor substrate, wherein the stress-adjustable film is formed on the front side of the semiconductor substrate. The device further includes a controller configured to have instructions for performing the following operations: providing a semiconductor substrate in a processing chamber, and selectively exposing one or more first zones of the stress-adjustable film to UV light using a patterned window so as to locally adjust the stress on the stress-adjustable film. In some implementations, the stress tunable film includes silicon nitride, silicon oxide, silicon oxynitride, or silicon carbonitride, and the window includes quartz.
[0006] Also provided herein is a method of selective UV exposure. The method includes providing a semiconductor substrate on a substrate support in a processing chamber, wherein the semiconductor substrate includes a stress-adjustable film, wherein a quartz window is positioned between the processing chamber and an ultraviolet (UV) light source, wherein the quartz window is patterned to have one or more UV transparent regions and one or more UV opaque regions. The method further includes selectively exposing one or more first regions of the stress-adjustable film to UV light via the one or more UV transparent regions of the quartz window, and selectively blocking the UV light for one or more second regions of the stress-adjustable film through the one or more UV opaque regions of the quartz window.
[0007] In some implementations, selectively exposing one or more first regions of the stress-adjustable film includes locally adjusting the stress in the one or more first regions of the stress-adjustable film. In some implementations, the quartz window is patterned to have a metal coating corresponding to one or more UV opaque regions. In some implementations, the quartz window is patterned to have a ceramic cover or a metal cover configured on the quartz window and corresponding to one or more UV opaque regions. In some implementations, the quartz window is further patterned to have one or more transition regions between one or more UV transparent regions and one or more UV opaque regions, wherein the one or more transition regions are translucent to UV light. In some implementations, the one or more transition regions include a metal layer having a thickness of less than about 100 nm. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1 A perspective view of a curved semiconductor substrate is shown illustrating wafer bow in the x-axis direction and the y-axis direction.
[0009] Figure 2 A top view schematic diagram of an exemplary system for mitigating wafer bow using a partitioned mask adjacent to a semiconductor substrate is shown.
[0010] Figure 3 A top view schematic diagram of an exemplary system for mitigating wafer bow using a multi-plenum showerhead is shown.
[0011] Figure 4A A schematic diagram of an exemplary apparatus for UV treatment is shown, the apparatus comprising a window positioned between a UV source and a semiconductor substrate.
[0012] Figure 4B Display pair Figure 4A Top view of a UV radiation transparent window.
[0013] Figure 5A A schematic diagram of an exemplary apparatus for UV processing is shown, the apparatus including a patterned window positioned between a UV source and a semiconductor substrate according to some implementations.
[0014] Figure 5B A metal coating is shown according to some implementations. Figure 5A Schematic cross-sectional view of a patterned window.
[0015] Figure 5C A ceramic cover is shown according to some implementations. Figure 5A Schematic cross-sectional view of a patterned window.
[0016] Fig. 6A Shown is a top view schematic of a patterned window having UV transparent areas and UV opaque areas according to some implementations.
[0017] Figure 6B A schematic top view of a patterned window having UV transparent regions occupying a larger surface area than UV opaque regions is shown according to some implementations.
[0018] Figure 6C Shown is a top view schematic of a patterned window having UV transparent regions, UV opaque regions, and a transition region that is semi-transparent to UV radiation according to some implementations.
[0019] Fig.6D Shown is a top view schematic of a patterned window having UV transparent regions, UV opaque regions, and a transition region made of a grid-like mesh according to some implementations.
[0020] Figure 7 A schematic diagram of an exemplary apparatus for UV backside processing is shown, the apparatus including a patterned window positioned between a UV source and a semiconductor substrate according to some implementations.
[0021] Figure 8 A flow chart is shown of an exemplary method of selective UV exposure according to some implementations.
[0022] Fig. 9 A schematic diagram of an exemplary apparatus for selective UV exposure of a stress-tunable film according to some implementations is shown.
[0023] Fig.10 A schematic diagram of an exemplary processing tool for performing selective UV exposure operations according to some implementations is shown. DETAILED DESCRIPTION
[0024] In the present disclosure, the terms "semiconductor wafer", "wafer", "substrate", "wafer substrate" and "partially manufactured integrated circuit" are used interchangeably. It should be understood by those of ordinary skill in the art that the term "partially manufactured integrated circuit" can refer to a silicon wafer during any of the many stages of integrated circuit manufacturing. Wafers or substrates used in the semiconductor device industry typically have a diameter of 200 mm, or 300 mm, or 450 mm. The following detailed description assumes that the present disclosure is implemented on a wafer. However, the present disclosure is not limited thereto. The workpiece can have a variety of shapes, sizes, and materials.
[0025] Semiconductor manufacturing processes involve the formation of various structures, many of which can be two-dimensional. As semiconductor device dimensions shrink and devices become scaled smaller, the density of features on semiconductor substrates increases, resulting in the etching and deposition of material layers in various ways, including three dimensions. For example, 3D-NAND is an increasingly popular technology because it offers lower cost, higher storage density, and greater reliability in a variety of applications compared to other technologies (such as 2D-NAND). Wafer bow can vary dramatically during the manufacturing process of 3D-NAND structures. For example, the deposition of thick hard mask materials and the etching of trenches along the surface of the wafer can cause wafer bow when manufacturing 3D-NAND structures.
[0026] As film layers are stacked on top of each other during the manufacturing process, more stress is introduced into the semiconductor wafer, which can cause bowing. Bowing can have various shapes. In a concave wafer (sometimes called a "smiling wafer" or a curved wafer), the lowest point is the center of the wafer and the highest point is the edge of the wafer. In a convex wafer (sometimes called a "sad wafer" or a dome-shaped wafer), the lowest point is the edge of the wafer and the highest point is the center of the wafer.
[0027] Bowing can be measured using optical techniques. Wafer bowing can be measured or assessed by obtaining a wafer map or stress map. Bowing can be quantified using a bow value or warp value as described herein, which is measured as the vertical distance between the lowest point of the semiconductor wafer to the highest point on the wafer. The warp value can be along one or more axes, for example, an asymmetrically warped wafer may have an x-axis warp and / or a y-axis warp.
[0028] In a curved wafer, the lowest point is the center of the wafer and the highest point is the edge of the wafer. In a domed wafer, the lowest point is the edge of the wafer and the highest point is the center of the wafer. Curved and domed wafers have symmetrical or substantially symmetrical curvature. Wafers may also have asymmetrical curvature. In asymmetrical curvature, the warp is measured along the x-axis and the y-axis. Asymmetrically curved wafers have different x-axis warp values and y-axis warp values. In some cases, an asymmetrically curved wafer has a negative x-axis warp and a positive y-axis warp. In some cases, an asymmetrically curved wafer has a positive x-axis warp and a negative y-axis warp. In some cases, an asymmetrically curved wafer has both a positive x-axis warp and a positive y-axis warp, but the warp values are different. In some cases, an asymmetrically curved wafer has both a negative x-axis warp and a negative y-axis warp, but the warp values are different. An example of an asymmetrically curved wafer is a saddle-shaped wafer. For a saddle-shaped wafer, in one example, the warp on the x-axis may be +200 μm and the warp on the y-axis may be -200 μm. A saddle-shaped wafer has two opposing edges of the wafer that are curved upward, while the other two opposing edges of the wafer are curved downward. As used herein, warp may refer to any deviation from planarity exhibited by a wafer, wherein curved wafers, dome-shaped wafers, and saddle-shaped wafers are examples of different types of warp in a wafer.
[0029] If the substrate is warped, the warping may cause many problems in subsequent processing. For example, in a lithography process, if the substrate is warped, etching may be uneven. This may cause problems related to defocusing and coverage degradation, resulting in significant yield losses. High bowing may be caused by the deposition of thick, highly stressed hard mask layers. In addition, due to the presence of multilayer stacked films and thick, highly stressed hard masks used in such manufacturing processes, etching may cause some asymmetric warping, while the deposition process may cause significant wafer warping, with warping ranging from +500μm to -1300μm. For example, an ashable hard mask can have a stress value of up to -1000MPa and a bow value of up to -1000μm. In some cases, high aspect ratio slit etching and metal filling (e.g., tungsten filling) can induce large anisotropic stresses on the semiconductor substrate.
[0030] Addressing this wafer warpage can be a challenge because subsequent or downstream processing may be affected by wafer warpage of more than ±200 μm, more than ±300 μm, or more than ±500 μm. For example, mechanical wafer processing may be affected by wafer warpage, where an uneven wafer may not be effectively clamped or held by a wafer robot or wafer handling mechanism. In addition, wafer warpage may cause processing non-uniformity, where downstream etching, deposition, or cleaning operations may be adversely affected due to processing non-uniformity on the wafer surface. In some cases, processing a highly warped wafer may cause further warpage. For example, etching a groove in one direction may cause asymmetrically curved warpage due to asymmetric stresses on the wafer. In addition, lithography operations may be adversely affected by wafer warpage because precise patterns cannot be formed. When the wafer is used in subsequent processing involving clamping the wafer into an electrostatic chuck, a highly warped wafer may not be processed in certain tools. Many electrostatic chucks have a "chucking limit" that is defined as the maximum warpage tolerated before the wafer cannot be effectively clamped. For example, the chucking limit of some electrostatic chucks is about ±300 μm. In this case, a warped wafer that exceeds the clamping limit may not be processed.
