Nonaqueous electrolyte and lithium secondary battery comprising same

By adjusting the degree of ethylene carbonate ionization in the non-aqueous electrolyte and using a non-solvent, the problem of CO2 gas generation in lithium secondary batteries under high voltage was solved, thereby reducing the amount of gas generated and maintaining battery life.

CN118891765APending Publication Date: 2024-11-01LG ENERGY SOLUTION LTD

Patent Information

Application Number
CN202380028353.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-30
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

When existing lithium secondary batteries operate at high voltage, ethylene carbonate decomposes to produce CO2 gas, leading to battery safety issues. Furthermore, traditional methods may affect battery life characteristics when reducing gas generation.

Method used

By adjusting the degree of free ethylene carbonate in the non-aqueous electrolyte to below 30%, and combining this with the use of non-solvents such as fluorobenzene and appropriate lithium salt concentrations, the proportion of free ethylene carbonate can be reduced, thus preventing the decomposition of ethylene carbonate.

Benefits of technology

It effectively reduces CO2 gas generation while maintaining or improving lithium-ion conductivity and battery life characteristics, thus enhancing battery safety and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891765A_ABST
    Figure CN118891765A_ABST
Patent Text Reader

Abstract

The present invention relates to a non-aqueous electrolyte and a lithium secondary battery comprising the same, the non-aqueous electrolyte comprising an organic solvent containing ethylene carbonate, a non-solvent, and a lithium salt, in which the freeness (A) of ethylene carbonate represented by formula (1) is 30% or less. Equation (1): A = {Pfreeness-EC / (Pfreeness-EC + Pcoordination-EC)} * 100 In Equation (1), A is the freeness of ethylene carbonate, Pfreeness-EC is the integral area of a pattern obtained by deconvolution of a Raman spectrum of an electrolyte with a Gaussian function on the basis of a peak at 893 cm <-1 >, and Pfreeness-EC is the integral area of a pattern obtained by deconvolution of a Raman spectrum of an electrolyte with a Gaussian function on the basis of a peak at 893 cm <-1 >. P coordination-EC is an integral area of a graph obtained by deconvolution of a Raman spectrum of the electrolyte by using a Gaussian function based on a peak at 903 cm <-1 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application claims priority to Korean Patent Application No. 10-2022-0039950, filed on March 30, 2022, the disclosure of which is incorporated herein by reference.

[0002] The present invention relates to a non-aqueous electrolyte and a lithium secondary battery including the same, and more particularly to a non-aqueous electrolyte capable of suppressing a change in the cell volume during operation of the lithium secondary battery and a lithium secondary battery including the same. Background Art

[0003] As interest in energy storage technology has grown in recent years and its applications have expanded to power mobile phones, camcorders, laptops and even electric vehicles, research and development of electrochemical devices has gradually crystallized.

[0004] Among these electrochemical devices, interest has been aroused in the development of rechargeable secondary batteries, and in particular, lithium secondary batteries developed in the early 1990s have attracted attention due to advantages of higher operating voltage and significantly higher energy density.

[0005] Lithium secondary batteries are generally prepared by providing a separator between a positive electrode (including a positive electrode active material formed of a lithium-containing transition metal oxide) and a negative electrode (including a negative electrode active material capable of storing lithium ions) to form an electrode assembly, inserting the electrode assembly into a battery case, injecting a non-aqueous electrolyte that serves as a medium for transmitting lithium ions, and then sealing the battery case. The non-aqueous electrolyte is generally composed of a lithium salt and an organic solvent capable of dissolving the lithium salt.

[0006] Carbonate solvents are mainly used as organic solvents for non-aqueous electrolytes, among which ethylene carbonate is a solvent that is continuously used to dissociate lithium salts with high dielectric constants. However, under high voltage and high temperature conditions, ethylene carbonate decomposes due to the reaction of O2 radicals generated at the positive electrode, and generates CO2 gas as a decomposition product. In recent years, with the increasing demand for secondary batteries with high energy density (such as batteries for electric vehicles), secondary batteries operating at high voltages are being developed, wherein, during the operation of these high-voltage lithium secondary batteries, the gas produced by the decomposition of ethylene carbonate may cause serious battery safety problems.

[0007] Therefore, there is a need to develop a non-aqueous electrolyte that can minimize gas generation by suppressing the decomposition of ethylene carbonate, thereby improving the safety of a lithium secondary battery. Summary of the invention

[0008] Technical issues

[0009] One aspect of the present invention provides a nonaqueous electrolyte and a lithium secondary battery including the same, wherein the nonaqueous electrolyte can suppress volume change caused by generation of a small amount of CO2 gas during battery operation by adjusting the degree of freedom of ethylene carbonate in the electrolyte to satisfy a specific range.

[0010] Technical Solution

[0011] According to one embodiment, the present invention provides a non-aqueous electrolyte comprising an organic solvent containing ethylene carbonate, a non-solvent and a lithium salt, wherein the freeness A of ethylene carbonate represented by equation (1) is 30% or less, preferably 10% to 30%, and more preferably 20% to 30%.

[0012] Equation (1): A = {P 游离-EC / (P 游离-EC +P 配位-EC )}×100

[0013] In equation (1), A is the degree of freeness of ethylene carbonate, P 游离-EC Based on 893cm -1 The peak at is deconvoluted using a Gaussian function to obtain the integral area of ​​the graph, P 配位-EC Based on 903cm -1 The peak at is the integrated area of ​​the graph obtained by deconvolving the Raman spectrum of the electrolyte with a Gaussian function.

[0014] In the non-aqueous electrolyte, the ratio of the volume of the non-solvent to the volume of ethylene carbonate may be 1-6, preferably 1-5, more preferably 1-4.

