Separator for lithium secondary battery and lithium secondary battery including same
By forming a ceramic heat-resistant layer and an IPN structure adhesive layer on the lithium secondary battery separator, the shortcomings of the separator in terms of thermal stability, structural stability and air permeability are solved, and the stable operation and high efficiency of the battery are achieved.
Patent Information
- Application Number
- CN202380022892.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-11-10
- Filing Date
- 2023-08-30
- Publication Date
- 2024-11-01
AI Technical Summary
Existing lithium secondary battery separators have shortcomings in terms of thermal stability, structural stability, adhesion, and air permeability, which affect the stable operation of the battery.
The design employs a heat-resistant layer and an adhesive layer sequentially formed on the substrate surface. The heat-resistant layer contains ceramic materials, and the adhesive layer contains an adhesive binder with an interpenetrating polymer network structure and organic fillers, which enhances the thermal stability and adhesive strength of the diaphragm while maintaining air permeability.
It improves the thermal stability, structural stability, and adhesive strength of the lithium secondary battery separator, ensuring stable battery operation and maintaining appropriate permeability after hot pressing.
Smart Images

Figure CN118891778A_ABST
Abstract
Description
Technical Field
[0001] Disclosed are a separator for a lithium secondary battery and a lithium secondary battery including the separator. Background Art
[0002] Recently, rechargeable batteries have attracted much attention as energy sources. Among them, lithium secondary batteries with high energy density and discharge voltage have been available on the market and widely used, but efforts have been made to improve the performance of lithium secondary batteries.
[0003] The separator, which is an element constituting the lithium secondary battery, enables the lithium secondary battery to be charged and discharged by continuously maintaining ion conductivity while separating a positive electrode and a negative electrode from each other.
[0004] In order to stably operate a lithium secondary battery, it is important to ensure excellent thermal stability, structural stability, adhesive strength, gas permeability, etc. of the separator. Summary of the invention
[0005] Technical issues
[0006] Provided is a separator for a lithium secondary battery having excellent thermal stability, structural stability, adhesion, gas permeability, etc.
[0007] Technical Solution
[0008] In an embodiment, a separator for a lithium secondary battery includes a heat-resistant layer and an adhesive layer sequentially formed on at least one surface of a substrate, wherein the heat-resistant layer includes ceramic, the adhesive layer includes an adhesive binder and an organic filler, and the adhesive binder includes a polymer having an interpenetrating polymer network (IPN) structure.
[0009] Another embodiment provides a lithium secondary battery including the separator for a lithium secondary battery.
[0010] Beneficial Effects
[0011] The separator for a lithium secondary battery according to the embodiment exhibits excellent thermal stability, structural stability, adhesiveness, gas permeability, etc., and contributes to stable operation of the lithium secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figures 1 to 3 Each of them is a view schematically showing a separator for a lithium secondary battery according to an embodiment.
[0013] Figure 4 is an exploded perspective view of a lithium secondary battery according to an embodiment. DETAILED DESCRIPTION
[0014] Hereinafter, specific embodiments will be described in detail so that those skilled in the art can easily implement the specific embodiments. However, the present disclosure may be implemented in many different forms and is not to be construed as limited to the example embodiments set forth herein.
[0015] The terms used herein are only used to describe the embodiments and are not intended to limit the present invention. Unless the context clearly indicates otherwise, a singular expression includes a plural expression.
[0016] "Combinations thereof" refers to mixtures, stacks, composites, copolymers, alloys, blends, reactants, and the like of the components.
[0017] It should be understood that terms such as “includes,” “comprising,” or “having” are intended to indicate the presence of the presented features, quantities, steps, elements, or combinations thereof, but do not exclude the possibility of the presence or addition of one or more other features, quantities, steps, elements, or combinations thereof.
[0018] In the drawings, the thickness of layers, films, panels, regions, etc., is exaggerated for clarity, and the same reference numerals represent the same elements throughout the specification. It will be understood that when an element such as a layer, film, region, or substrate is referred to as being "on" another element, the element may be directly on the other element, or there may be intervening elements. Conversely, when an element is referred to as being "directly on" another element, there are no intervening elements.
[0019] The "layer" here includes not only a shape formed on the entire surface when viewed from a plan view but also a shape formed on a part of the surface.
[0020] "Particle size" or "average particle size" can be measured by methods known to those skilled in the art, for example, by a particle size analyzer, or by transmission electron micrographs or scanning electron micrographs. Alternatively, the average particle size value can be obtained by measuring using a dynamic light scattering method, performing data analysis, counting the number of particles in each size range, and calculating therefrom. Unless otherwise defined, the average particle size can mean the diameter of particles having a cumulative volume of 50% by volume in a particle size distribution (D50).
[0021] The "thickness" can be measured by a thickness measuring device or a photograph taken with an optical microscope (such as a scanning electron microscope).
[0022] (Separator for lithium secondary battery)
[0023] In an embodiment, a separator for a lithium secondary battery includes a heat-resistant layer and an adhesive layer sequentially formed on at least one surface of a substrate, wherein the heat-resistant layer includes ceramic, the adhesive layer includes an adhesive binder and an organic filler, and the adhesive binder includes a polymer having an interpenetrating polymer network (IPN) structure.
[0024] The separator for a lithium secondary battery according to the embodiment may simultaneously exhibit excellent adhesive strength and air permeability through the adhesive layer while ensuring thermal stability and structural stability through the heat-resistant layer.
[0025] For example, the heat-resistant layer includes ceramics, and ceramics correspond to a material having excellent heat resistance and durability. Therefore, the separator for a lithium secondary battery according to an embodiment can ensure thermal stability and structural stability through the heat-resistant layer.
[0026] In addition, the adhesive layer includes an adhesive binder and an organic filler. Specifically, the adhesive binder includes a polymer with an interpenetrating polymer network (IPN) structure, wherein the polymer of the interpenetrating polymer network structure means that two types of polymers are entangled in a network form, and at least one polymer has a network structure. Therefore, compared with the adhesive binder of a non-IPN structure such as a linear polymer, the polymer with an interpenetrating polymer network structure can enhance bonding strength by a hot pressing process. In addition, the organic filler is a material with a high melting temperature (Tm), and even after the hot pressing process, the shape of the particles is maintained, thereby helping to ensure the air permeability after the hot pressing of the diaphragm. Therefore, the diaphragm for the lithium secondary battery according to the embodiment can simultaneously show excellent bonding strength and air permeability by an adhesive layer.