[0031] Figure 1 A perspective view of a curved semiconductor substrate is shown, which shows the curvature of the wafer in the x-axis direction and the y-axis direction. The curved semiconductor substrate is superimposed in a three-dimensional (3-D) coordinate system, the reference plane of the curved semiconductor substrate is defined by the x-axis direction and the y-axis direction, and the u-axis represents the warpage. Figure 1 As shown, the curved semiconductor substrate is asymmetrically curved, meaning that the x-axis warp value and the y-axis warp value are different. This produces a saddle-shaped curvature. As described above, warp refers to any deviation from planarity exhibited by a semiconductor substrate, with a saddle-shaped wafer representing an example of warpage in a semiconductor substrate.
[0032] As 3D-NAND technology continues to scale and high aspect ratio features become increasingly common, new challenges related to local stress and inter-die stress variations on semiconductor substrates are emerging. Local stress and inter-die stress variations may lead to block bending, cell cross-talk, cell loss, and / or cell misalignments. Local stress refers to stress changes that occur within a wafer in a non-uniform manner. Poorly compensated / corrected local stress may lead to changes in local wafer topology, which in turn may lead to poor alignment during lithography etching. Such poor alignment is usually observed in terms of in-plane distortion (IPD), which quantifies the vector displacement of alignment marks on the wafer from their expected positions due to the wafer topology. High IPD during lithography etching may lead to undesirable changes in critical dimensions or any other features defined in the lithography etching step, which may cause the above-mentioned phenomena of block bending, cell cross-talk, cell loss, and / or cell misalignments due to lithography etching errors.
[0033] Certain techniques exist for addressing symmetrical bowing of semiconductor wafers, and in some cases, techniques can be used to reduce warping by changing the process of manufacturing the desired layers in the substrate. Techniques for addressing symmetrical bowing of semiconductor substrates may involve deposition of a bow compensation layer on the back side of the semiconductor substrate. Application of a bow compensation layer on the back side of a semiconductor substrate has been largely limited to monotonic global wafer warpage mitigation. In other words, such techniques for addressing bowing of semiconductor substrates have been primarily limited to axisymmetric or multi-axis symmetric techniques. However, a few techniques exist for addressing asymmetric bowing, such as saddle-shaped bowing. The complexity of current techniques results in more complex wafer bow shapes, such as saddle-shaped bowing.
[0034] Among the few techniques used to address asymmetric curvature, one such technique may involve a precursor zoned mask provided adjacent to the backside of the curved semiconductor substrate. For example, a carrier ring supporting the curved semiconductor substrate may be designed with a carrier ring mask for shielding certain areas of the curved semiconductor substrate during deposition. Another technique may involve a multi-plenum showerhead to control the delivery of gases to different locations. For example, a precursor material for depositing a compressive film may be delivered via a first zone of the showerhead base and a precursor material for depositing a tensile film may be delivered via a second zone of the showerhead base.
[0035] Figure 2A schematic top view of an exemplary system for alleviating wafer bending using a partition mask adjacent to a semiconductor substrate is shown. A semiconductor substrate 203 may be provided in a processing chamber. The semiconductor substrate 203 may be supported in the processing chamber by a substrate holder 201. A partition mask 205 is positioned between the semiconductor substrate 203 and a gas distributor (e.g., a showerhead pedestal) (not shown). The partition mask 205 may shield or block certain areas of the semiconductor substrate 203 during deposition. For illustrative purposes, the partition mask 205 is depicted as transparent to show the semiconductor substrate 203 below the partition mask 205. Only the upper right and lower left quadrants of the semiconductor substrate 203 are exposed to the deposited material. In some implementations, the partition mask 205 may be a circular, planar material block divided into four quadrants. The upper right and lower left quadrants of the partition mask 205 are exposed, while the upper left and lower right quadrants of the partition mask 205 are not exposed.
[0036] Figure 3 A schematic top view of an exemplary system for mitigating wafer bow using a multi-plenum showerhead is shown. The showerhead 300 can be divided into four zones or regions 301, 302, 303, 304, each of which can deliver different or the same gases for forming different or the same materials. Figure 3 , regions 301 and 303 are "opposing regions" and regions 302 and 304 are "opposing regions". For deposition of a bend compensation layer on an asymmetrically curved semiconductor substrate, the gas delivered to a first set of opposing regions (e.g., regions 301 and 303) may be the same, and the gas delivered to a second set of opposing regions (e.g., regions 302 and 304) may be the same. However, the delivered gas between the first and second sets may be different. For illustration, a gas for depositing a compressive silicon oxide film may be delivered via a first set of opposing regions, and a gas for depositing a tensile silicon nitride film may be delivered via a second set of opposing regions.
[0037] By using Figure 2 The partition mask shown in FIG. 1 delivers precursor material to certain areas or regions of the curved semiconductor substrate to achieve local stress modulation. Figure 3 The use of multiple plenum chambers to control the precursor partitioning of gas delivery to different locations as shown in achieves local stress regulation. However, due to high IPD coverage and problems associated with clamping semiconductor substrates, such techniques have been limited or ineffective. The problems of high coverage error and vacuum clamping may be the result of the sharp transition of film stress between regions and the difficulty in designing regional layouts that minimize local topological changes.
[0038] The present disclosure provides a method and apparatus for alleviating asymmetric bending in a curved semiconductor substrate by selective UV exposure. Rather than depositing a compression film and a stretch film separately in different regions of a curved semiconductor substrate, a single compression film or stretch film is deposited on the front or back side of the curved semiconductor substrate. The compression or stretch film is a stress-adjustable film that adjusts stress from UV exposure. The UV chamber is equipped with a UV light source, a substrate support for supporting a curved semiconductor substrate, and a window positioned between the substrate support and the UV light source. The window is patterned to have a UV transparent area and a UV opaque area to allow selective exposure of certain areas of the stress-adjustable film to experience stress changes. In some implementations, the window is patterned to have a metal coating or a ceramic cover. In some implementations, the window is further patterned to have a transition zone that allows partial transmission of UV light so that the corresponding area of the stress-adjustable film experiences partial stress changes.
[0039] As used herein, a substrate support is configured to hold, maintain, or otherwise support a substrate in a processing chamber. During various processing steps performed in the processing chamber, the substrate is placed or provided on the substrate support. As such, a substrate such as a semiconductor wafer is placed on a substrate support in a UV chamber while the substrate is being processed (e.g., UV exposure). In some implementations, the substrate support is a pedestal (e.g., a ceramic pedestal), an electrostatic chuck, a mechanical chuck, a plate, or other form of substrate support.
[0040] As used herein, a window is a piece of material between a substrate support and a UV light source, or a piece of material separating a UV light chamber from a substrate processing chamber, wherein the piece of material is transmissive or at least partially transmissive to UV radiation. Generally, the window is made of a glass material such as quartz glass. In some implementations, the glass material is quartz glass, borosilicate glass, or phosphate glass.
[0041] As used herein, UV radiation or UV light can broadly include radiation from 150 nm to the infrared region (about 1 to 10 μm). In some implementations, the UV radiation or UV light is between about 150 nm to about 800 nm. The UV radiation or UV light can be emitted from a UV source within a range or at a single wavelength.
[0042] Figure 4A A schematic diagram of an exemplary apparatus for UV treatment is shown, the apparatus comprising a window positioned between a UV source and a semiconductor substrate. Figure 4B Display pair Figure 4A4. The apparatus 400 includes a processing chamber 410 for processing or processing a substrate 412, and a UV light chamber 420 for accommodating a UV light source 422. The apparatus 400 includes a substrate holder 414 for supporting the substrate 412 in the processing chamber 410. The apparatus 400 may include one or more heating elements 416 for controlling the temperature of the substrate 412. In some implementations, the substrate holder 414 may be a pedestal equipped with one or more heating elements 416 for controlling the temperature of the substrate 412. In some implementations, the substrate 412 may be in full contact with the pedestal or the substrate 412 may be supported above the pedestal by an attachment (e.g., a pin). In some implementations, the substrate holder 414 may clamp or hold the substrate 412 so that the back side or front side of the substrate 412 faces the UV light source 422. The substrate 412 may be a curved semiconductor substrate, wherein the curved semiconductor substrate may have a stress-adjustable film (not shown) deposited on the back side or front side of the curved semiconductor substrate. The UV light source 422 may be configured to emit UV light to cure the stress tunable film such that the stress tunable film undergoes a stress change.
[0043] The UV light source 422 may be any suitable illumination source that emits UV radiation. The UV light source 422 may include a lamp, a light emitting diode (LED), a bulb, a laser, or a combination thereof. In some cases, the UV light source 422 may emit UV light across a broadband wavelength from 170 nm to 400 nm, or may emit UV light across a narrower band of wavelengths from 185 nm to 255 nm. For example, the UV light source 422 may be a broadband UV light source. The UV light source 422 and / or the UV light chamber 420 may be equipped with aperture and beam shaping optics such as lenses or reflectors. For example, the UV light chamber 420 may include a cold mirror for reflecting UV radiation. The UV light source 422 and / or the UV light chamber 420 may be equipped with filters, reflectors, gratings, prisms, or other wavelength selection optics. For example, when the UV light source 422 generates a broadband UV light source with a broad spectrum of radiation, optical components such as reflectors, filters, or a combination of reflectors and filters may be used to adjust the portion of the broad spectrum that reaches the substrate 412.