[0015] Specifically, based on the total volume of the non-aqueous electrolyte, the content of ethylene carbonate can be 1 volume % to 10 volume %, preferably 3 volume % to 10 volume %, more preferably 5 volume % to 10 volume %, and based on the total volume of the non-aqueous electrolyte, the content of the non-solvent can be 10 volume % to 40 volume %, preferably 10 volume % to 30 volume %.

[0016] For example, the non-solvent may be at least one selected from the group consisting of fluorobenzene, difluorobenzene, hexafluorobenzene, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (HFE), and bis(2,2,2-trifluoroethyl)ether (BTFE).

[0017] The concentration of the lithium salt contained may be 1.3M to 2M, preferably 1.3M to 1.8M, more preferably 1.3M to 1.7M.

[0018] The organic solvent may further include a linear carbonate solvent, and the linear carbonate solvent may be contained in an amount of 50 to 85 volume %, preferably 50 to 80 volume %, more preferably 60 to 80 volume % based on the total volume of the nonaqueous electrolyte.

[0019] According to another embodiment, the present invention provides a lithium secondary battery including the nonaqueous electrolyte of the present invention.

[0020] Beneficial Effects

[0021] Since the non-aqueous electrolyte of the present invention replaces part of the ethylene carbonate with a non-solvent that does not participate in the dissociation of lithium in the electrolyte, the amount of free ethylene carbonate that does not coordinate with lithium ions and the amount of ethylene carbonate in the electrolyte can be reduced. Specifically, in the non-aqueous electrolyte of the present invention, the freeness A of ethylene carbonate represented by formula (1) is less than 30%. When the freeness A of ethylene carbonate satisfies the above range, the effect of significantly reducing the amount of CO2 gas generated can be obtained.

[0022] If the content of ethylene carbonate in the non-aqueous electrolyte is high, the ethylene carbonate will cause CO2 to be generated when it is oxidized and decomposed at the positive electrode during the charge and discharge process, which will have an adverse effect on the safety of the battery. If the proportion of ethylene carbonate in the organic solvent is reduced, the generation of CO2 due to the decomposition of ethylene carbonate can be reduced, but the amount of gas (such as CH4) generated by the decomposition of linear carbonates (such as ethyl methyl carbonate and dimethyl carbonate) added instead of ethylene carbonate will also increase, so the effect of reducing the amount of gas generation is not obvious.

[0023] If the ethylene carbonate in the non-aqueous electrolyte forms a coordination bond with the lithium ion, the oxidation stability can be increased and the oxidative decomposition of ethylene carbonate can be inhibited, but the ethylene carbonate that is not bound to the lithium ion will be oxidatively decomposed at the positive electrode and generate CO2 gas. In other words, the amount of gas produced by the decomposition of ethylene carbonate is largely affected by the amount of free ethylene carbonate. When the lithium salt concentration increases, the proportion of free ethylene carbonate can be reduced, but since the viscosity of the electrolyte increases and the conductivity decreases with the increase of the lithium salt concentration, there is a problem of reduced life characteristics of lithium secondary batteries.

[0024] Therefore, in the present invention, since a non-solvent that does not participate in the dissociation of lithium in the electrolyte is used in combination without reducing the amount of ethylene carbonate, the amount of free ethylene carbonate that does not coordinate with lithium ions and the amount of ethylene carbonate in the electrolyte can be reduced without increasing the amount of linear carbonate or the concentration of lithium salt, thereby effectively reducing the generation of CO2 gas and minimizing the degradation of life characteristics.

[0025] Generally, since the non-solvent has a lower viscosity characteristic than ethylene carbonate, when the non-solvent is used in combination in the present invention, an effect of lowering the viscosity of the electrolyte can also be obtained.

[0026] If the nonaqueous electrolyte of the present invention is used, electrolyte consumption and gas generation during operation of a lithium secondary battery can be effectively prevented, and thus a lithium secondary battery having excellent life characteristics and safety can be realized. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 3 is a diagram showing the Raman spectrum of the non-aqueous electrolyte of Example 1.

[0028] Figure 2 : is a graph showing the life characteristics of lithium secondary batteries using the non-aqueous electrolytes of Examples 1 to 3 and Comparative Examples 1 to 5. DETAILED DESCRIPTION

[0029] Hereinafter, the present invention will be described in more detail.

[0030] Non-aqueous electrolytes

[0031] The nonaqueous electrolyte of the present invention comprises: (1) an organic solvent containing ethylene carbonate, (2) a non-solvent, and (3) a lithium salt, wherein the degree of freeness A of ethylene carbonate represented by the following equation (1) is 30% or less, preferably 10% to 30%, and more preferably 20% to 30%.

[0032] Equation (1): A = {P 游离-EC / (P 游离-EC +P 配位-EC )}×100

[0033] In equation (1), A is the degree of freeness of ethylene carbonate, P 游离-EC Based on 893cm -1 The peak at is deconvoluted using a Gaussian function to obtain the integral area of ​​the graph, P 配位-EC Based on 903cm -1 The peak at is the integrated area of ​​the graph obtained by deconvolving the Raman spectrum of the electrolyte with a Gaussian function.

[0034] The degree of freeness (A) of ethylene carbonate is a value indicating the ratio of free ethylene carbonate not coordinated with lithium ions to the total ethylene carbonate in the electrolyte. -1 Nearby P 游离-EC The peak is caused by free ethylene carbonate that is not bound to lithium ions and appears at 903 cm -1 Nearby P 配位-ECThe peaks are caused by ethylene carbonate coordinated with lithium ions. The integrated area of ​​each peak corresponds to the content of the component representing the peak. Therefore, P in equation (1) 游离-EC / (P 游离-EC +P 配位-EC ) is a value corresponding to the ratio of free ethylene carbonate to total ethylene carbonate present in the electrolyte.