[0027] Hereinafter, a separator for a lithium secondary battery according to an embodiment will be described in detail.
[0028] Adhesive adhesive
[0029] The adhesive binder may be an adhesive binder in which a cross-linked acrylate polymer and a cross-linked vinylidene fluoride polymer form an interpenetrating polymer network. The two cross-linked polymers forming the interpenetrating polymer network may impart excellent adhesive strength to the separator for a lithium secondary battery according to an embodiment.
[0030] For example, the cross-linked acrylate polymer and the cross-linked vinylidene fluoride polymer each have a network structure, and they may be entangled in the form of a network.
[0031] The cross-linked acrylate polymer may be a cross-linked polymer selected from polymethacrylate, polyethyl acrylate, polyacrylate, polybutyl acrylate, and the like.
[0032] The cross-linked vinylidene fluoride polymer may be a cross-linked polymer selected from a homopolymer including only a structural unit derived from a vinylidene fluoride monomer and a copolymer of a structural unit derived from vinylidene fluoride and a structural unit derived from other monomers.
[0033] The copolymer may include at least one of structural units derived from trifluorochloroethylene, trifluoroethylene, hexafluoropropylene, tetrafluoroethylene and ethylene monomers and structural units derived from vinylidene fluoride, but is not limited thereto. For example, the copolymer may be a polyvinylidene fluoride-hexafluoropropylene (PVdF-HFP) copolymer including structural units derived from vinylidene fluoride monomers and structural units derived from hexafluoropropylene monomers.
[0034] The weight ratio of the cross-linked acrylate polymer to the cross-linked vinylidene fluoride polymer in the adhesive binder may be 8:2 to 1:9. Within the above range, excellent adhesive strength may be maintained even after the separator for a lithium secondary battery according to an embodiment is heat-pressed.
[0035] For example, when the content of the cross-linked acrylate polymer is relatively increased within the above range, the internal resistance of the battery may increase, and when the content of the cross-linked acrylate polymer is relatively reduced, the adhesive function of the adhesive binder including the material may deteriorate. Considering this balance relationship, the weight ratio of the cross-linked acrylate polymer to the cross-linked vinylidene fluoride polymer may be adjusted.
[0036] For example, the weight ratio of the cross-linked acrylate polymer to the cross-linked vinylidene fluoride polymer in the adhesive binder may be 8:2 to 1:9, 7:3 to 2:8, or 6:4 to 2:8, or 5:5 to 3:7.
[0037] The adhesive binder may have a weight average molecular weight greater than or equal to 100,000 g / mol. Within the above range, excellent adhesive strength may be maintained even after the separator for a lithium secondary battery according to an embodiment is heat-pressed.
[0038] For example, when the weight average molecular weight of the adhesive binder decreases within the above range, the adhesive binder may be electrochemically unstable. In view of this relationship, the weight average molecular weight of the adhesive binder may be adjusted. For example, the weight average molecular weight of the adhesive binder may be greater than or equal to 100,000 g / mol, greater than or equal to 200,000 g / mol, or greater than or equal to 300,000 g / mol.
[0039] Even if the weight average molecular weight of the adhesive binder increases, physical properties are not deteriorated, so the upper limit is not limited thereto, but the weight average molecular weight may be less than or equal to 1,500,000 g / mol, which is the upper limit of the weight average molecular weight of commercially available adhesive binders.
[0040] Here, the weight average molecular weight may be an average molecular weight of polystyrene measured using gel permeation chromatography.
[0041] Organic fillers
[0042] The organic filler may be a particle type filler including a vinylidene fluoride-based polymer.
[0043] The organic filler is a material having a high melting point (Tm) of 100° C. to 200° C. and can maintain the shape of particles even after a hot pressing process, thereby helping to ensure the air permeability of the separator after hot pressing.
[0044] For example, the melting point of the organic filler may be greater than or equal to 100°C, greater than or equal to 120°C, or greater than or equal to 130°C and less than or equal to 200°C, less than or equal to 180°C, or less than or equal to 170°C.
[0045] The organic filler is a particle type filler and can be arranged in the network structure of the polymer having the interpenetrating polymer network structure to enhance air permeability. In addition, the organic filler as a vinylidene fluoride-based polymer can exhibit excellent adhesive strength.
[0046] The organic filler may have a D50 particle size of 50 nm to 1,000 nm. For example, within the above range, the separator for a lithium secondary battery according to an embodiment may be imparted with excellent air permeability.
[0047] In the above range, when the D50 particle size of the organic filler increases, the thickness of the adhesive layer increases and the adhesive function may be deteriorated instead. In consideration of this balance relationship, the D50 particle size of the organic filler may be adjusted.
[0048] For example, the organic filler may have a D50 particle size of 50 nm or more, 100 nm or more, 150 nm or more, or 200 nm or more and 1,000 nm or less, 800 nm or less, 600 nm or less, 400 nm or less, or 300 nm or less.
[0049] The organic filler may have a weight average molecular weight of greater than or equal to 100,000 g / mol. Within the above range, the separator for a lithium secondary battery according to an embodiment may be imparted with excellent air permeability.
[0050] For example, when the weight average molecular weight of the organic filler decreases within the above range, the organic filler may be electrochemically unstable. Taking this relationship into consideration, the weight average molecular weight of the organic filler may be adjusted. For example, the weight average molecular weight of the organic filler may be greater than or equal to 100,000 g / mol, greater than or equal to 200,000 g / mol, or greater than or equal to 300,000 g / mol.
[0051] Even if the weight average molecular weight of the organic filler increases, physical properties are not deteriorated, and the upper limit is not limited thereto but may be 1,500,000 g / mol or less, which is the upper limit of the weight average molecular weight of organic fillers available on the market.