[0044] The apparatus 400 also includes a window 430 positioned between the UV light source 422 and the substrate holder 414. The window 430 can separate the UV light chamber 420 from the processing chamber 410. The window 430 can be a quartz window that is transparent or at least substantially transparent to UV radiation. By varying the levels of metal impurities and water content in the quartz window, the window 430 can be manufactured to block radiation of undesirable wavelengths. High purity silica quartz with very few metal impurities is more transparent in the deeper ultraviolet spectrum. As an example, quartz with a thickness of 1 cm will have a transmittance of about 50% at a wavelength of 170 nm, while it drops to only a few percent at 160 nm. Increased impurity levels in quartz will cause reduced transmission of UV at lower wavelengths. Fused quartz has more metal impurities present and limits its UV transmission wavelength to around 200 nm and longer. On the other hand, synthetic silica has a higher purity and will shift down to 170 nm. For infrared radiation, the transmittance through quartz is determined by the water content. More moisture in the quartz means that infrared radiation is more easily absorbed. The moisture content in the quartz can be controlled through the production process. Thus, the spectrum of radiation transmitted through the window 430 can be controlled to cut off or reduce UV transmission at shorter wavelengths and / or reduce infrared transmission at longer wavelengths. Figure 4A and 4B , window 430 is unpatterned so that all or substantially all of the UV light from UV light chamber 420 enters into processing chamber 410 through window 430 .
[0045] The processing chamber 410 may be equipped to control the temperature of the substrate 412. One or more heating elements 416 may face the substrate 412 for substrate temperature control. As used herein, a "heating element" is used to control the temperature of a workpiece or substrate. The heating element may be embedded in the substrate holder 414, positioned adjacent to the substrate 412, positioned in the processing chamber 410, or positioned outside the processing chamber 410 for heating the substrate 412. In some embodiments, the one or more heating elements 416 may be one or more LEDs, wherein the LEDs may be configured in a plurality of independently controllable heating zones. Independently controllable heating zones facilitate temperature control in various regions of the substrate 412. In some embodiments, the one or more heating elements 416 are resistive heaters. The one or more heating elements 416 are configured to control the temperature of the substrate 412, wherein the one or more heating elements 416 may allow the substrate temperature to be controlled in a range between about 5°C and about 675°C, or between about 50°C and about 500°C.
[0046] Figure 5AA schematic diagram of an exemplary apparatus for UV treatment is shown, the apparatus including a patterned window positioned between a UV source and a semiconductor substrate according to some implementations. The apparatus 500 includes a processing chamber 510 for treating or processing a substrate 512, and a UV light chamber 520 for accommodating a UV light source 522. The apparatus 500 includes a substrate holder 514 for supporting the substrate 512 in the processing chamber 510. The apparatus 500 may include one or more heating elements 516 for controlling the temperature of the substrate 512. In some implementations, the substrate holder 514 may clamp or hold the substrate 512 so that the back side or the front side of the substrate 512 faces the UV light source 522. Thus, in some cases the UV light source 522 may be configured to direct UV light to the back side of the substrate 512, or in other cases the UV light source 522 may be configured to direct UV light to the front side of the substrate 512. Figure 4A The one or more heating elements 416, substrate holder 414, substrate 412, process chamber 410, UV light chamber 420, and UV light source 422 are described with reference to the accompanying drawings. Figure 5A 5. Various aspects of one or more heating elements 516, substrate holder 514, substrate 512, process chamber 510, UV light chamber 520, and UV light source 522 are shown.
[0047] The substrate 512 may be a curved semiconductor substrate, wherein the curved semiconductor substrate may have a stress-adjustable film (not shown) deposited on the back side or the front side of the curved semiconductor substrate. A curved semiconductor substrate refers to any semiconductor substrate having a surface that deviates from a flat reference plane. In particular, the curved semiconductor substrate may have a warp exceeding ±300 μm. In certain embodiments, the curved semiconductor substrate may be asymmetrically curved.
[0048] The stress adjustable film can be deposited on the front or back side of the substrate 512 to have a compressive film stress or a tensile film stress. The stress adjustable film is configured to undergo a significant stress change in response to UV exposure, thermal exposure, or a combination of the above. Therefore, the stress adjustable film can be a UV curable film, a thermally curable film, or both. The stress adjustable film may include a dielectric material such as an ultra-low k dielectric material. In some implementations, the stress adjustable film includes a nitride, an oxide, or a doped nitride. Nitrides and oxides can undergo significant stress changes after UV curing. In some examples, the stress adjustable film includes silicon nitride, silicon oxide, silicon oxynitride, or silicon carbonitride. In some embodiments, the thickness of the stress adjustable film is between about 20nm and about 150nm, between about 25nm and about 100nm, or between about 30nm and about 100nm. The thickness of the stress adjustable film is thin enough for complete penetration of UV radiation to occur, and thick enough to induce stress on the curved semiconductor substrate below.
[0049] In some implementations, the stress tunable film may be deposited on the substrate 512 using any suitable deposition technique. In some implementations, the stress tunable film is deposited by a chemical vapor deposition method such as plasma enhanced chemical vapor deposition (PECVD). During PECVD, a silicon-containing precursor such as silane may be exposed to one or more reactive gases in a plasma to form a stress tunable film, wherein the stress tunable film is a silicon-containing film. For example, silane (SiH4) may be flowed into a deposition chamber with ammonia (NH3) and / or nitrogen (N2) to deposit silicon nitride. Films deposited by PECVD typically contain a large amount of hydrogen. The amount of hydrogen in the film may affect the degree of stress in the stress tunable film. In fact, the amount of hydrogen in the film may affect the degree of stress change that occurs after exposure to elevated temperatures or after exposure to UV light. Specifically, nitride films such as silicon nitride films deposited by PECVD may contain Si-H bonds and NH bonds in addition to Si-N bonds. Without being bound by any theory, exposing the silicon nitride film to elevated temperature or UV radiation causes the Si-H bonds to begin to break, allowing hydrogen atoms to be released from the silicon nitride film. As the Si-H bonds break and hydrogen atoms are released from the film, the internal bond structure within the silicon nitride film reorganizes. The silicon atoms and nitrogen atoms rearrange and reorganize in the film. This reorganization and rearrangement in the silicon nitride film may include stress changes resulting in high stress excursions in response to thermal or UV curing.
[0050] The apparatus 500 further includes a window 530 positioned between the UV light source 522 and the substrate holder 514. The window 530 can separate the UV light chamber 520 from the processing chamber 510. The window 530 can be patterned to define one or more UV transparent areas 532 and one or more UV opaque areas 534. Transparency as used herein can be defined as a transmittance of about 70% or more of UV light, such as about 80% or more, or about 90% or more. That is, the amount of UV light passing through a certain thickness of the window 530 in the one or more UV transparent areas 532 is equal to or greater than about 70%. The one or more UV opaque areas 534 prevent or otherwise limit the transmission of UV light through the window 530. In other words, the one or more UV opaque areas 534 hinder the transmission of UV light by reflecting or absorbing UV light, wherein opacity as used herein can be defined as a reflection or absorption of UV light of about 70% or more, such as about 80% or more, or even about 90% or more. This can be accomplished using materials that are opaque or reflective to UV light.
[0051] The window 530 is patterned to have a UV transparent area 532 and a UV opaque area 534 to provide a mask for selective UV exposure of the substrate 512. The UV opaque area 534 shields or otherwise blocks UV light from reaching non-target areas of the substrate 512, while the UV transparent area 532 promotes the transmission of UV light to the target area of the substrate 512. The window 530 can be configured to cover the substrate 512. The transparent and opaque portions of the window 530 can correspond to areas of the substrate without UV exposure and areas of the substrate with UV exposure, respectively. The transparent and opaque portions of the window 530 are positioned, sized, and shaped to cope with local bending areas and stresses in the substrate 512. Thus, the window 530 is patterned according to the target area and non-target area of the substrate 512 for selective UV exposure. In some implementations, the window 530 is sized and shaped to accommodate the size and shape of the substrate 512 to be processed.
[0052] During operation, the UV light source 522 emits UV light and passes through the patterned window 530 to selectively cure one or more regions of the stress-adjustable film of the substrate 512. The stress-adjustable film can be deposited on the substrate 512 to have a tensile stress value (e.g., between about +0.1 MPa and about +2000 MPa) or to have a compressive stress value (e.g., between about -0.1 MPa and about -2000 MPa). By way of example, a nitrogen-doped silicon carbide film can have an as-deposited stress value of about -400 MPa. In another example, a silicon nitride film can have an as-deposited stress value of about +700 MPa. In response to UV exposure, or both UV and heat exposure, the stress-adjustable film can undergo a stress shift of about 20% or more, about 30% or more, about 40% or more, or about 50% or more. In some cases, the stress shift can cause the stress-adjustable film to change from a tensile film to a compressive film, or vice versa. Portions of the stress tunable film that are selectively exposed to UV light experience stress changes while portions of the stress tunable film that are not exposed to UV light avoid stress changes. After the selective UV exposure, the exposed portions become more tensile or more compressive. This enables the stress tunable film to locally adjust stress at different portions of the stress tunable film, thereby relieving bending in a curved semiconductor substrate.
[0053] The window 530 is patterned with a material that is opaque to UV light. In some implementations, the window 530 is patterned with a metal coating 540 that corresponds to one or more UV opaque regions 534. Figure 5B A metal coating 540 is shown according to some implementations. Figure 5A530 . The metal coating 540 shields certain areas of the window 530 so that UV light does not pass through the shielded areas. The metal coating 540 can help reflect UV light in the UV opaque area 534 and increase the transmission efficiency of UV light through the UV transparent area 532. Specifically, by reflecting UV light, the UV light can be reflected by reflectors positioned at various locations of the UV light chamber 520, thereby increasing the intensity of UV light passing through the UV transparent area 532. The metal coating 540 can be positioned directly on the surface of the window 530, on the surface of the window 530 facing the substrate holder 514 or on the surface of the window 530 facing the UV light source 522. In some implementations, the metal coating 540 includes silver, aluminum, or a combination of the above. The metal coating 540 can even be a combination of multiple metal layers. The metal coating 540 can have a thickness sufficient to prevent UV light transmission. In some implementations, the metal coating 540 has a thickness equal to or greater than 100nm, for example, between about 100nm and about 1000nm.