[0035] If ethylene carbonate forms a coordination bond with lithium ions, the oxidation stability can be increased, the oxidative decomposition of ethylene carbonate can be suppressed, and the ethylene carbonate that is not combined with lithium ions is oxidatively decomposed at the positive electrode and generates CO2 gas. That is, the amount of gas generated by the decomposition of ethylene carbonate is largely affected by the proportion of free ethylene carbonate. According to the research of the inventors, when the ratio of free ethylene carbonate to total ethylene carbonate in the electrolyte is less than 30%, that is, when the freeness A of ethylene carbonate represented by equation (1) is less than 30%, it is found that the amount of CO2 gas generated is significantly reduced, and the effect of minimizing the degradation of life characteristics is minimized. When the freeness A of ethylene carbonate represented by equation (1) is greater than 30%, since the effect of reducing CO2 is reduced, volume changes may occur during battery operation, which may lead to a significant reduction in life characteristics.

[0036] Preferably, the freeness A of ethylene carbonate represented by equation (1) may be in the range of 10% to 30%, more preferably 20% to 30%. The lower the freeness A of ethylene carbonate, the more favorable it is to suppress the decomposition of ethylene carbonate, thereby reducing the amount of gas generated, but when the amount of ethylene carbonate is reduced or the amount of lithium salt is increased to reduce the freeness A, the problem of reduced performance of the battery cell may occur due to insufficient formation of the solid electrolyte interface (SEI) film of the negative electrode, increased electrolyte viscosity and reduced ion conductivity.

[0037] The degree of freeness A of ethylene carbonate represented by equation (1) can be adjusted by adjusting the concentration of the lithium salt and the composition of the solvent in the non-aqueous electrolyte.

[0038] Hereinafter, each component of the nonaqueous electrolyte of the present invention will be described in more detail.

[0039] (1) Organic solvents

[0040] In the present invention, the organic solvent includes ethylene carbonate.

[0041] Due to its high dielectric constant, ethylene carbonate can dissociate lithium salts in the electrolyte well. Therefore, when ethylene carbonate is used as an organic solvent, excellent electrochemical performance can be achieved due to excellent lithium mobility.

[0042] In the present invention, based on the total volume of the non-aqueous electrolyte, the content of ethylene carbonate can be 10% by volume or less, preferably 1% by volume to 10% by volume, more preferably 3% by volume to 10% by volume, and even more preferably 5% by volume to 10% by volume. When the amount of ethylene carbonate meets the above range, it is easy to adjust the A value of equation (1) to less than 30%, so that a non-aqueous electrolyte with high lithium ion conductivity and low gas generation can be prepared. Specifically, if the content of ethylene carbonate is too low, the lithium ion conductivity can be reduced, thereby reducing the electrochemical performance, and if the content of ethylene carbonate is too high, the proportion of free ethylene carbonate may increase, thereby increasing the gas generation.

[0043] In addition to ethylene carbonate, the organic solvent may also include a linear carbonate solvent. A linear carbonate solvent is an organic solvent with low viscosity and low dielectric constant, wherein, for example, the linear carbonate solvent may be at least one selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate and ethyl propyl carbonate.

[0044] Based on the total volume of the non-aqueous electrolyte, the content of the linear carbonate solvent can be 50 volume % to 85 volume %, preferably 50 volume % to 80 volume %, more preferably 60 volume % to 80 volume %. When the amount of the linear carbonate solvent meets the above range, the viscosity of the non-aqueous electrolyte can be properly maintained, and the effect of reducing gas generation is excellent. If the amount of the linear carbonate solvent is too low, the viscosity of the non-aqueous electrolyte may increase, thereby reducing ionic conductivity, and if the amount of the linear carbonate solvent is too high, then due to the generation of excessive gas (e.g., CH4) when the linear carbonate solvent decomposes during battery operation, the effect of suppressing gas generation may be reduced.

[0045] Although not essential, the organic solvent may further contain a cyclic carbonate-based solvent or a linear ester-based solvent other than ethylene carbonate, if desired.

[0046] As a cyclic carbonate solvent other than ethylene carbonate, for example, at least one selected from the group consisting of propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate and vinylene carbonate can be used, and as a linear ester solvent, for example, at least one selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate and butyl propionate can be used.

[0047] (2) Non-solvent

[0048] Non-solvent refers to a solvent that does not participate in the dissociation of lithium salts due to its low solubility to lithium salts. In the present invention, since a non-solvent that does not participate in the dissociation of lithium in the electrolyte is used in combination without reducing the amount of ethylene carbonate, the amount of free ethylene carbonate in the electrolyte can be reduced without increasing the concentration of lithium salts. If the amount of a solvent (e.g., linear carbonate) that forms a coordination bond with lithium ions increases, even if the amount of ethylene carbonate is reduced, the combination between the increased linear carbonate and lithium ions will increase, so it is limited in terms of increasing the ratio of ethylene carbonate coordinated with lithium ions. Therefore, the reduction of the ratio of free ethylene carbonate to total ethylene carbonate is limited. However, since the non-solvent does not bind to lithium ions, it will not affect the degree of dissociation of ethylene carbonate, so when the amount of ethylene carbonate is reduced, the ratio of free ethylene carbonate to total ethylene carbonate can be effectively reduced by adding a non-solvent.

[0049] As a non-solvent, for example, at least one selected from the group consisting of fluorobenzene, difluorobenzene, hexafluorobenzene, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (HFE) and bis (2,2,2-trifluoroethyl) ether (BTFE) can be used, among which fluorobenzene is particularly preferred. As for fluorobenzene, since its viscosity characteristics are lower than ethylene carbonate, when fluorobenzene is used as a non-solvent, the effect of reducing the viscosity of the electrolyte can be obtained, and since no oxidation / reduction reaction occurs at the operating potential of the secondary battery of 2.5V to 4.3V, fluorobenzene has electrochemical stability.