[0052] Adhesive layer
[0053] The weight ratio of the adhesive binder to the organic filler in the adhesive layer may be 5:95 to 85:15. Within this range, there is a synergistic effect in enhancing air permeability by the organic filler while exhibiting excellent adhesive strength due to the adhesive binder.
[0054] For example, when the content of the adhesive binder is relatively high within the above range, the air permeability of the separator may increase, thereby increasing the internal resistance of the battery, and when the content of the adhesive binder is reduced, the adhesive ability of the adhesive layer may decrease. Considering this balance relationship, the weight ratio of the adhesive binder and the organic filler can be adjusted.
[0055] For example, the weight ratio of the adhesive binder to the organic filler in the adhesive layer may be 5:95 to 85:15, 15:85 to 85:15, 20:80 to 80:20 (1:4 to 4:1).
[0056] The loading amount of the adhesive layer relative to one surface of the substrate may be 0.1 g / m 2 Up to 1.0g / m 2 Within this range, thermal stability, structural stability, and the like may be improved while exhibiting excellent adhesive strength.
[0057] For example, when the loading amount of the adhesive layer increases within the above range, the air permeability of the separator may increase, and thus the internal resistance of the battery may increase, and when the loading amount of the adhesive layer decreases, the adhesive ability of the adhesive layer may decrease. Considering this balance relationship, the loading amount of the adhesive layer may be adjusted.
[0058] For example, the loading amount of the adhesive layer relative to one surface of the substrate is greater than or equal to 0.1 g / m 2 , greater than or equal to 0.2g / m 2 , or greater than or equal to 0.3g / m 2 And less than or equal to 1.0g / m2 , less than or equal to 8.0g / m 2 , or less than or equal to 7.0g / m 2 .
[0059] ceramics
[0060] The ceramic can be selected from boehmite, Al2O3, B2O3, Ga2O3, TiO2, SnO2, CeO2, MgO, NiO, CaO, GaO, ZnO, ZrO2, Y2O3, SrTiO3, BaTiO3, Mg(OH)2 and combinations thereof.
[0061] The ceramic can have a D50 particle size of 1nm to 2000nm (e.g., 100nm to 1000nm or 100nm to 700nm). In addition, two or more types of ceramics with different particle sizes can also be mixed and used. If the D50 particle size of the ceramic is within the above range, when a heat-resistant layer is formed, the ceramic can be uniformly coated on the substrate, the short circuit between the positive electrode and the negative electrode can be suppressed, and the resistance of the lithium ion can also be minimized to ensure the performance of the lithium secondary battery.
[0062] Heat resistant layer
[0063] In order to achieve bonding between the ceramic particles and between the ceramic particles and the substrate, the heat-resistant layer may also include at least one binder for the heat-resistant layer, wherein the binder for the heat-resistant layer is selected from polyvinylidene fluoride (PVdF), styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), polyvinylidene fluoride-hexafluoropropylene (PVdF-HFP) copolymer, ethylene vinyl acetate (EVA), hydroxyethyl cellulose (HEC), polyvinyl alcohol (PVA), polyvinyl butyral (PVB), ethylene-acrylic acid copolymer, acrylonitrile, vinyl acetate derivatives, polyethylene glycol and acrylic rubber.
[0064] For example, the acrylic rubber may be a copolymer including a repeating unit derived from acrylamide and a repeating unit derived from 2-acrylamido-2-methylpropanesulfonic acid, but is not limited thereto.
[0065] The weight ratio of ceramic to binder in the heat-resistant layer may be 50: 1 to 10: 1. Within the above range, the effects of heat resistance and durability of ceramics may be fully exhibited while ensuring bonding strength between ceramic particles and between ceramic particles and the substrate.
[0066] For example, when the content of the binder is relatively high within the above range, the air permeability of the separator may increase, thereby increasing the internal resistance of the battery. When the content of the binder decreases, not only the heat resistance of the heat-resistant layer decreases, but the heat-resistant layer may also detach. Considering this balance relationship, the weight ratio of the ceramic to the binder in the heat-resistant layer can be adjusted.
[0067] The heat-resistant layer may have a thickness of 0.5 μm to 20 μm (e.g., 1 μm to 10 μm or 1 μm to 5 μm). If the thickness of the heat-resistant layer is within the above range, heat resistance is improved, thereby suppressing internal short circuits of the battery, ensuring a stable separator, and suppressing an increase in the internal resistance of the battery.
[0068] Base
[0069] The substrate may include polyolefin, polyester, polytetrafluoroethylene (PTFE), polyacetal, polyamide, polyimide, polycarbonate, polyetheretherketone, polyaryletherketone, polyetherimide, polyamideimide, polybenzimidazole, polyethersulfone, polyphenylene ether, cyclic olefin copolymer, polyphenylene sulfide, polyethylene naphthalate, glass fiber, or a combination thereof, but is not limited thereto.
[0070] Examples of polyolefins include polyethylene and polypropylene, and examples of polyesters include polyethylene terephthalate and polybutylene terephthalate.
[0071] In addition, the substrate can be a nonwoven fabric or a porous substrate in the form of a textile, and can have a single film or a multilayer structure. For example, the substrate can include a polyethylene single film, a polypropylene single film, a polyethylene / polypropylene double film, a polypropylene / polyethylene / polypropylene three film, a polyethylene / polypropylene / polyethylene three film, etc.
[0072] The substrate may have a thickness of 1 μm to 40 μm (e.g., 1 μm to 30 μm, 1 μm to 20 μm, 5 μm to 15 μm, or 5 μm to 10 μm). If the thickness of the substrate is within the above range, a short circuit between the positive electrode and the negative electrode may be prevented without increasing the internal resistance of the battery.
[0073] Diaphragm structure
[0074] As described above, the separator of the embodiment includes: a substrate; and a heat-resistant layer and an adhesive layer sequentially formed on “at least one surface” of the substrate.
[0075] For example, Figure 1 As shown in , the separator of the embodiment may include: a substrate 10 ; and a heat-resistant layer 20 and an adhesive layer 30 sequentially formed on a first surface of the substrate 10 .
[0076] In addition, if Figure 2As shown in , a separator for a lithium secondary battery may include: a substrate 10 ; a first heat-resistant layer 20 and a first adhesive layer 30 sequentially formed on a first surface of the substrate 10 ; and a second adhesive layer 30 formed on a second surface of the substrate 10 .