[0054] In some implementations, the window is patterned as a ceramic cover 550 having corresponding one or more UV opaque regions 534 . Figure 5C A ceramic cover 550 is shown according to some implementations. Figure 5A 530 . The ceramic cover 550 is designed to shield the area of the window 530 so that UV light does not pass through the shielded area. The ceramic cover 550 includes a ceramic material that is opaque to UV light. Examples of such ceramic materials include, but are not limited to, aluminum nitride or aluminum oxide. The ceramic cover 550 has an opening 552 corresponding to the UV transparent area 532 and a ceramic material block 554 corresponding to the UV opaque area 534. The design of the ceramic cover 550 can be customizable or configured to be placed in the device 500 so that the ceramic cover 550 is removably inserted above or below the window 530. In some implementations, the ceramic cover 550 is removably positioned on the window 530. The structure and design of the window 530 can be manufactured independently of the ceramic cover 550. The ceramic cover 550 may have a thickness sufficient for processing and sufficient to prevent the transmission of UV light. In some implementations, the ceramic cover 550 may have a thickness equal to or greater than about 0.1 mm, for example, between about 0.1 mm and about 10 mm.
[0055] In some alternative implementations, the window is patterned with a metal cover (not shown) corresponding to one or more UV opaque areas 534. The metal cover uses a metal material such as aluminum, rather than a ceramic material, to shield areas of the window 530 so that UV light does not pass through the shielded areas. The metal material can absorb or reflect UV light from the UV light source 522.
[0056] Fig. 6AA schematic top view of a patterned window having UV transparent areas and UV opaque areas according to some implementations is shown. The patterned window 610 can be any suitable shape for processing semiconductor substrates. In some implementations, the patterned window 610 is a circular block of material. UV light can pass through the patterned window 610 to expose the semiconductor substrate, wherein the patterned window can be made of a suitable material such as quartz. The patterned window 610 can be defined by a plurality of zones or regions 611, 612, 613, 614. The regions 611, 613 are "opposite regions" and are used as UV transparent regions 611, 613, while the regions 612, 614 are "opposite regions" and are used as UV opaque regions 612, 614. The regions 612, 614 can also be referred to as shielding regions or covering regions. In some implementations, the UV opaque regions 612, 614 can use a metal coating, a metal cover, or a ceramic cover to block or reflect UV light. In Fig. 6A In FIG. 6 , regions 611 , 612 , 613 , and 614 are equal in area.
[0057] Figure 6B A schematic top view of a patterned window having a UV transparent area occupying a larger surface area than the UV opaque area according to some implementations is shown. The patterned window 620 can be any suitable shape for processing semiconductor substrates. In some implementations, the patterned window 620 is a circular block of material. UV light can pass through the patterned window 620 to expose the semiconductor substrate, wherein the patterned window can be made of a suitable material such as quartz. The patterned window 620 can be defined by multiple zones or areas 621, 622, 623, 624. Areas 621, 623 are "opposite areas" and are used as UV transparent areas 621, 623, while areas 622, 624 are "opposite areas" and are used as UV opaque areas 622, 624. In some implementations, the UV opaque areas 622, 624 can use a metal coating, a metal cover, or a ceramic cover to block or reflect UV light. In Figure 6B In the embodiment of the present invention, UV transparent areas 621, 623 occupy a larger surface area than UV opaque areas 622, 624. Specifically, the size and shape of UV opaque areas 622, 624 can be designed and configured based on the curved nature or shape of the semiconductor substrate being processed. The geometric patterning of patterned window 620 allows certain areas of the semiconductor substrate to be specifically targeted with UV radiation.
[0058] Selective UV exposure produces UV exposed areas and UV unexposed areas in the stress adjustable film to alleviate asymmetric bending, wherein the stress variation between the UV exposed area and the UV unexposed area may be quite large. When the stress variation is too large and sudden, peaks or ridges may be formed in the processed semiconductor substrate. In some cases, film cracking may even occur. By way of example, the deposited stress adjustable film may have a stress value of +500MPa. After selective UV exposure, the UV unexposed area maintains a stress value of +500MPa and the UV exposed area changes to a stress value of -500MPa. The stress offset of 1000MPa between the tensile and compressive regions of the stress adjustable film may be sudden. However, the warping across the surface of the substrate is usually gradual and smooth, meaning that the change in the local wafer topology occurs in a smooth, gradual manner rather than in a sudden, step-by-step manner. Thus, the stress variation occurring at the interface between the UV exposed area and the UV unexposed area in the stress adjustable film may cause peaks or ridges in the substrate. It is desirable to make the stress change at the interface between the UV exposed and UV unexposed areas of the stress tunable film more gradual and smoother.
[0059] In some implementations, a window (e.g., window 530) may be further patterned to have one or more transition zones for partial or limited transmission of UV light through one or more transition zones of the window. For example, a transition zone may allow a transmittance of about 50% of UV light, while a UV transparent zone may allow a transmittance of more than 90% of UV light and a UV opaque zone may allow a transmittance of less than 5% of UV light. One or more transition zones provide partial or reduced UV exposure of a corresponding transition zone of the stress adjustable film. In this way, a corresponding transition zone of the stress adjustable film undergoes a stress excursion that is less than a stress excursion of a UV exposed zone of the stress adjustable film. A corresponding transition zone of the stress adjustable film provides an interface between a UV exposed zone and a UV unexposed zone of the stress adjustable film so that the stress change between the UV exposed zone and the UV unexposed zone is not like abrupt. This alleviates film cracking and the formation of peaks or ridges in the substrate by causing the stress change to occur more gradually rather than suddenly.
[0060] In certain embodiments, the window may include a plurality of transition zones lining the interface between the UV transparent zone and the UV opaque zone. At least some of the plurality of transition zones may allow for varying amounts of UV light transmission to provide a more gradual stress change in the corresponding zone of the stress adjustable film. For example, a first transition zone may allow for approximately 60% UV light transmittance, and a second transition zone adjacent to the first transition zone may allow for approximately 30% UV light transmittance. The corresponding first transition zone of the stress adjustable film may experience a greater amount of stress excursion than the corresponding second transition zone of the stress adjustable film, and the UV exposed zone of the stress adjustable film experiences the greatest amount of stress excursion.
[0061] Figure 6CA schematic top view of a patterned window having a UV transparent region, a UV opaque region, and a transition region that is semi-transparent to UV radiation according to some implementations is shown. Fig. 6A and 6B , the patterned window 630 can be defined by a plurality of zones or regions 631, 632, 633, 634. The regions 631, 633 are "opposite regions" and serve as UV transparent regions 631, 633, while the regions 632, 634 are "opposite regions" and serve as UV opaque regions 632, 634. The patterned window 630 can be further defined by a transition region 635. The transition region 635 lines the interface between the UV transparent regions 631, 633 and the UV opaque regions 632, 634. In other words, the transition region 635 occupies the region of the patterned window 630 between the UV transparent regions 631, 633 and the UV opaque regions 632, 634. In Figure 6C In the embodiment of the present invention, the transition zone 635 is semi-transparent to UV light. The UV transparent zones 631, 633 are transparent or at least substantially transparent to UV light, and the UV opaque zones 632, 634 are opaque or reflective to UV light.
[0062] In some implementations, a material that is partially transparent to UV light can be used to achieve the translucency of transition zone 635. By way of example, such a translucent material can include quartz.
[0063] In some implementations, the semi-transparency of the transition zone 635 can be achieved using a reduced thickness of metal or opaque ceramic material. Typically, a metal coating having a thickness equal to or greater than about 100 nm is effective for reflecting UV light. The transition zone 635 may include a metal layer having a thickness less than 100 nm to allow partial transmission of UV light. Thus, the transition zone 635 may include a UV opaque material having a reduced thickness relative to the UV opaque zones 632, 634.
[0064] Fig.6D A schematic top view of a patterned window having a UV transparent region, a UV opaque region, and a transition region made of a grid-like mesh according to some implementations is shown. Fig. 6A and 6B , the patterned window 640 can be defined by a plurality of zones or regions 641, 642, 643, 644. The regions 641, 643 are "opposite zones" and are used as UV transparent zones 641, 643, while the regions 642, 644 are "opposite zones" and are used as UV opaque zones 642, 644. The patterned window 640 can be further defined by a transition zone 645. As Figure 6C The transition zone 645 lines the interface between the UV transparent zones 641, 643 and the UV opaque zones 642, 644. Fig.6DIn the embodiment of the present invention, the transition zone 645 partially transmits UV light using a grid-like pattern or mesh. The UV transparent zones 641, 643 are transparent or at least substantially transparent to UV light, and the UV opaque zones 642, 644 are opaque or reflective to UV light.
[0065] In some implementations, the grid-like pattern of the transition zone 645 may include a mixture of UV opaque materials and UV transparent materials. For example, the grid-like pattern may include metal lines or shapes on a quartz material, or may include opaque ceramic lines or shapes on a quartz material. In this way, UV light passing through the grid-like pattern of the transition zone 645 may be partially reflected or absorbed and partially transmitted.