[0050] Based on the total volume of the non-aqueous electrolyte, the content of the non-solvent may be 10% to 40% by volume, preferably 10% to 30% by volume. When the amount of the non-solvent satisfies the above range, CO2 generation is significantly reduced, and the effect of reducing the viscosity of the non-aqueous electrolyte is excellent.

[0051] In the non-aqueous electrolyte of the present invention, the ratio of the volume of the non-solvent to the volume of ethylene carbonate can be 1 to 6, preferably 1 to 5, and more preferably 1 to 4. When the volume ratio of the non-solvent to ethylene carbonate satisfies the above range, the effect of reducing the amount of gas generated and the effect of reducing the viscosity of the non-aqueous electrolyte are excellent. When the volume of the non-solvent contained is less than that of ethylene carbonate, the effect of suppressing the amount of gas generated is not obvious. If the volume of the non-solvent is significantly higher than the volume of ethylene carbonate, the lithium ion conductivity may be reduced, thereby causing the electrochemical characteristics to deteriorate.

[0052] (3) Lithium salt

[0053] Various lithium salts commonly used in the electrolyte of lithium secondary batteries can be used as the lithium salt used in the present invention without limitation. For example, the lithium salt may include Li +as a cation, and may include at least one selected from the group consisting of: F - , Cl - Br - ,I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - 、AlO4 - 、AlCl4 - PF6 - 、SbF6 - 、AsF6 - , B 10 Cl 10 - 、BF2C2O4 - , BC4O8 - PF4C2O4 - PF2C4O8 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - CF3SO3 - 、C4F9SO3 - CF3CF2SO3 - 、(FSO2)2N - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - 、CH3SO3 - CF3(CF2)7SO3 - CF3CO2 - 、CH3CO2 - 、SCN - and (CF3CF2SO2)2N - .

[0054] Specifically, the lithium salt may include at least one selected from the group consisting of LiCl, LiBr, LiI, LiBF4, LiClO4, LiAlO4, LiAlCl4, LiPF6, LiSbF6, LiAsF6, LiB 10 Cl 10, LiBOB (LiB (C2O4) 2), LiCF3SO3, LiFSI (LiN (SO2F) 2), LiCH3SO3, LiCF3CO2, LiCH3CO2 and LiBETI (LiN (SO2CF2CF3) 2). Specifically, the lithium salt may include a single material selected from the group consisting of LiBF4, LiClO4, LiPF6, LiBOB (LiB (C2O4) 2), LiCF3SO3, LiTFSI (LiN (SO2CF3) 2), LiFSI (LiN (SO2F) 2) and LiBETI (LiN (SO2CF2CF3) 2) or a mixture of two or more thereof.

[0055] The lithium salt may be contained in the nonaqueous electrolyte at a concentration of 1.3 M to 2 M, preferably 1.3 M to 1.8 M, and more preferably 1.3 M to 1.7 M. In the case where the concentration of the lithium salt is less than 1.3 M, since the amount of lithium ions that can be coordinated with ethylene carbonate is low, it is difficult to reduce the proportion of free ethylene carbonate to a desired level, and therefore, the reduction in the amount of CO2 generation is limited, and the lithium mobility in the electrolyte may also be reduced, thereby reducing the life characteristics.

[0056] Since the nonaqueous electrolyte of the present invention includes a non-solvent with a low degree of lithium salt dissociation, when the concentration of the lithium salt is greater than 2 M, the lithium salt may not be completely dissociated and the electrolyte viscosity may increase, thereby reducing ionic conductivity.

[0057] (4) Other components

[0058] Although not essential, the nonaqueous electrolyte of the present invention may further include additives in addition to the above-mentioned components to further improve the physical properties of the secondary battery.

[0059] Examples of the additive may be at least one selected from the group consisting of cyclic carbonate compounds, halogenated carbonate compounds, sultone compounds, sulfate compounds, phosphate compounds, borate compounds, amine compounds, silane compounds and lithium salt compounds.

[0060] For example, the cyclic carbonate compound may be vinylene carbonate (VC) or vinyl ethylene carbonate (VEC).

[0061] For example, the halogenated carbonate compound may be fluoroethylene carbonate (FEC).

[0062] For example, the sultone compound may be 1,3-propane sultone or 1,3-propene sultone.

[0063] For example, the sulfate compound may be ethylene sulfate (Esa), trimethylene sulfate (TMS), or methyltrimethylene sulfate (MTMS).

[0064] For example, the phosphate compound may be at least one compound selected from the group consisting of lithium difluorobis(oxalato)phosphate, lithium difluorophosphate, tetramethyltrimethylsilyl phosphate, trimethylsilyl phosphite, tris(2,2,2-trifluoroethyl)phosphate and tris(trifluoroethyl)phosphite.

[0065] For example, the borate compound may be tetraphenylborate or lithium difluorooxalatoborate (LiODFB).

[0066] The amine compound may be triethanolamine or ethylenediamine, and the silane compound may be tetravinylsilane.

[0067] The lithium salt compound is a compound different from the lithium salt contained in the non-aqueous electrolyte, wherein the lithium salt compound can be at least one compound selected from the group consisting of LiPO2F2, LiODFB, LiBOB (lithium bis(oxalato)borate (LiB(C2O4)2)) and LiBF4.

[0068] The above-mentioned additives may be used alone, or two or more thereof may be mixed and used.

[0069] The total amount of the additive may be in the range of 0.1 wt % to 20 wt %, preferably 0.1 wt % to 15 wt %, based on the total weight of the electrolyte. When the content of the additive is within the above range, side reactions or residue or precipitation of the additive during the initial activation of the secondary battery can be prevented, while a film can be stably formed on the electrode, and a fire phenomenon during overcharging can be suppressed.