[0077] In addition, if Figure 3 As shown in , a separator for a lithium secondary battery may include: a substrate 10; a second heat-resistant layer 20 and a third adhesive layer 30 sequentially formed on a first surface of the substrate 10; and a third heat-resistant layer 20 and a fourth adhesive layer 30 sequentially formed on a second surface of the substrate 10.
[0078] In the above three examples, the heat-resistant layer and the first to third heat-resistant layers respectively include ceramic 1, and the first to fourth bonding layers respectively include adhesive binders 2 and organic fillers 3, wherein the adhesive binders include polymers having an interpenetrating polymer network (IPN) structure.
[0079] like Figure 2 When the adhesive layer is formed on both surfaces of the substrate and the heat-resistant layer is formed on one surface of the substrate, the Figure 1 Compared with when the heat-resistant layer is formed on one surface of the substrate and the adhesive layer is formed only on the surface on which the heat-resistant layer is formed as shown in , excellent adhesive strength with both the positive electrode and the negative electrode can be ensured.
[0080] In addition, if Figure 3 As shown in , when an adhesive layer is formed on both surfaces of a substrate and a heat-resistant layer is formed on both surfaces of the substrate, Figure 1 and Figure 2 Compared with the case shown in , not only can excellent bonding strength with the positive electrode and the negative electrode be ensured, but also heat resistance can be improved.
[0081] (Lithium secondary battery)
[0082] Another embodiment provides a lithium secondary battery, which includes the separator for a lithium secondary battery according to the above embodiment.
[0083] The separator for a lithium secondary battery of the aforementioned embodiment exhibits excellent thermal stability, structural stability, adhesive strength, gas permeability, etc., and contributes to the stable operation of the lithium secondary battery.
[0084] Hereinafter, except for descriptions repeated in the foregoing, the lithium secondary battery will be described in detail.
[0085] Figure 3 is an exploded perspective view of a lithium secondary battery according to an embodiment. Figure 3According to an embodiment, a lithium secondary battery 100 includes: a battery cell including a negative electrode 112, a positive electrode 114 facing the negative electrode 112, a separator 113 disposed between the negative electrode 112 and the positive electrode 114, and an electrolyte solution (not shown) impregnating the negative electrode 112, the positive electrode 114 and the separator 113; a battery case 120 accommodating the battery cell; and a sealing member 140 sealing the battery case 120.
[0086] Positive electrode
[0087] The positive electrode 114 includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material, a positive electrode binder, and an optional conductive material.
[0088] The positive electrode current collector may use aluminum, nickel, etc., but is not limited thereto.
[0089] The positive electrode active material may use a compound capable of inserting and extracting lithium. For example, at least one of a composite oxide or composite phosphate of a metal selected from cobalt, manganese, nickel, aluminum, iron, or a combination thereof and lithium may be used. For example, the positive electrode active material may be lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, or a combination thereof.
[0090] The binder improves the bonding performance of the positive electrode active material particles to each other and to the current collector, and specific examples may be polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited thereto. These binders may be used alone or as a mixture of two or more.
[0091] The conductive material improves the conductivity of the electrode, and examples of the conductive material may be natural graphite, artificial graphite, carbon black, carbon fiber, metal powder, metal fiber, etc., but are not limited thereto. These conductive materials may be used alone or as a mixture of two or more. Metal powder and metal fiber may use metals such as copper, nickel, aluminum, silver, etc.
[0092] Negative electrode
[0093] The negative electrode 112 includes a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector.
[0094] The negative electrode current collector can be made of copper, gold, nickel, copper alloy, etc., but is not limited thereto.
[0095] The negative electrode active material layer may include a negative electrode active material, a negative electrode binder, and an optional conductive material. The negative electrode active material can be a material that reversibly intercalates / deintercalates lithium ions, lithium metal, a lithium metal alloy, a material capable of doping and dedoping lithium, a transition metal oxide, or a combination thereof.
[0096] The material that reversibly intercalates / deintercalates lithium ions can be a carbon material, which is any common carbon-based negative electrode active material, and examples thereof can be crystalline carbon, amorphous carbon, or a combination thereof. Examples of crystalline carbon can be graphite, such as natural graphite or artificial graphite in irregular, sheet-like, flaky, spherical, or fibrous shapes. Examples of amorphous carbon can be soft carbon or hard carbon, mesophase pitch carbonization products, calcined coke, etc. The lithium metal alloy can be an alloy of lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn. The material capable of doping and dedoping lithium can be Si, SiO x (0 < x < 2), Si-C composite, Si-Y alloy, Sn, SnO2, Sn-C composite, Sn-Y alloy, etc., and at least one of these materials capable of doping and dedoping lithium can be mixed with SiO2. Specific examples of element Y can be selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof. The transition metal oxide can be vanadium oxide, lithium vanadium oxide, etc.
[0097] The binder and conductive material used in the negative electrode 112 can be the same as those of the positive electrode 114 described above.
[0098] The positive electrode 114 and the negative electrode 112 can be manufactured by mixing the corresponding active material composition including the corresponding active material, binder, and optional conductive material in a solvent and coating the active material composition on the corresponding current collector. Here, the solvent can be N-methylpyrrolidone, etc., but is not limited thereto. The electrode manufacturing method is well-known and will not be described in detail in this specification.
[0099] Electrolyte solution
[0100] The electrolyte solution includes an organic solvent and a lithium salt.
[0101] The organic solvent is used as a medium for transmitting ions involved in the electrochemical reaction of the battery. The organic solvent can be a carbonate solvent, an ester solvent, an ether solvent, a ketone solvent, an alcohol solvent, and an aprotic solvent. The carbonate solvent can be dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl ethyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, etc., and the ester solvent can be methyl acetate, ethyl acetate, n-propyl acetate, 1,1-dimethylethyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, decalactone, valerolactone, mevalonolactone, caprolactone, etc. The ether solvent can be dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc., and the ketone solvent can be cyclohexanone, etc. The alcohol solvent can be ethanol, isopropanol, etc., and the aprotic solvent can be nitrile (such as R-CN (R is a linear, branched or cyclic hydrocarbon from C2 to C20, and includes double bonds, aromatic rings, ether bonds), etc.), amide (such as dimethylformamide), dioxolane (such as 1,3-dioxolane), cyclopentane, etc.