[0066] The stress-adjustable film may be deposited on the front or back side of a semiconductor substrate. Typically, the front side of a semiconductor substrate contains various circuits, transistors, or other device components. To alleviate the curvature in a curved semiconductor substrate, it may be desirable to deposit the stress-adjustable film on the back side of the semiconductor substrate to avoid deposition on the circuits, transistors, and other device components.
[0067] Figure 7 A schematic diagram of an exemplary apparatus for UV backside processing is shown, the apparatus including a patterned window positioned between a UV source and a semiconductor substrate according to some implementations. Figure 7 The device 700 in A can be used with Figure 5A The apparatus 700 is similar to the apparatus 500 such that the processing chamber 710 is shown above the UV light chamber 720. The apparatus 700 includes a processing chamber 710 for processing or processing a substrate 712, and a UV light chamber 720 for accommodating a UV light source 722. The apparatus 700 includes a substrate holder 714 for supporting the substrate 712 in the processing chamber 710. In certain embodiments, the substrate holder 714 can hold the substrate 712 by an edge and the back side of the substrate 712 can face the UV light source 722. In some implementations, the back side of the substrate 712 is not patterned. In some implementations, the back side of the substrate 712 includes a stress-adjustable film. The apparatus 700 may include one or more heating elements 716 for controlling the temperature of the substrate 712. The substrate 712 may be subjected to a stress-adjustable film. Figure 4A and 5A The one or more heating elements 416 / 516, substrate holders 414 / 514, substrates 412 / 512, process chambers 410 / 510, UV light chambers 420 / 520, and UV light sources 422 / 522 are described with reference to the accompanying drawings. Figure 7 Aspects of one or more heating elements 716, substrate holder 714, substrate 712, process chamber 710, UV light chamber 720, and UV light source 722 in A.
[0068] The apparatus 700 also includes a window 730 positioned between the UV light source 722 and the substrate holder 714. The window 730 can separate the UV light chamber 720 from the processing chamber 710. The window 730 can be patterned to define one or more UV transparent regions 732 and one or more UV opaque regions 734. The window 730 is patterned to have the UV transparent regions 732 and the UV opaque regions 734 to provide a mask for selective UV exposure of the back side of the substrate 712. This allows target areas of the stress tunable film deposited on the back side of the substrate 712 to experience stress changes to obtain localized regulated stresses, thereby relieving bending in the substrate 712. In some implementations, the window 730 is patterned using a metal coating, a ceramic cover, or a metal cover. In some implementations, the window 730 is further patterned to have one or more transition regions for partial or reduced transmission of UV light. In Figure 7 , the UV light source 722 is configured to direct UV light to the back side of the substrate 712 , where the stress tunable film is formed on the back side of the substrate 712 .
[0069] Figure 8 A flow chart of an exemplary method of selective UV exposure according to some implementations is shown. The operations of process 800 may be performed in a different order and / or may have different, fewer, or additional operations. Figure 5A , Figure 7 ,or Fig. 9 The operations of process 800 may be performed using an apparatus for UV treatment in a computer program product. In some implementations, the operations of process 800 may be performed at least in part according to software stored in one or more non-transitory computer-readable media.
[0070] At frame 810 of process 800, a semiconductor substrate is provided on a substrate support in a processing chamber, wherein the semiconductor substrate includes a stress-adjustable film. A quartz window is positioned between the processing chamber UV light sources, wherein the quartz window is patterned to have one or more UV transparent areas and one or more UV opaque areas. The semiconductor substrate may be a curved semiconductor substrate. A curved semiconductor substrate may be provided in the processing chamber to at least perform a UV treatment operation. However, it should be understood that in some implementations, the processing chamber may be configured to perform one or both of the UV treatment and deposition operations. The semiconductor substrate may be a silicon wafer, such as a 200-mm wafer, a 300-mm wafer, or a 450-mm wafer, including a wafer having one or more layers of material deposited thereon, such as a dielectric, conductive, or semiconductive material. Some of the one or more layers may be patterned. Non-limiting examples of layers include dielectric layers and conductive layers, such as silicon oxide, silicon nitride, silicon carbide, metal oxides, metal nitrides, metal carbides, and metal layers. In various implementations, the semiconductor substrate is patterned.
[0071] In some implementations, the semiconductor substrate includes a patterned 3D-NAND structure and one or more etched grooves in the substrate. In some implementations, the semiconductor substrate may be asymmetrically curved. The curved semiconductor substrate may have a warp of about +1000 μm. In some implementations, the curved semiconductor substrate has a warp greater than about +300 μm. In some implementations, the curved semiconductor substrate has a warp greater than about +300 μm and less than about +1000 μm. The warp may occur at one or more local areas of the curved semiconductor substrate. The warp may have different values between the x-axis warp and the y-axis warp. Thus, the warp along one axis may be more significant than the other axis.
[0072] The stress-adjustable film may be deposited on the front or back side of the semiconductor substrate. In some implementations, the stress-adjustable film is deposited on the back side of the semiconductor substrate. In this way, the stress-adjustable film is prevented from being deposited on circuits, transistors, or other device components on the front side of the semiconductor substrate. The stress-adjustable film may be used as a bend compensation layer for alleviating bends in the semiconductor substrate.
[0073] The stress-adjustable film can be one or both of a UV-curable film and a heat-curable film. Once the stress-adjustable film is exposed to one or both of UV exposure and heat exposure, it can experience stress changes. In some implementations, once the stress-adjustable film is exposed to UV light and / or elevated temperature, it will undergo a stress shift equal to or greater than about 20%, equal to or greater than about 30%, equal to or greater than about 40%, or equal to or greater than about 50%. In some implementations, the stress-adjustable film is a UV-curable film and is subjected to a stress value variation greater than about 200MPa, for example, between about 200MPa and about 4000MPa. This means that the deposited stress value of the stress-adjustable film can vary by 200MPa or more relative to the post-curing stress value of the stress-adjustable film. In some cases, the stress-adjustable film can be changed from tension to compression, or from compression to tension.
[0074] In some implementations, the stress-adjustable film includes a dielectric material such as an ultra-low-k dielectric material. In some implementations, the stress-adjustable film includes a nitride, a doped nitride, or an oxide. In some examples, the stress-adjustable film includes silicon nitride. In some examples, the stress-adjustable film includes silicon carbonitride.
[0075] The quartz window between the substrate and the UV light source can be pre-patterned so that UV light can selectively pass through the quartz window. By having the quartz window pre-patterned, this avoids having to introduce a separate component or mask between the substrate and the light source. The preparation of a separate component or mask may require additional steps of manufacturing, patterning, and insertion into the gap between the substrate and the light source. These additional steps may be time-consuming, cumbersome, and expensive. The quartz window is already a component of a UV treatment chamber or device. In some implementations, the quartz window is patterned to have a metal coating such as a silver or aluminum coating. The metal coating may correspond to the UV opaque area of the quartz window. The metal coating may have a thickness equal to or greater than about 100nm, for example, between about 100nm and about 1000nm. In some implementations, the quartz window is patterned to have a ceramic cover such as an aluminum nitride or aluminum oxide cover. The ceramic cover may correspond to the UV opaque area of the quartz window. The ceramic cover may have a thickness equal to or greater than about 1mm, for example, between about 1mm and about 100mm. In some implementations, the quartz window is patterned with a metal cover such as an aluminum cover. The metal cover may correspond to the UV opaque region of the quartz window. The quartz window may be patterned to allow UV light transmission in the UV transparent region and to block or reflect UV light in the UV opaque region. In some implementations, the quartz window may be patterned based on a measurement of local stress on the semiconductor substrate. The measurement of local stress on the semiconductor substrate may be generated from the stress map.
[0076] At block 820 of process 800, one or more first regions of the stress tunable film are selectively exposed to UV light via one or more UV transparent regions of the quartz window, and UV light is selectively blocked for one or more second regions of the stress tunable film by one or more UV opaque regions of the quartz window. The one or more first regions correspond to the UV transparent regions, and the one or more second regions correspond to the UV opaque regions. The selective exposure of the one or more first regions to UV light locally adjusts stress of the stress tunable film. After locally adjusting stress in various regions of the stress tunable film, the stress tunable film helps to alleviate bowing in the semiconductor substrate.
[0077] The patterned quartz window selectively blocks UV exposure so that only certain areas of the semiconductor substrate are exposed to UV radiation. In this way, one or more first areas represent UV exposure areas where stress changes are performed, and one or more second areas represent UV non-exposed areas where stress changes are not performed. Compared to one or more second areas, one or more first areas of the stress adjustable film can become more tensile or more compressive in stress. Stress in the stress adjustable film after selective UV exposure can be directed to one or more areas of the semiconductor substrate to relieve the bending in the semiconductor substrate. The local stress in the stress adjustable film after selective UV exposure can be adjusted to achieve a local warping topology.
[0078] Without being limited by any theory, the stress change may evolve from the removal of hydrogen in the stress-adjustable film during UV exposure. This can be observed in PECVD silicon nitride films. The loss of hydrogen and / or the shrinkage of pores may lead to a reduction in volume in the stress-adjustable film. However, the constraints of the semiconductor substrate prevent any lateral shrinkage, thereby applying tensile strain in the exposed areas of the stress-adjustable film. In some implementations, selectively exposing one or more first regions of the stress-adjustable film causes such regions to become more tensile in stress compared to unexposed regions of the stress-adjustable film.