[0070] Lithium secondary battery

[0071] Next, the lithium secondary battery of the present invention will be described.

[0072] The lithium secondary battery of the present invention comprises the nonaqueous electrolyte of the present invention described above. Specifically, the lithium secondary battery of the present invention comprises a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a nonaqueous electrolyte, in which case the nonaqueous electrolyte is the nonaqueous electrolyte of the present invention described above. Since the nonaqueous electrolyte has been described above, its description will be omitted, and other components will be described below.

[0073] positive electrode

[0074] The positive electrode may include a positive electrode active material layer including a positive electrode active material, and if necessary, the positive electrode active material layer may further include a conductive agent and / or a binder.

[0075] The positive electrode active material is a compound capable of reversibly inserting and extracting lithium. Among them, various positive electrode active materials used in the art can be used. For example, lithium manganese oxides (such as LiMnO2, LiMn2O4, etc.), lithium cobalt oxides (such as LiCoO2, etc.), lithium nickel oxides (such as LiNiO2, etc.), lithium nickel manganese oxides (such as LiNi 1-Y Mn Y O2 (where 0 < Y < 1), LiMn 2-Z Ni Z O4 (where 0 < Z < 2)), lithium nickel cobalt oxides (such as LiNi 1-Y1 Co Y1 O2 (where 0 < Y1 < 1)), lithium manganese cobalt oxides (such as LiCo 1-Y2 Mn Y2 O2 (where 0 < Y2 < 1), LiMn 2-Z1 Co Z1 O4 (where 0 < Z1 < 2)), lithium nickel manganese cobalt oxides (such as Li(Ni p1 Co q1 Mn r1 )O2 (where 0 < p1 < 1, 0 < q1 < 1, 0 < r1 < 1, p1 + q1 + r1 = 1) or Li(Ni p2 Co q2 Mn r2 )O4 (where 0 < p2 < 2, 0 < q2 < 2, 0 < r2 < 2, p2 + q2 + r2 = 2), lithium nickel cobalt transition metal (M) oxides (such as Li(Ni p3 Co q3 Mn r3 M S3 )O2 (where M is selected from the group consisting of aluminum (Al), iron (Fe), vanadium (V), chromium (Cr), titanium (Ti), tantalum (Ta), magnesium (Mg), and molybdenum (Mo), and p3, q3, r3, and S3 are the atomic fractions of each independent element, where 0 < p3 < 1, 0 < q3 < 1, 0 < r3 < 1, 0 < S3 < 1, p2 + q2 + r3 + S2 = 1).

[0076] Preferably, the positive electrode active material may include at least one of a manganese oxide represented by the following [Formula 1] and a lithium nickel oxide represented by [Formula 2].

[0077] [Formula 1]

[0078] Li 1+x [Ni a Co b Mn c M 1d 1-x O 2-y

[0079] In Formula 1, 0.05 ≤ x ≤ 1, 0 ≤ a ≤ 0.5, 0 ≤ b ≤ 0.1, 0.5 ≤ c ≤ 1.0, 0 ≤ d ≤ 0.2, and -1.0 ≤ y ≤ 1.0. M 1 may be at least one metal ion selected from the group consisting of Al, boron (B), cobalt (Co), tungsten (W), Mg, V, Ti, zinc (Zn), gallium (Ga), indium (In), ruthenium (Ru), niobium (Nb), tin (Sn), strontium (Sr), and zirconium (Zr).

[0080] [Formula 2]

[0081] Li 1+x1 [Ni a1 Co b1 Mn c1 M 2 d1 O2

[0082] In Formula 2, -0.2 ≤ x1 ≤ 0.2, 0.8 ≤ a1 < 1, 0 < b1 < 0.2, 0 < c1 < 0.2, and 0 ≤ d1 ≤ 0.2. M 2 may be at least one selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr.

[0083] The secondary battery using the lithium manganese-based oxide represented by [Formula 1] undergoes an activation process at a high voltage of 4.6 V or higher, where there is a problem of excessive CO2 generation due to the oxidative decomposition of ethylene carbonate at the positive electrode during this process. In addition, since the lithium nickel-based oxide represented by Formula 2 contains a large amount of nickel, its structure is unstable, and there is a problem of excessive CO2 generation due to the oxidative decomposition of ethylene carbonate at the positive electrode when operating at high temperature or high voltage. However, since the proportion of free ethylene carbonate that undergoes oxidative decomposition at the positive electrode in the non-aqueous electrolyte of the present invention is as low as 30% or less, when the non-aqueous electrolyte of the present invention is used together with the positive electrode active material of [Formula 1] and / or [Formula 2], CO2 generation can be effectively reduced.

[0084] Based on the total weight of the positive electrode active material layer, the content of the positive electrode active material may be 80% by weight to 99.9% by weight, preferably 85% by weight to 99% by weight.

[0085] ​Next, the conductive agent is used to provide conductivity to the electrode, wherein any conductive agent can be used without particular limitation, as long as it has suitable electronic conductivity and does not cause adverse chemical changes in the battery. Specific examples of the conductive agent can be: graphite, such as natural graphite or artificial graphite; carbon materials, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black and carbon fiber; metal powder or metal fiber, such as copper, nickel, aluminum and silver; conductive whiskers, such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides, such as titanium oxide; or conductive polymers, such as polyphenylene derivatives, any one of which or a mixture of two or more thereof can also be used. Based on the total weight of the positive electrode active material layer, the content of the conductive agent can be 0.1 wt % to 10 wt %, preferably 0.1 wt % to 5 wt %.

[0086] Next, the binder improves the adhesion between the positive active material particles and the adhesion between the positive active material and the current collector. Specific examples of binders can be polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber or its various copolymers, and any one of them or a mixture of two or more thereof can be used. Based on the gross weight of the positive active material layer, the content of the binder can be 0.1 wt % to 15 wt %, preferably 0.1 wt % to 10 wt %.