[0102] The organic solvent may be used alone or in a mixture of two or more, and if used in a mixture of two or more, the mixing ratio may be controlled according to desired battery performance.
[0103] Lithium salts are dissolved in organic solvents, provide lithium ions in the battery, enable the basic operation of lithium secondary batteries and improve the lithium ion transport between the positive electrode and the negative electrode in the battery. Examples of lithium salts may include LiPF6, LiBF4, LiSbF6, LiAsF6, LiN(SO3C2F5)2, LiN(CF3SO2)2, LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (x and y are natural numbers), LiCl, LiI, LiB(C2O4)2 or a combination thereof, but not limited thereto.
[0104] The lithium salt may be used in a concentration range of 0.1 M to 2.0 M. If the lithium salt is included in the above concentration range, the electrolyte solution may have excellent performance and lithium ion mobility due to optimal conductivity and viscosity of the electrolyte solution.
[0105] Examples of the present invention and comparative examples are described below. The following examples are merely examples of the present invention, but the present invention is not limited to the following examples.
[0106]
Preparation example
[0107] Preparation Example 1: Preparation of a binder (acrylic rubber) for a heat-resistant layer
[0108] In a 10L four-necked flask equipped with a stirrer, a thermometer and a cooling tube, distilled water (6361g), acrylic acid (72.06g, 1.0mol), acrylamide (604.1g, 8.5mol), potassium persulfate (2.7g, 0.01mol), 2-acrylamide-2-methylpropanesulfonic acid (103.6g, 0.5mol) and 5N lithium hydroxide aqueous solution (based on the total amount of 2-acrylamide-2-methylpropanesulfonic acid is 1.05 equivalents) were charged. After the internal pressure of the flask was reduced to 10mmHg by using a diaphragm pump, the internal pressure of the flask was restored to normal pressure by using nitrogen. This series of operations was repeated three times.
[0109] Subsequently, the reaction solution (reaction product) in the flask was reacted for 12 hours while its temperature was controlled to be stable in the range of 65° C. to 70° C. Next, the reaction solution was cooled to room temperature, and treated with a 25% ammonia aqueous solution to adjust the pH to 7 to 8. Then, about 10 mL of the reaction solution (reaction product) was taken out to measure the non-volatile component, which was 9.5% (theoretical value: 10%).
[0110] The non-volatile component is poly(acrylic acid-co-acrylamide-co-2-acrylamide-2-methylpropanesulfonic acid) sodium salt having repeating units derived from acrylic acid, repeating units derived from acrylamide and repeating units derived from 2-acrylamido-2-methylpropanesulfonic acid in a molar ratio of 10:85:5, which is obtained as a binder (acrylic rubber) for the heat-resistant layer.
[0111] Preparation Example 2: Preparation of a composition for a heat-resistant layer
[0112] Boehmite (manufacturer: NabalTec AG) having a D50 particle size of 300 nm was ground with a sand mill for 2 hours, and water was added thereto, thereby preparing a boehmite dispersion (boehmite content: 40 wt %).
[0113] The binder for the heat-resistant layer according to Preparation Example 1 was mixed with a boehmite dispersion to have a boehmite content of 95 wt % in the mixed solution, and water was added thereto to adjust the total solid (binder for the heat-resistant layer and boehmite) content to 5 wt %, thereby preparing a heat-resistant layer composition. In the heat-resistant layer composition, boehmite and the binder for the heat-resistant layer had a weight ratio of 30:1 based on the solid content. Preparation Example 3: Preparation of a composition for an adhesive layer having an IPN structure and an organic filler having a weight ratio of 1:1
[0114] As an adhesive binder having an IPN structure, a polymer including a cross-linked acrylate polymer and a cross-linked vinylidene fluoride polymer in a weight ratio of 3:7 and having a total weight average molecular weight of 500,000 g / mol (product name: LBG4330LX, manufacturer: Arkema) was prepared.
[0115] As the organic filler, polyvinylidene fluoride particles (product name: Sole flatex 2062, manufacturer: Solvay SA) having a D50 particle diameter of 250 nm and having a weight average molecular weight of 500,000 g / mol were prepared.
[0116] Here, the weight average molecular weight of the adhesive binder having an IPN structure and the weight average molecular weight of the organic filler are the average molecular weights of polystyrene measured by using gel permeation chromatography. Hereinafter, the weight average molecular weight mentioned hereinafter is measured in the same manner as described above, and therefore will not be further mentioned.
[0117] An adhesive binder having an IPN structure and an organic filler were mixed at a weight ratio of 1:1, and polyvinyl alcohol (PVA, manufacturer: Sumitomo Corporation) was added thereto to prepare a composition for an adhesive layer. Here, polyvinyl alcohol was added in an amount of 2 wt % based on the total amount of the composition for an adhesive layer.
[0118] Preparation Example 4: Preparation of a composition for an adhesive layer having an IPN structure and an organic filler in a weight ratio of 2:1
[0119] A composition for an adhesive layer according to Preparation Example 4 was prepared in the same manner as in Preparation Example 3, except that the adhesive binder having an IPN structure and the organic filler were mixed at a weight ratio of 2:1.
[0120] Preparation Example 5: Preparation of a composition for an adhesive layer having an IPN structure and an organic filler in a weight ratio of 1:3
[0121] A composition for an adhesive layer according to Preparation Example 5 was prepared in the same manner as in Preparation Example 3, except that the adhesive binder having an IPN structure and the organic filler were mixed in a weight ratio of 1:3.
[0122] Preparation Example 6: Preparation of a composition for an adhesive layer having an IPN structure and an organic filler in a weight ratio of 3:1
[0123] A composition for an adhesive layer according to Preparation Example 6 was prepared in the same manner as in Preparation Example 3, except that the adhesive binder having an IPN structure and the organic filler were mixed at a weight ratio of 3:1.