[0079] In some implementations, stress changes may occur in one or more first regions of the stress adjustable film when exposed to elevated temperatures. Without being limited by any theory, elevated temperatures may cause the removal of hydrogen in the stress adjustable film, which may result in a reduction in volume in the stress adjustable film. In some implementations, the elevated temperature may be between about 200°C and about 800°C or between about 300°C and about 700°C. One or more heating elements in a processing chamber or substrate support may control the substrate temperature. One or more heating elements may control the temperature independently in partitions or regions so that certain regions of the stress adjustable film may have elevated temperatures. Using one or more heating elements, stress changes may be introduced in a targeted manner in one or more first regions and / or one or more second regions of the stress adjustable film. In some cases, a combination of selective UV exposure and targeted temperature control may be used to locally adjust stress in the stress adjustable film.
[0080] The degree of local stress regulation in one or more first zones depends on the processing conditions during UV exposure and / or thermal exposure. In some implementations, the degree of local stress regulation in one or more first zones depends on the time of UV exposure, substrate temperature, intensity of UV radiation, and / or wavelength of UV radiation. However, it will be appreciated by those skilled in the art that other conditions during UV exposure and / or thermal exposure can be controlled to affect the degree of local stress regulation. Nevertheless, by adjusting one or more of the following: (1) the time of UV exposure, (2) the substrate temperature during UV exposure, (3) the intensity of UV exposure, or (4) the wavelength of UV exposure, the amount of stress change induced in the exposed zone relative to the unexposed zone will change. For example, longer UV exposure times result in higher stress values, higher substrate temperatures result in higher stress values, and higher UV intensities result in higher stress values. It should be understood that longer UV exposure times, higher substrate temperatures, and higher intensities may reach specific limits in controlling stress values. The aforementioned UV exposure conditions can be finely adjusted to achieve a specific level of local stress regulation in one or more first zones. The UV light source may be configured to control the time (ie, dose) of UV exposure, the intensity of UV exposure, and the wavelength of UV exposure.The substrate support (ie, susceptor) may be configured to control substrate temperature.
[0081] In some implementations, the time of UV exposure is between about 0.5 minutes and about 120 minutes, between about 1 minute and about 60 minutes, or between about 2 minutes and about 30 minutes. The time or period of UV exposure is sufficient to observe the desired stress changes. In some implementations, the temperature during UV exposure is between about 100°C and about 700°C, between about 150°C and about 550°C, or between about 200°C and about 500°C. The temperature range may be limited by thermal budget constraints, meaning that the substrate temperature during UV treatment is affected by the devices and films on the semiconductor substrate. For example, the use of a nickel silicide (NiSi) layer constrains the substrate temperature to less than 400°C, while the use of a nickel platinum silicide (NiPtSi) layer constrains the substrate temperature to less than 480°C. In some implementations, the intensity of UV exposure is between about 1 μW / cm 2 About 10W / cm 2 Between, about 10μW / cm 2 About 5W / cm 2 Between or about 50μW / cm 2 About 1W / cm 2 The intensity of the UV radiation can provide sufficient energy to break certain bonds (eg, Si-H and NH bonds) in the stress tunable film.
[0082] In some implementations, one or more first regions of the stress tunable film may experience a stress change of about 20% or more, about 30% or more, about 40% or more, or about 50% or more. One or more first regions of the stress tunable film may become more compressive or more tensile than one or more second regions of the stress tunable film. It should be understood that the degree of stress modulation in one or more first regions may depend on the conditions of the UV and thermal treatment. Processing conditions such as exposure time, substrate temperature, UV light intensity, and UV light wavelength may be controlled to vary local stress modulation.
[0083] For example, a silicon carbonitride film may be deposited on a semiconductor substrate by PECVD. The silicon carbonitride film may have a deposited compressive stress value of about 400 MPa (-400 MPa). As shown in Table 1 below, the first region of the silicon carbonitride film after selective UV exposure undergoes a stress change to become tensile, so that the first region has a tensile stress value of about 400 MPa (+400 MPa). The second region of the silicon carbonitride film is still at a compressive stress value of about 400 MPa (-400 MPa). In another example, a silicon nitride film may be deposited on a semiconductor substrate by PECVD. The silicon nitride film may have a deposited tensile stress value of about 700 MPa (+700 MPa). As shown in Table 1 below, the first region of the silicon nitride film after selective UV exposure undergoes a stress change to become more tensile, so that the first region has a tensile stress value of about 1600 MPa (+1600 MPa). Table 1
[0084] In some implementations, the quartz window is further patterned to have one or more transition zones between one or more UV transparent areas and one or more UV opaque areas. One or more transition zones may be semi-transparent to UV light. Although UV light may selectively pass through one or more UV transparent areas, UV light may partially pass through one or more transition zones. For example, one or more transition zones may have a transmittance of UV light between about 10% and about 90%, between about 20% and about 80%, or between about 25% and about 75%. By reducing the transmission of UV light in one or more transition zones that can be lining the interface between the UV transparent area and the UV opaque area, the corresponding area of the stress adjustable film that is exposed to the reduced transmission of UV light will experience a reduced amount of stress change. This prevents a sudden change in stress between one or more first areas and one or more second areas of the stress adjustable film.
[0085] In some implementations, one or more transition zones may include a semi-transparent material. In some implementations where the UV opaque zone includes a metal coating, one or more transition zones may include a metal layer having a relatively small thickness. For example, one or more transition zones may include a metal layer having a thickness of less than about 100 nm. In some implementations, one or more transition zones include a grid-like pattern or mesh of UV transparent and UV opaque materials.
[0086] The disclosed embodiments may be performed in any suitable apparatus or tool. The apparatus or tool may include one or more processing stations. Described below are exemplary processing stations and tools that may be used in certain embodiments.
[0087] Fig. 9A schematic diagram of an exemplary device for UV curing of a stress-adjustable film according to some implementations is shown. Device 901 is suitable for use involving broadband UV sources. Device 901 includes a plurality of curing stations 903 and 905 in which substrates 913 and 915 are each accommodated. Substrates 913 and 915 are located above bases 923 and 925. There is a gap 904 between the substrate and the base. The substrate can be supported above the base by accessories such as pins or floating on a gas. Parabolic or flat cold mirrors 953 and 955 are located above broadband UV source groups 933 and 935. UV light from lamp groups 933 and 935 passes through windows 943 and 945. 943 and 945 can be patterned to have a metal coating, a ceramic cover, a metal cover, or other components to provide selective UV exposure to certain areas of substrates 913 and 915. In an alternative embodiment, substrates 913 and 915 can be supported by bases 923 and 925, respectively. In such an embodiment, the lamp may or may not be equipped with a cold mirror. By having the substrate in full contact with the susceptor, the substrate temperature may be maintained through the use of a conductive gas, such as helium or a mixture of helium and argon, at a sufficient pressure to conduct heat transfer, typically between about 20 and about 760 Torr, or between about 100 and about 600 Torr.
[0088] In operation, a substrate enters a chamber at station 903 where a first UV curing operation is performed. A window 943 is provided between the substrate 913 and the UV source group 933, wherein the window 943 is pre-patterned. The susceptor temperature at station 903 is set to a first temperature, for example, between about 200° C. and about 500° C., and has a UV lamp above station 903 set to a first intensity, for example, 100% maximum intensity, and a first wavelength of about 200 to 800 nm. In some implementations, after curing for a sufficient time in station 903, the substrate 913 may be transferred to station 905 for further curing or removed from the device 901. A second window 945 may be provided between the substrate 915 and the UV source group 935. The susceptor temperature at station 905 is set to a second temperature, which may be the same or different from the first station, and the UV intensity is set to a second intensity, for example, 90% intensity. Additional stations may be used for additional UV curing under different conditions.
[0089] In order to irradiate the substrate at different wavelengths or wavelength ranges when using a broadband UV source (which produces radiation in a broad spectrum), optical components can be used in the radiation source to adjust the portion of the broad spectrum that reaches the substrate. For example, a reflector, a filter, or a combination of both can be used to subtract a portion of the spectrum from the radiation. Upon reaching the filter, the light can be reflected, absorbed into the filter material, or transmitted through.
[0090] A high pass filter is an interference filter that provides a sharp cutoff below a specific wavelength. It can be used to isolate a specific region of the spectrum. A high pass filter is used to pass or transmit a certain range of wavelengths and block or reflect other wavelengths on the shorter wavelength side of the passband. Long wavelength radiation is transmitted, while short wavelength radiation is reflected. The region of high transmittance is called the passband, and the region of high reflectivity is called the stopband or reflection band. A roll-off region separates the passband from the reflection band. The complexity of the long pass filter depends mainly on the steepness of the transition region and also on the ripple specification in the passband. In the case of relatively high angles of incidence, polarization-dependent losses may occur. Long pass filters are composed of a hard, durable surface material covered with a dielectric coating. They are designed to withstand routine cleaning and handling.
[0091] Another type of filter is a UV cut-off filter. These filters do not allow UV penetration below a set value of, for example, 280 nm. These filters work by absorbing wavelengths below the cut-off value. This may help optimize the desired curing effect.
[0092] Another filter that can be used to select a wavelength range is a bandpass filter. An optical bandpass filter is designed to transmit a specific wavelength band. It is composed of many thin layers of dielectric materials with different refractive indices to produce constructive and destructive interference in the transmitted light. In this way, an optical bandpass filter can be designed to transmit only a specific wavelength band. The range limit usually depends on the composition of the interference filter lens and the thin film filter material. The incident light passes through two coated reflective surfaces. The distance between the reflective coatings determines which wavelengths will produce destructive interference and which wavelengths will be allowed to pass through the coated surfaces. In the case where the reflected beams are in phase, the light will pass through the two reflective surfaces. However, if the wavelengths are out of phase, destructive interference will block most of the reflection and almost no transmission. In this way, the interference filter is able to attenuate the intensity of the transmitted light at wavelengths above or below the desired range.