[0087] The positive electrode of the present invention described above can be prepared by a method for preparing a positive electrode known in the art. For example, the positive electrode can be prepared by the following method: coating the positive electrode collector with a positive electrode slurry prepared by dissolving or dispersing a positive electrode active material, a binder and / or a conductive agent in a solvent, drying and then rolling, or casting the positive electrode slurry on a separate support and then laminating the film separated from the support on the positive electrode collector.

[0088] The positive electrode current collector is not particularly limited as long as it has conductivity without causing adverse chemical changes in the battery, and can use, for example, stainless steel, aluminum, nickel, titanium, fired carbon, or aluminum or stainless steel surface-treated with one of carbon, nickel, titanium, silver, etc. In addition, the thickness of the positive electrode current collector is generally 3 μm to 500 μm, and fine irregularities may be formed on the surface of the current collector to improve the adhesion of the positive electrode material. For example, the positive electrode current collector may be used in various shapes such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.

[0089] The solvent can be a solvent commonly used in the art, and can include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone or water, and any one or a mixture of two or more thereof can be used. If the coating thickness, manufacturing yield and processability of the positive electrode material mixture are considered, and the positive electrode material mixture can be adjusted to have an appropriate viscosity, the amount of the solvent may be sufficient and there is no particular limitation.

[0090] Negative electrode

[0091] Next, the negative electrode will be described.

[0092] The negative electrode of the present invention includes a negative electrode active material layer containing a negative electrode active material, and if necessary, the negative electrode active material layer may further contain a conductive agent and / or a binder.

[0093] As the negative electrode active material, various negative electrode active materials used in the art can be used, such as carbon-based negative electrode active materials, silicon-based negative electrode active materials or metal alloys.

[0094] As the carbon-based negative electrode material, various carbon-based negative electrode active materials used in the art can be used, such as graphite-based materials, such as natural graphite, artificial graphite and Kish graphite; pyrolytic carbon, mesophase pitch-based carbon fibers, mesophase carbon microbeads, mesophase pitch, high-temperature sintered carbon (such as coke derived from petroleum or coal tar pitch), soft carbon and hard carbon. The shape of the carbon-based negative electrode active material is not particularly limited, and materials of various shapes can be used, such as irregular shape, planar shape, sheet shape, spherical shape or fibrous shape.

[0095] The silicon-based negative electrode active material can include at least one selected from the group consisting of: metallic silicon (Si), silicon oxide (SiO x , where 0 < x < 2), silicon carbide (SiC), and Si-Y alloy (where Y is an element selected from the group consisting of: alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements and combinations thereof, but not Si). The element Y can be selected from magnesium, calcium (Ca), Sr, barium (Ba), radium (Ra), scandium (Sc), yttrium (Y), Ti, Zr, hafnium (Hf), (Rf), V, Nb, Ta, (Db), Cr, Mo, W, (Sg), technetium (Tc), rhenium (Re), (Bh), Fe, lead (Pb), Ru, osmium (Os), The group consisting of: sulphur (S), selenium (Se), tellurium (Te), polonium (Po), and combinations thereof.

[0096] The negative electrode active material may be contained in an amount of 80 wt % to 99 wt % based on the total weight of the negative electrode active material layer. When the amount of the negative electrode active material satisfies the above range, excellent capacity characteristics and electrochemical performance may be obtained.

[0097] Next, the conductive agent is a component for further improving the conductivity of the negative electrode active material, wherein the conductive agent can be added in an amount of 10 wt % or less, for example, 5 wt % or less, based on the total weight of the negative electrode active material layer. Any conductive agent can be used without particular limitation, as long as it has conductivity and does not cause adverse chemical changes in the battery, for example, the following conductive materials can be used, for example: graphite, such as natural graphite and artificial graphite; carbon black, such as acetylene black, ketjen black, channel black, furnace black, lamp black and thermal black; conductive fibers, such as carbon fibers or metal fibers; fluorocarbon powder; metal powders, such as aluminum powder and nickel powder; conductive whiskers, such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides, such as titanium oxide; or polyphenylene derivatives.

[0098] The binder is a component that helps to bind the conductive agent, the active material and the current collector, wherein the binder is generally added in an amount of 0.1% to 10% by weight based on the total weight of the negative electrode active material layer. Examples of binders may be polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile rubber, fluororubber and various copolymers thereof.

[0099] The negative electrode can be prepared by a method for preparing a negative electrode known in the art. For example, the negative electrode can be prepared by coating a negative electrode current collector with a negative electrode slurry prepared by dissolving or dispersing a negative electrode active material and an optional binder and / or conductive agent in a solvent, rolling and drying; or casting the negative electrode slurry on a separate support and then laminating a film separated from the support on the negative electrode current collector.

[0100] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing adverse chemical changes in the battery, and can use, for example, copper, stainless steel, aluminum, nickel, titanium, fired carbon, copper or stainless steel surface-treated with one of carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy. In addition, the thickness of the negative electrode current collector can generally be 3 μm to 500 μm, and similar to the positive electrode current collector, fine irregularities can be formed on the surface of the current collector to improve the adhesion of the negative electrode active material. For example, the negative electrode current collector can be used in various shapes such as a film, a sheet, a foil, a mesh, a porous body, a foam body, a non-woven fabric body, etc.

[0101] The solvent may be a commonly used solvent in the art, and may include dimethyl sulfoxide (DMSO), isopropanol, N-methylpyrrolidone (NMP), acetone or water, and any one or a mixture of two or more thereof may be used. If the coating thickness, manufacturing yield and processability of the negative electrode material mixture are taken into consideration, the negative electrode slurry may be adjusted to have an appropriate viscosity, and the amount of solvent may be sufficient, and there is no particular limitation.