[0124] Preparation Example 7: Preparation of a composition for an adhesive layer having an IPN structure and an organic filler in a weight ratio of 1:2
[0125] A composition for an adhesive layer according to Preparation Example 7 was prepared in the same manner as in Preparation Example 3, except that the adhesive binder having an IPN structure and the organic filler were mixed in a weight ratio of 1:2.
[0126] Preparation Comparative Example 1: Preparation of a composition for an adhesive layer having a non-IPN structure and an organic filler in a weight ratio of 1:1
[0127] Polyacrylate (a linear polymer having a weight average molecular weight of 500,000 g / mol) was prepared as an adhesive binder having a non-IPN structure.
[0128] A composition for an adhesive layer according to Preparation Comparative Example 1 was prepared in the same manner as in Preparation Example 3, except that a linear polymer (polyacrylate) was used.
[0129] Preparation Comparative Example 2: Preparation of a composition for an adhesive layer having a non-IPN structure and an organic filler in a weight ratio of 1:3
[0130] Polyacrylate (a linear polymer having a weight average molecular weight of 500,000 g / mol) was prepared as an adhesive binder having a non-IPN structure.
[0131] A composition for an adhesive layer according to Preparation Comparative Example 2 was prepared in the same manner as in Preparation Example 5, except that the linear polymer polyacrylate was used.
[0132] Preparation Comparative Example 3: Preparation of a composition for an adhesive layer having a non-IPN structure and an organic filler in a weight ratio of 1:1
[0133] PVdF-HFP (polyvinylidene fluoride-co-hexafluoropropylene) copolymer (linear polymer having a weight average molecular weight of 500,000 g / mol) was prepared as an adhesive binder having a non-IPN structure.
[0134] A composition for an adhesive layer according to Preparation Comparative Example 3 was prepared in the same manner as in Preparation Example 3, except that the linear polymer PVdF-HFP was used.
[0135] Preparation Comparative Example 4: Preparation of a composition for an adhesive layer having a non-IPN structure and an organic filler in a weight ratio of 1:3
[0136] PVdF-HFP (polyvinylidene fluoride-co-hexafluoropropylene) copolymer (linear polymer having a weight average molecular weight of 500,000 g / mol) was prepared as an adhesive binder having a non-IPN structure.
[0137] A composition for an adhesive layer according to Preparation Comparative Example 4 was prepared in the same manner as in Preparation Example 5, except that the linear polymer PVdF-HFP was used.
[0138] Preparation Comparative Example 5: Preparation of a composition for an adhesive layer including an adhesive binder having a non-IPN structure
[0139] A vinylidene fluoride-acrylic acid copolymer (product name: Solef 5130, manufacturer: Solvay SA) having a weight average molecular weight of about 1,100,000 g / mol and including acrylic acid (AA) within 1 wt % was prepared as an adhesive binder having a non-IPN structure.
[0140] A composition for an adhesive layer according to Preparation Comparative Example 5 was prepared in the same manner as in Preparation Example 5, except that the vinylidene fluoride-acrylic acid copolymer was used.
[0141] [Example]
[0142] Example 1
[0143] The composition for a heat-resistant layer according to Preparation Example 2 was coated on the first surface of a 5.5 μm thick polyethylene monofilm substrate by a gravure coating method. The coated substrate was dried at 70° C. and a wind speed of 15 m / sec for 10 seconds to obtain a substrate coated with a 2 μm thick heat-resistant layer on one side.
[0144] The composition for an adhesive layer according to Preparation Example 3 is coated only on the heat-resistant layer on the first surface of the substrate coated with the heat-resistant layer on one side by a gravure coating method, and on the second surface, the composition for an adhesive layer according to Preparation Example 3 is also coated by a gravure coating method.
[0145] Subsequently, the coated substrate was dried at 70° C. and a wind speed of 15 m / sec for 10 seconds to obtain a Figure 2 The separator has the structure of [adhesive layer / substrate / heat-resistant layer / adhesive layer] shown in . Here, the loading amount of the adhesive layer provided on both surfaces of the substrate is 0.5 g / ㎡ on each surface and 1.0 g / ㎡ in total on both surfaces.
[0146] Example 2
[0147] A separator according to Example 2 was manufactured in the same manner as in Example 1, except that the composition for an adhesive layer of Preparation Example 4 was used instead of the composition for an adhesive layer of Preparation Example 3.
[0148] Example 3
[0149] A separator according to Example 3 was manufactured in the same manner as in Example 1, except that the composition for an adhesive layer of Preparation Example 5 was used instead of the composition for an adhesive layer of Preparation Example 3.
[0150] Example 4
[0151] A separator according to Example 4 was manufactured in the same manner as in Example 1, except that the composition for an adhesive layer of Preparation Example 6 was used instead of the composition for an adhesive layer of Preparation Example 3.
[0152] Example 5
[0153] A separator according to Example 5 was manufactured in the same manner as in Example 1, except that the composition for an adhesive layer of Preparation Example 7 was used instead of the composition for an adhesive layer of Preparation Example 3.
[0154]
Comparison example
[0155] Comparative Example 1
[0156] A separator according to Comparative Example 1 was manufactured in the same manner as that of Example 1, except that the composition for an adhesive layer of Preparation Example 1 was used instead of the composition for an adhesive layer of Preparation Example 3.
[0157] Comparative Example 2
[0158] A separator according to Comparative Example 2 was manufactured in the same manner as in Example 1, except that the composition for an adhesive layer of Preparation Example 2 was used instead of the composition for an adhesive layer of Preparation Example 3.
[0159] Comparison Example 3
[0160] A separator according to Comparative Example 3 was manufactured in the same manner as in Example 1, except that the composition for an adhesive layer of Preparation Example 3 was used instead of the composition for an adhesive layer of Preparation Example 3.
[0161] Comparison Example 4
[0162] A separator according to Comparative Example 4 was manufactured in the same manner as in Example 1, except that the composition for an adhesive layer of Preparation Example 4 was used instead of the composition for an adhesive layer of Preparation Example 3.
[0163] Comparative Example 5
[0164] The adhesive layer was coated on both sides of the substrate, and the heat-resistant layer was not formed on one side. A separator according to Comparative Example 5 was manufactured in the same manner as that of Example 1 except for the above.