[0093] In addition to changing the wavelength by changing the radiation reaching the substrate, the wavelength of the radiation can also be controlled by changing the properties of the light generator. Broadband UV sources can produce a wide spectrum of radiation from UV to infrared, but other light generators can also be used to emit a smaller spectrum or increase the intensity of a narrower spectrum. Other light generators can be mercury vapor lamps, doped mercury vapor lamps, electrode lamps, excimer lamps, excimer lasers, pulsed xenon lamps, doped xenon lamps. Lasers (such as excimer lasers) can emit radiation of a single wavelength. When dopants are added to mercury vapor and xenon lamps, narrow band radiation can become more intense. Common dopants are iron, nickel, cobalt, tin, zinc, indium, gallium, thallium, antimony, bismuth, or combinations of these. For example, a mercury vapor lamp doped with indium emits strongly in the visible spectrum and around 450nm; iron, emits strongly at 360nm; and gallium, emits strongly at 320nm. The wavelength of radiation can also be controlled by changing the fill pressure of the lamp. For example, high pressure mercury vapor lamps may be used to more strongly emit wavelengths of 250 nm to 440 nm, especially 310 nm to 350 nm. Low pressure mercury vapor lamps emit shorter wavelengths.
[0094] In addition to changing the properties of the light generator and using filters, reflectors that preferentially transmit one or more segments of the lamp's spectral output may also be used. A commonly used reflector is a cold mirror, which allows infrared radiation to pass but reflects other light. Other reflectors that preferentially reflect spectral bands of light may be used. Thus, the substrate may be exposed to radiation of different wavelengths at different stations. Of course, the radiation wavelength may be the same in some stations.
[0095] exist Fig. 9 In the embodiment of the present invention, pedestals 923 and 925 are fixed. An indexer 911 lifts and moves each substrate from one pedestal to another between each exposure period. The indexer 911 includes an indexing plate 921 attached to a motion mechanism 931 having rotational and axial motion. An upward axial motion is provided to the indexing plate 921 to pick up a substrate from each pedestal. The rotational motion is used to advance the substrate from one station to another. The motion mechanism then provides a downward axial motion to the plate to place the substrate down onto the station.
[0096] The pedestals 923 and 925 are electrically heated and maintained at the desired processing temperature. The pedestals 923 and 925 may also be configured with cooling lines to achieve accurate substrate temperature control. In alternative embodiments, a large heating block may be used to support the substrate to replace each pedestal. A heat conducting gas (e.g., helium) is used to achieve good thermal coupling between the pedestal and the substrate. In some embodiments, a casting pedestal with a coaxial heat exchanger may be used.
[0097] Fig. 9Only examples of suitable devices are shown, and other devices designed for other methods involved in previous and / or subsequent processing can be used. For example, in another embodiment using a broadband UV source, the substrate support is a carousel. Unlike a fixed base substrate support, the substrate does not move relative to the carousel. After the substrate is loaded onto the carousel, if necessary, the carousel rotates to expose the substrate to light from the UV lamp group. The carousel is stationary during exposure. After the exposure period, the carousel rotates to advance each substrate to be exposed to the next group of lamps. The heating and cooling elements can be embedded in the rotating carousel. Alternatively, the carousel can contact or hold the substrate with a hot plate so that it is suspended above the hot plate.
[0098] In certain embodiments, the substrate is exposed to UV radiation from a focused rather than flooded lamp. Fig. 9 In a broadband source embodiment (shown in FIG. 1 ), when scanning the substrate, there is relative movement between the substrate and the light source during exposure to the focused light. In other embodiments, the substrate can be rotated relative to the light source to average out intensity differences across the substrate.
[0099] Fig.10 A schematic diagram of an exemplary processing tool for performing operations for local stress adjustment according to some implementations is shown. In FIG. 5 , a multi-station processing tool 1000 may include an inbound load lock 1002 and an outbound load lock 1004, either or both of which may include a plasma source and / or a UV source. A robot 1006 at atmospheric pressure is configured to remove a wafer from a box loaded into the inbound load lock 1002 via an atmospheric port (not shown) through a pod 1008. A wafer or substrate is placed on a pedestal 1012 in the inbound load lock 1002 by the robot 1006, the atmospheric port is closed, and the load lock is evacuated. In the case where the inbound load lock 1002 includes a remote plasma source, the wafer may be exposed to a remote plasma treatment in the load lock before being introduced into a processing chamber such as a processing chamber 1014a. In the case where the inbound load lock 1002 includes a UV source, the wafer may be exposed to a UV treatment in the load lock before being introduced into a processing chamber such as a processing chamber 1014a. In addition, the wafer may also be heated in the inbound load lock 1002 to, for example, remove moisture and adsorbed gases. Next, the chamber transfer port 1016 leading to the processing chamber 1014a is opened, and another robot 1026 places the wafer into the reactor on the pedestal 1018 of the first station (labeled 1) of the processing chamber 1014a and is shown to be processed in the reactor. Although the embodiment depicted in FIG. 5 includes a load lock, it will be appreciated that in certain embodiments, the wafer may be allowed to enter the processing station directly.
[0100] Each of the depicted processing chambers, such as processing chamber 1014a, includes four processing stations. Each station has a heated base and a gas pipeline inlet. It should be understood that in certain embodiments, each processing station may have different or multiple purposes. For example, a processing station may be used to deposit a tensile or compressive material as part of a bending compensation layer by a suitable deposition technique such as PECVD. Another processing station may be used to process tensile or compressive materials by selective UV curing. In certain embodiments, deposition and UV treatment may occur in the same processing station. Although the depicted processing chamber 1014a includes four stations, it should be understood that the processing chamber according to certain disclosed embodiments may have any suitable number of stations. For example, in certain embodiments, the processing chamber may have four or more stations, while in other embodiments, the processing chamber may have three or fewer stations. In addition, although the depicted processing tool 1000 has three processing chambers 1014a, 1014b and 1014c, it should be understood that the processing tool according to certain disclosed embodiments may have any suitable number of processing chambers.
[0101] Fig.10 One embodiment of a wafer handling system 1090 for transferring wafers within the processing chamber 1014a is depicted. In some embodiments, the wafer handling system 1090 can transfer wafers between various processing stations and / or between a processing station and a loading chamber. It should be understood that any suitable wafer handling system can be used. Non-limiting examples include a wafer turntable and a robot for handling wafers. Fig.10 Also depicted is one embodiment of a system controller 1050 for controlling processing conditions and hardware states of the processing tool 1000. The system controller 1050 may include one or more memory devices 1056, one or more mass storage devices 1054, and one or more processors 1052. The processor 1052 may include a computer or CPU, analog and / or digital input / output connections, a stepper motor controller board, etc.
[0102] In some embodiments, the system controller 1050 controls all activities of the processing tool 1000. The system controller 1050 executes system control software 1058 stored in the mass storage device 1054, loaded into the memory device 1056, and executed by the processor 1052. Alternatively, the control logic can be hard-coded in the controller 1050. Application specific integrated circuits, programmable logic devices (e.g., field programmable gate arrays, or FPGAs), etc. can be used for these purposes. In the following discussion, whether "software" or "code" is used, functionally equivalent hard-coded logic can be used instead. The system control software 1058 may include instructions for controlling the transfer of wafers into and out of the processing chamber, rotating the wafer within the processing chamber, aligning the wafer with the showerhead or quartz window in the processing chamber, the transfer of wafers into and out of the processing chamber, the timing of gases coming out of specific areas of the showerhead, the mixing of gases, the amount of gas coming out of specific areas of the showerhead, the pressure of the chamber and / or station, the back gas flow pressure coming out of specific areas of the showerhead, the chamber and / or reactor temperature, the wafer temperature, the bias power, the target power level, the RF power level and type (e.g., single frequency or dual frequency or high frequency or low frequency), the pedestal, chuck and / or susceptor position, the UV wavelength, the UV dose, the UV intensity, and other parameters of the specific process performed by the processing tool 1000. The system control software 1058 may be configured in any suitable manner. For example, various processing tool component subroutines or control objects may be written to control the operation of the processing tool components used to perform various processing tool processes. The system control software 1058 may be encoded in any suitable computer readable programming language.
[0103] In some embodiments, the system control software 1058 may include input / output control (IOC) sequencing instructions for controlling the various parameters described above. Other computer software and / or programs associated with the system controller 1050 and stored in the mass storage device 1054 and / or the memory device 1056 may be employed in some embodiments. Examples of programs or program segments for this purpose include substrate positioning programs, process gas control programs, pressure control programs, heater control programs, electrostatic chuck power control programs, UV light control programs, and plasma control programs.
[0104] The substrate positioning program may include program code for a processing tool component that is used to load a substrate onto the pedestal 1018 and control the spacing between the substrate and other parts of the processing tool 1000. The UV light control program may include code for controlling UV light conditions (e.g., time, intensity, and wavelength as described herein). The pressure control program may include code for controlling the pressure in the processing station by adjusting, for example, a throttle valve in the exhaust system of the processing station, the gas flow into the processing station, the gas pressure introduced to the back side of the wafer during the adjustment operation, and the like.