[0102] Diaphragm

[0103] Next, the separator will be described.

[0104] The separator is disposed between the negative electrode and the positive electrode to separate the positive electrode and the negative electrode and to provide a path for the movement of lithium ions, wherein any separator can be used as the separator without particular limitation as long as it is commonly used in lithium secondary batteries, and in particular, a separator having high moisture retention capacity for electrolytes and low resistance to the transfer of electrolyte ions can be used.

[0105] Specifically, porous polymer film can be used, for example, porous polymer film prepared by polyolefin polymer (for example ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer and ethylene / methacrylate copolymer) or its two or more layers of laminated structure. In addition, typical porous nonwoven fabrics can be used, for example, nonwoven fabrics formed by high melting point glass fiber or polyethylene terephthalate fiber. In addition, the coated diaphragm including ceramic component or polymer material can be used to ensure heat resistance or mechanical strength, and the diaphragm with single layer or multilayer structure can be optionally used.

[0106] The lithium secondary battery of the present invention described above can be suitably used in portable devices such as mobile phones, notebook computers, digital cameras, and electric vehicles.

[0107] Therefore, according to another embodiment of the present invention, a battery module including the above-mentioned lithium secondary battery as a unit cell and a battery pack including the battery module are provided.

[0108] The battery module or battery pack can be used as a power source for at least one of the following large and medium-sized devices: a power tool; an electric vehicle, including an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0109] The shape of the lithium secondary battery of the present invention is not particularly limited, but a cylindrical type using a can, a prismatic type, a pouch type, or a coin type may be used.

[0110] The lithium secondary battery of the present invention can be used not only as a battery unit used as a power source for small devices but also as a unit cell in a medium or large battery module including a plurality of unit batteries.

[0111] Hereinafter, the present invention will be described in detail according to specific embodiments.

[0112] Example 1

[0113] Ethylene carbonate (EC):ethyl methyl carbonate (EMC):dimethyl carbonate (DMC):fluorobenzene (FB) were mixed in a volume ratio of 10:5:75:10, and LiPF6 was dissolved therein so that the concentration of LiPF6 was 1.4M to prepare a non-aqueous electrolyte.

[0114] Example 2

[0115] Ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC): fluorobenzene (FB) were mixed in a volume ratio of 5:5:75:15, and LiPF6 was dissolved therein so that the concentration of LiPF6 was 1.4M to prepare a non-aqueous electrolyte.

[0116] Example 3

[0117] Ethylene carbonate (EC):ethyl methyl carbonate (EMC):dimethyl carbonate (DMC):fluorobenzene (FB) were mixed in a volume ratio of 10:5:75:10, and LiPF6 was dissolved therein so that the concentration of LiPF6 was 1.6M to prepare a nonaqueous electrolyte.

[0118] Comparative Example 1

[0119] Ethylene carbonate (EC):ethyl methyl carbonate (EMC):dimethyl carbonate (DMC) were mixed in a volume ratio of 20:5:75, and LiPF6 was dissolved therein so that the concentration of LiPF6 was 1.4M to prepare a nonaqueous electrolyte.

[0120] Comparative Example 2

[0121] Ethylene carbonate (EC):ethyl methyl carbonate (EMC):dimethyl carbonate (DMC):fluorobenzene (FB) were mixed in a volume ratio of 15:5:75:5, and LiPF6 was dissolved therein so that the concentration of LiPF6 was 1.4M to prepare a nonaqueous electrolyte.

[0122] Comparative Example 3

[0123] Ethylene carbonate (EC):ethyl methyl carbonate (EMC):dimethyl carbonate (DMC) were mixed in a volume ratio of 10:5:85, and LiPF6 was dissolved therein so that the concentration of LiPF6 was 1.4M to prepare a nonaqueous electrolyte.

[0124] Comparative Example 4

[0125] Ethyl methyl carbonate (EMC):dimethyl carbonate (DMC) was mixed in a volume ratio of 5:95, and LiPF6 was dissolved therein so that the concentration of LiPF6 was 1.4M to prepare a non-aqueous electrolyte.

[0126] Comparative Example 5

[0127] Ethylene carbonate (EC):ethyl methyl carbonate (EMC):dimethyl carbonate (DMC):fluorobenzene (FB) were mixed in a volume ratio of 10:5:75:10, and LiPF6 was dissolved therein so that the concentration of LiPF6 was 1.2M to prepare a nonaqueous electrolyte.

[0128] [Table 1]

[0129]

[0130] Experimental Example 1

[0131] The Raman spectra of the non-aqueous electrolytes prepared in Examples 1 to 3 and Comparative Examples 1 to 5 were measured using a Raman spectrometer (ThermoFisher Scientific, model name: DXR3Xi), and the freeness A of ethylene carbonate was calculated according to equation (1) using the Raman spectra. The measurement results are shown in Table 2 below. In addition, the Raman spectrum of the non-aqueous electrolyte of Example 1 is shown in Table 2. Figure 1 shown.

[0132] Experimental Example 2

[0133] The viscosity (unit: cps) of the nonaqueous electrolytes prepared by Examples 1 to 3 and Comparative Examples 1 to 5 was measured using a viscometer (BrookField, model name: DV-3ULTRA) at 25° C. and 250 rpm, and the viscosity increase rate was calculated based on the viscosity of the nonaqueous electrolyte of Comparative Example 1, as shown in the following Table 2. The viscosity increase rate was calculated by the following equation (2).