[0165] Comparative Example 6
[0166] A separator according to Comparative Example 6 was manufactured in the same manner as in Example 1, except that the composition for an adhesive layer of Preparation Example 5 was used instead of the composition for an adhesive layer of Preparation Example 3.
[0167]
Evaluation example
[0168] Evaluation Example 1: Evaluation of Separator
[0169] (1) Immediate air permeability of the diaphragm after manufacture
[0170] Immediately after the production, the gas permeability of each of the separators for lithium secondary batteries of the Examples and Comparative Examples was measured.
[0171] For example, immediately after manufacturing each of the above-mentioned diaphragms, the diaphragms were processed as samples for measuring air permeability. An air permeability measuring instrument (model: EG01-55-1MR, manufacturer: Asahi Seiko Co., Ltd.) was used to measure the time (seconds) required for 100cc of air to pass through each sample for measuring air permeability at a constant pressure of (0.05MPa). After measuring the time at each 1 point (3 points in total) of the left / center / right of the sample, the average value thereof was recorded in Table 1.
[0172] (2) Thermal shrinkage
[0173] Each separator for lithium secondary battery according to the example and the comparative example was cut into a size of 10 cm × 10 cm to prepare a sample for measuring thermal shrinkage. After drawing a 5 cm × 5 cm quadrilateral on the surface of the sample for measuring thermal shrinkage, the sample was inserted between papers or between alumina powders, placed in an oven at 150 ° C for 1 hour, and taken out therefrom to measure the sides of the quadrilateral and calculate the corresponding shrinkage in the horizontal direction (MD) and the vertical direction (TD), and the results are shown in Table 1.
[0174] (3) Electrode bonding strength
[0175] LiCoO2, polyvinylidene fluoride and carbon black in a weight ratio of 96:2:2 were added to an N-methylpyrrolidone solvent to prepare a slurry. The slurry was coated on an aluminum film, then dried and roll-pressed to manufacture a positive electrode.
[0176] In addition, graphite, CMC, SBR, and carbon black were added to DIW in a weight ratio of 97:1:1.5:0.5 to prepare slurry. The slurry was coated on a copper foil, and then dried and roll-pressed to manufacture a negative electrode.
[0177] Each separator for lithium secondary battery according to the example and the comparative example is cut into a length of 25 mm in width and 80 mm in length, and the polyethylene nonwoven fabric is also cut into the same size. The positive electrode is cut into a width of 30 mm and a length of 80 mm and the positive electrode is arranged on one side of each separator, and the polyethylene nonwoven fabric and the positive electrode are arranged on the other side thereof, thereby manufacturing a unit cell. The unit cell is provided with an electrolyte solution. The electrolyte solution is prepared by dissolving 1M LiBF4 in propylene carbonate (PC).
[0178] For adhesion, the corresponding unit cell was tested at 300kgf / cm at about 80°C for 1 hour. Subsequently, the unit cell was disassembled to separate the separator from the positive electrode plate by about 10mm to 20mm, and after the separator was fixed to the upper fixture and the positive electrode plate was fixed to the lower fixture with a fixture interval of 20mm, the separator was stretched in a 180° direction and the separator was peeled off from the positive electrode plate. The peeling was performed at 20mm / min, and after measuring the force required to peel the separator 40mm from the start of the peeling three times, the average value thereof was calculated. The results are shown in Table 1.
[0179] The adhesive strength of the negative electrode was measured in the same manner as described above, and the results are shown in Table 1. (4) Air Permeability after Hot Pressing in the Presence of Electrolyte Solution
[0180] (a) Each separator for lithium secondary batteries according to the examples and comparative examples was cut into a size of 5 cm×5 cm, and polyethylene nonwoven fabric, aluminum substrate and positive electrode were also cut into the same size. On both sides of the separator, polyethylene nonwoven fabric was arranged to manufacture a unit cell, and the air permeability of the unit cell was measured. A total of three individual unit cells were manufactured.
[0181] (b) An aluminum substrate and a positive electrode are arranged on both sides of each unit cell whose permeability is measured according to (a), and then an electrolyte solution is provided. The electrolyte solution is prepared by dissolving 1M LiBF4 in propylene carbonate (PC). The corresponding battery is tested at about 80°C for 1 hour at 300kgf / cm. Subsequently, the battery is disassembled to remove the aluminum substrate and the positive electrode, the battery is washed with dimethyl carbonate (DMC) for 20 seconds to remove the lithium salt, and after drying the solvent, the permeability is measured.
[0182] The time (seconds) required for 100cc of air to pass through each sample for measuring air permeability at a constant pressure (0.05MPa) was measured using an air permeability meter (Model: EG01-55-1MR, Manufacturer: Asahi Seiko Co., Ltd.) The air permeability of three unit cells was averaged to obtain the change before / after hot pressing, and the results are shown in Table 1.
[0183] (Air permeability after bonding (b) - air permeability before bonding (a))
[0184] (Table 1)
[0185]
[0186] Referring to Table 1, the exemplified separator not only exhibits air permeability within an appropriate range and low heat shrinkage immediately after manufacture, but also maintains high electrode bonding strength and high air permeability within an appropriate range after hot pressing under an electrolyte solution. For example, the separator of the comparative example in which a heat-resistant layer and an adhesive layer are sequentially formed on the first surface of the substrate exhibits at least one of the above-mentioned characteristics that is degraded due to the application of an adhesive binder having a non-IPN structure to the adhesive layer.
[0187] For example, compared to the separators of Examples 1 and 3 in which the same amount of an adhesive binder having an IPN structure was applied, the separators of Comparative Examples 1 and 2 in which a polyacrylate having a linear structure was applied to the adhesive layer as an adhesive binder having a non-IPN structure exhibited significantly deteriorated air permeability after hot pressing under an electrolyte solution and exhibited low air permeability immediately after manufacturing.
[0188] On the other hand, compared with the separators of Examples 1 and 3 in which the same amount of an adhesive binder having an IPN structure was applied, the separators of Comparative Examples 3 and 4 in which PVdF-HFP having a linear structure was applied as an adhesive binder having a non-IPN structure exhibited significantly deteriorated bonding strength with the negative electrode after hot pressing under an electrolyte solution.