[0105] The heater control program may include code for controlling the current to a heating unit that is used to heat the substrate for temperature control operations as described herein. Alternatively, the heater control program may control the delivery of a heat transfer gas (such as helium) toward the substrate. The plasma control program may include code for setting the RF power level applied to the processing electrodes in one or more processing stations according to embodiments herein. The pressure control program may include code for maintaining the pressure within the reaction chamber according to embodiments herein.
[0106] In some embodiments, there may be a user interface associated with the system controller 750. The user interface may include a display screen, a graphical software display of apparatus and / or process conditions, and user input devices such as a pointing device, keyboard, touch screen, microphone, and the like.
[0107] In some embodiments, the parameters adjusted by the system controller 1050 may relate to process conditions. Non-limiting examples include process gas composition and flow rate, temperature, pressure, plasma conditions (e.g., RF bias power level), UV dose, UV intensity, UV wavelength, etc. These parameters may be provided to the user in the form of a recipe, which may be entered using the user interface.
[0108] Signals for monitoring the process may be provided from various process tool sensors by analog and / or digital input connections of the system controller 1050. Signals for controlling the process may be output through analog and digital output connections of the process tool 1000. Non-limiting examples of process tool sensors that may be monitored include mass flow controllers, pressure sensors (e.g., manometers), thermocouples, etc. Appropriately programmed feedback and control algorithms may be used with the data from these sensors to maintain process conditions.
[0109] The system controller 1050 may provide program instructions for implementing the above-described deposition process. The program instructions may control various process parameters, such as UV dose, UV intensity, UV wavelength, pressure, temperature, etc. The instructions may control the parameters to operate the UV treatment of the stress tunable film according to various embodiments described herein.
[0110] The system controller 1050 will typically include one or more memory devices and one or more processors configured to execute instructions so that the apparatus will perform the methods described in accordance with the disclosed embodiments. A machine-readable medium containing instructions for controlling processing operations in accordance with the disclosed embodiments may be coupled to the system controller 1050.
[0111] In some implementations, the system controller 1050 is part of a system, which can be part of the above examples. Such a system can include a semiconductor processing device, which includes one or more processing tools, one or more processing chambers, one or more platforms for processing, and / or specific processing components (wafer pedestals, gas flow systems, etc.). These systems can be integrated with electronic devices for controlling their operation before, during, and after processing semiconductor wafers or substrates. The electronic device can be referred to as a "controller", which can control various elements or subcomponents of one or more systems. Depending on the processing requirements and / or the type of system, the system controller 1050 can be programmed to control any process disclosed herein, including controlling process gas and / or inhibitor gas delivery, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings, RF matching circuit settings, frequency settings, flow rate settings, fluid delivery settings, position and operation settings, wafer transfer in and out of tools and other transfer tools and / or loading chambers connected to or connected to a specific system through an interface.
[0112] In a broad sense, the system controller 1050 can be defined as an electronic device with various integrated circuits, logic, memory and / or software that receives instructions, issues instructions, controls operations, enables cleaning operations, enables endpoint measurements, etc. The integrated circuit can include a chip in the form of firmware that stores program instructions, a digital signal processor (DSP), a chip defined as an application specific integrated circuit (ASIC), and / or one or more microprocessors or microcontrollers that perform program instructions (e.g., software). The program instructions can be instructions transmitted to the system controller 750 in the form of various separate settings (or program files) that define operating parameters for performing specific processing on or for a semiconductor wafer or system. In some embodiments, the operating parameters can be part of a recipe defined by a process engineer for completing one or more processing steps during the preparation of one or more layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits, and / or dies of a wafer.
[0113] In some implementations, the system controller 1050 may be part of or coupled to a computer that is integrated with, coupled to, or connected to the system via a network, or a combination thereof. For example, the system controller 1050 may be in the "cloud" or all or part of a wafer fab host system, thereby allowing remote access to wafer processing. The computer may enable remote access to the system to monitor the current progress of a manufacturing operation, examine the history of past manufacturing operations, examine trends or performance criteria for multiple manufacturing operations, to change parameters of a current process, set processing steps to follow a current process, or start a new process. In some examples, a remote computer (e.g., a server) may provide a process recipe to the system via a network, which may include a local network or the Internet. The remote computer may include a user interface that allows input or programming of parameters and / or settings, which are then transmitted from the remote computer to the system. In some examples, the system controller 750 receives instructions in the form of data that specify parameters for each processing step to be performed during one or more operations. It should be understood that the parameters may be specific to the type of process to be performed and the type of tool to which the system controller 750 is configured to connect or control the tool type. Thus, as described above, the system controller 750 can be distributed, for example, by including one or more discrete controllers that are networked together and work toward a common goal (e.g., the processes and controls described herein). An example of a distributed controller for these purposes can be one or more integrated circuits on the chamber that communicate with one or more remote integrated circuits (e.g., at a platform level or as part of a remote computer) that are combined to control the processes within the chamber.
[0114] In the foregoing description, numerous specific details are set forth to provide a thorough understanding of the embodiments presented. The disclosed embodiments may be practiced without some or all of these specific details. In other instances, well-known processing operations are not described in detail to avoid unnecessarily obscuring the disclosed embodiments. Although the disclosed embodiments are described in conjunction with specific embodiments, it should be understood that they are not intended to limit the disclosed embodiments.
[0115] Although the above embodiments have been described in some detail for the purpose of clarity of understanding, it is apparent that certain variations and modifications may be implemented within the scope of the appended claims. It should be noted that there are many alternative ways of implementing the processes, systems and devices of the embodiments of the present invention. Therefore, the embodiments of the present invention should be considered illustrative rather than restrictive, and the embodiments are not limited to the details given herein.
Claims
1. A device for selective UV exposure, comprising: Ultraviolet (UV) light source; A processing chamber comprising: A substrate support configured to support a semiconductor substrate, wherein the semiconductor substrate comprises a stress-adjustable film ; as well as one or more heating elements configured to control the temperature of the semiconductor substrate; as well as A window is positioned between the substrate support and the UV light source, wherein the window is patterned to have one or more UV transparent regions for selectively exposing one or more first regions of the stress tunable film to UV light and one or more UV opaque regions for selectively blocking UV light for one or more second regions of the stress tunable film. 2 . The device of claim 1 , wherein the window is patterned with a metal coating corresponding to the one or more UV opaque regions.
3. The device of claim 2, wherein the metal coating comprises silver, aluminum, or a combination thereof. 4 . The device of claim 1 , wherein the window is patterned to have a ceramic cover disposed on the window and corresponding to the one or more UV opaque regions. The device of claim 4 , wherein the ceramic cover comprises aluminum nitride or aluminum oxide.
6. The device of any one of claims 1 to 5, wherein the window is patterned to have a metal cover disposed on the window and corresponding to the one or more UV opaque regions.
7. A device according to any one of claims 1 to 5, wherein the window is further patterned to have one or more transition zones lining an interface between the one or more UV transparent zones and the one or more UV opaque zones, wherein the one or more transition zones are translucent to UV light or contain a grid pattern of UV transparent and UV opaque materials.
8. The device of claim 7, wherein the one or more transition regions comprise a metal layer having a thickness less than about 100 nm.
9. The device of claim 7, wherein the one or more transition regions are configured to provide a more gradual stress change at an interface between the one or more first regions of the stress tunable film and the one or more second regions of the stress tunable film.
10. The device of any one of claims 1 to 5, wherein the one or more UV transparent regions are configured to induce a stress shift in the one or more first regions of the stress tunable film in an amount equal to or greater than about 50%.
11. The apparatus according to any one of claims 1 to 5, wherein the UV light source is configured to direct UV light to a back side of the semiconductor substrate, wherein the stress tunable film is formed on the back side of the semiconductor substrate.
12. The apparatus of any one of claims 1 to 5, wherein the UV light source is configured to direct UV light to a front side of the semiconductor substrate, wherein the stress tunable film is formed on the front side of the semiconductor substrate.
13. The device according to any one of claims 1 to 5, further comprising: A controller configured with instructions for performing the following operations: providing the semiconductor substrate in the processing chamber; and The one or more first regions of the stress tunable film are selectively exposed to UV light using the patterned window to locally tune stress on the stress tunable film.
14. The device of any one of claims 1 to 5, wherein the stress tunable film comprises silicon nitride, silicon oxide, silicon oxynitride, or silicon carbonitride, and wherein the window comprises quartz.
15. A method of selective UV exposure, comprising: providing a semiconductor substrate on a substrate support in a process chamber, wherein the semiconductor substrate comprises a stress tunable film, wherein a quartz window is positioned between the process chamber and an ultraviolet (UV) light source, wherein the quartz window is patterned to have one or more UV transparent regions and one or more UV opaque regions; and One or more first regions of the stress tunable film are selectively exposed to UV light via the one or more UV transparent regions of the quartz window, and UV light is selectively blocked for one or more second regions of the stress tunable film by the one or more UV opaque regions of the quartz window. 16 . The method of claim 15 , wherein selectively exposing the one or more first regions of the stress tunable film comprises locally tuning stress in the one or more first regions of the stress tunable film.
17. The method of claim 15, wherein the quartz window is patterned with a metal coating corresponding to the one or more UV opaque regions.
18. The method of any one of claims 15 to 17, wherein the quartz window is patterned to have a ceramic cover or a metal cover disposed on the quartz window and corresponding to the one or more UV opaque regions.
19. The method of any one of claims 15 to 17, wherein the quartz window is further patterned to have one or more transition zones between the one or more UV transparent zones and the one or more UV opaque zones, wherein the one or more transition zones are semi-transparent to UV light.
20. The method of claim 19, wherein the one or more transition regions comprise a metal layer having a thickness less than about 100 nm.