[0134] Equation (2): Viscosity increase rate (%) = {(viscosity of measured non-aqueous electrolyte - viscosity of non-aqueous electrolyte of Comparative Example 1) / viscosity of non-aqueous electrolyte of Comparative Example 1} × 100

[0135] <Preparation of lithium secondary battery>

[0136] (Preparation of positive electrode)

[0137] LiNi as the positive electrode active material 0.8 Co 0.1 Mn 0.1 O2, carbon black as a conductive agent, and polyvinylidene fluoride (PVDF) as a binder were added to N-methyl-2-pyrrolidone (NMP) as a solvent at a weight ratio of 98:1:1 to prepare a positive electrode slurry. The positive electrode current collector (aluminum (Al) film) was coated with the positive electrode slurry, dried, and then rolled to prepare a positive electrode.

[0138] (Preparation of negative electrode)

[0139] Graphite as a negative electrode active material, PVDF as a binder, and carbon black as a conductive agent were added to NMP as a solvent in a weight ratio of 96:1:3 to prepare a negative electrode slurry. The negative electrode current collector (copper (Cu) film) was coated with the negative electrode slurry, dried, and then rolled to prepare a negative electrode.

[0140] (Preparation of Secondary Battery)

[0141] The positive electrode and the negative electrode prepared by the above method were stacked in sequence with a polyethylene porous film by a conventional method to prepare an electrode assembly, and then the electrode assembly was housed in a pouch-type secondary battery shell, and the non-aqueous electrolytes prepared in Examples 1 to 3 and Comparative Examples 1 to 5 were respectively injected to prepare a lithium secondary battery.

[0142] Experimental Example 3

[0143] The lithium secondary batteries prepared above were each fully charged, and then stored at 72°C for 30 days, a hole was opened in the battery shell, the generated gas was collected under negative pressure for 1 minute, and then the CO2 generation (unit: μL) and CH4 generation (unit: μL) were measured by chromatography. Then, the gas generation rate based on Comparative Example 1 was calculated by equation (3) and shown in Table 2 below.

[0144] Equation (3): Gas generation amount increase rate (%) = {(measured gas generation amount - gas generation amount of Comparative Example 1) / gas generation amount of Comparative Example 1} × 100

[0145] [Table 2]

[0146]

[0147] Referring to Table 2, it can be confirmed that the nonaqueous electrolytes of Examples 1 to 3 (including a non-solvent and having a degree of freeness A of ethylene carbonate of 30% or less) have a lower CO 2 gas generation amount than the nonaqueous electrolytes of Comparative Examples 1 to 5.

[0148] For the nonaqueous electrolyte of Comparative Example 3 in which no nonsolvent was used and the freeness A of ethylene carbonate was adjusted to 30% or less by increasing the amount of linear carbonate, the CO2 reduction amount was lower than that of the nonaqueous electrolytes of Examples 1 to 3, and the CH4 gas generation amount was significantly increased.

[0149] Experimental Example 4

[0150] Each lithium secondary battery prepared by injecting the non-aqueous electrolyte of Examples 1 to 3 and Comparative Examples 1 to 5 was charged to 4.2V (0.05C cutoff) at 1C under constant current / constant voltage (CC / CV) conditions at 25°C. Subsequently, each lithium secondary battery was discharged to 3V at 1C under CC. The above charging and discharging was set as one cycle, and the capacity retention rate was measured when the cycle was performed 120 times. The measurement results are shown in FIG. Figure 2 shown.

[0151] refer to Figure 2 , it was confirmed that, for the secondary batteries using the nonaqueous electrolytes of Examples 1 to 3, the life characteristics were at the same level, although the amount of gas generation was significantly reduced compared to the secondary batteries using the nonaqueous electrolytes of Comparative Examples 1 to 2. On the contrary, it was found that the secondary batteries using the nonaqueous electrolytes of Comparative Examples 3 to 5 had deteriorated life characteristics compared to the secondary batteries of Examples 1 to 3 and Comparative Examples 1 and 2.

Claims

1. A non-aqueous electrolyte comprising an organic solvent containing ethylene carbonate, a non-solvent and a lithium salt, in, The freeness A of ethylene carbonate represented by equation (1) is 30% or less, Equation (1): A = {P 游离-EC / (P 游离-EC +P 配位-EC )}×100 Wherein, in equation (1), A is the degree of freeness of ethylene carbonate, P 游离-EC Based on 893cm -1 The peak at is deconvoluted using a Gaussian function to obtain the integral area of ​​the graph, P 配位-EC Based on 903cm -1 The peak at is the integrated area of ​​the graph obtained by deconvolving the Raman spectrum of the electrolyte with a Gaussian function.

2. The nonaqueous electrolyte according to claim 1, wherein The freeness A of ethylene carbonate represented by equation (1) is 20% to 30%.

3. The nonaqueous electrolyte according to claim 1, wherein The ratio of the volume of the non-solvent to the volume of ethylene carbonate is 1 to 6.

4. The nonaqueous electrolyte according to claim 1, wherein The ethylene carbonate may be included in an amount of 1 volume % to 10 volume % based on the total volume of the non-aqueous electrolyte.

5. The nonaqueous electrolyte according to claim 1, wherein The non-solvent may be included in an amount of 10 volume % to 40 volume % based on the total volume of the non-aqueous electrolyte.

6. The nonaqueous electrolyte according to claim 1, wherein The non-solvent is at least one selected from the group consisting of fluorobenzene, difluorobenzene, hexafluorobenzene, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (HFE) and bis(2,2,2-trifluoroethyl) ether (BTFE).

7. The nonaqueous electrolyte according to claim 1, wherein The concentration of the lithium salt contained is 1.3M to 2M.

8. The nonaqueous electrolyte according to claim 1, wherein The organic solvent further includes a linear carbonate solvent.

9. The nonaqueous electrolyte according to claim 8, wherein The linear carbonate solvent is included in an amount of 50 volume % to 85 volume % based on the total volume of the non-aqueous electrolyte. 10 . A lithium secondary battery comprising the nonaqueous electrolyte according to claim 1 .

Citation Information

Patent Citations

  • Digital transformation capability evaluation system and its method

    KR1020220039950A