[0189] Furthermore, compared with the separator of Example 1, the separator of Comparative Example 5 in which the same adhesive layer as that of Example 1 was formed without a heat-resistant layer exhibited significantly deteriorated heat resistance.
[0190] Therefore, a heat-resistant layer including ceramics is formed on the substrate of the diaphragm to ensure thermal stability and structural stability, and an adhesive layer including an adhesive binder having an IPN structure is formed on the substrate of the diaphragm to ensure bonding strength with the two electrodes (especially the negative electrode), wherein an organic filler as an additional component of the adhesive layer is important for ensuring proper air permeability after hot pressing.
[0191] While the invention has been described in conjunction with what are presently considered to be practical example embodiments, it is to be understood that the invention is not limited to the disclosed embodiments, but is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims.
[0192] <symbol description>
[0193] 1: Ceramics
[0194] 2: Adhesive adhesive
[0195] 3: Organic fillers
[0196] 10: Base
[0197] 20: Heat-resistant layer, first heat-resistant layer to third heat-resistant layer
[0198] 30: Adhesive layer, first adhesive layer to fourth adhesive layer
[0199] 100: Lithium secondary battery
[0200] 112: Negative electrode
[0201] 113: Diaphragm
[0202] 114: Positive electrode
[0203] 120: Battery housing
[0204] 140: Sealing member.
Claims
1. A separator for a lithium secondary battery, the separator for a lithium secondary battery comprising: A heat-resistant layer and an adhesive layer are sequentially formed on at least one surface of a substrate, Wherein, the heat-resistant layer comprises ceramics, The adhesive layer includes an adhesive binder and an organic filler, and The adhesive binder includes a polymer having an interpenetrating polymer network structure.
2. The separator for a lithium secondary battery according to claim 1, wherein: The adhesive binder is an adhesive binder in which a cross-linked acrylate polymer and a cross-linked vinylidene fluoride polymer form an interpenetrating polymer network.
3. The separator for a lithium secondary battery according to claim 2, wherein: The weight ratio of the cross-linked acrylate polymer to the cross-linked vinylidene fluoride polymer in the adhesive binder is 8:2 to 1:
9.
4. The separator for a lithium secondary battery according to claim 1, wherein The adhesive binder has a weight average molecular weight greater than or equal to 100,000 g / mol.
5. The separator for a lithium secondary battery according to claim 1, wherein The organic filler is a material having a high melting point of 100°C to 200°C.
6. The separator for a lithium secondary battery according to claim 1, wherein The organic filler is a particle-type filler including a vinylidene fluoride polymer.
7. The separator for a lithium secondary battery according to claim 1, wherein: The organic filler has a D50 particle size of 50 nm to 1,000 nm.
8. The separator for a lithium secondary battery according to claim 1, wherein The organic filler has a weight average molecular weight greater than or equal to 100,000 g / mol.
9. The separator for a lithium secondary battery according to claim 1, wherein: The weight ratio of the adhesive binder to the organic filler in the adhesive layer is 5:95 to 85:
15.
10. The separator for a lithium secondary battery according to claim 1, wherein The loading amount of the adhesive layer relative to one surface of the substrate is 0.1 g / m 2 Up to 1.0g / m 2 .
11. The separator for a lithium secondary battery according to claim 1, wherein The ceramic is selected from boehmite, Al2O3, B2O3, Ga2O3, TiO2, SnO2, CeO2, MgO, NiO, CaO, GaO, ZnO, ZrO2, Y2O3, SrTiO3, BaTiO3, Mg(OH)2 and combinations thereof.
12. The separator for a lithium secondary battery according to claim 1, wherein The ceramic has a D50 particle size of 1 nm to 2000 nm.
13. The separator for a lithium secondary battery according to claim 1, wherein The heat-resistant layer also includes at least one binder selected from polyvinylidene fluoride, styrene-butadiene rubber, carboxymethyl cellulose, polyvinylidene fluoride-hexafluoropropylene copolymer, ethylene vinyl acetate, hydroxyethyl cellulose, polyvinyl alcohol, polyvinyl butyral, ethylene-acrylic acid copolymer, acrylonitrile, vinyl acetate derivatives, polyethylene glycol and acrylic rubber.
14. The separator for a lithium secondary battery according to claim 13, wherein: The weight ratio of the ceramic to the binder in the heat-resistant layer is 50:1 to 10:
1.
15. The separator for a lithium secondary battery according to claim 1, wherein The heat-resistant layer has a thickness of 0.5 μm to 20 μm.
16. The separator for a lithium secondary battery according to claim 1, wherein The substrate includes polyolefin, polyester, polytetrafluoroethylene, polyacetal, polyamide, polyimide, polycarbonate, polyetheretherketone, polyaryletherketone, polyetherimide, polyamideimide, polybenzimidazole, polyethersulfone, polyphenylene oxide, cyclic olefin copolymer, polyphenylene sulfide, polyethylene naphthalate, glass fiber or a combination thereof.
17. The separator for a lithium secondary battery according to claim 1, wherein: The substrate has a thickness of 1 μm to 40 μm.
18. The separator for a lithium secondary battery according to claim 1, wherein The separator for a lithium secondary battery comprises: the substrate; a first heat-resistant layer and a first adhesive layer, sequentially formed on a first surface of the substrate; and a second adhesive layer, formed on a second surface of the substrate, or the substrate; a second heat-resistant layer and a third adhesive layer, sequentially formed on the first surface of the substrate; and a third heat-resistant layer and a fourth adhesive layer, sequentially formed on the second surface of the substrate, Wherein, the first heat-resistant layer to the third heat-resistant layer respectively include the ceramic, The first to fourth adhesive layers respectively include the adhesive binder and the organic filler, and The adhesive binder includes a polymer having an interpenetrating polymer network structure. 19 . A lithium secondary battery, comprising the separator for a lithium secondary battery according to claim 1 .
20. The lithium secondary battery according to claim 19, wherein: The lithium secondary battery includes an assembly including a positive electrode and a negative electrode.