Monodisperse nano silver powder and preparation method and application thereof
By adding complexing agent and surfactant to the silver salt aqueous solution, combined with kinetic control, the complexity of the preparation process and particle size regulation of monodispersed nano silver powder was successfully solved, and efficient and flexible nano silver powder synthesis and low-temperature sintering performance was achieved. , suitable for high-power and highly integrated electronic devices.
Patent Information
- Application Number
- CN202410920917.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-05
AI Technical Summary
The existing preparation process of monodispersed nano silver powder is complex and cannot accurately control the size of nano silver powder, which limits its universality and efficiency in industrial applications.
By adding complexing agent to the aqueous solution of silver salt to regulate the redox potential, combining dual surfactant and morphological control agent, and then adding reducing agent and alkaline reagent to control the reaction conditions to achieve high-quality synthesis of monodispersed nano silver powder .
It realizes the efficient synthesis of nano silver powder with highly monodispersed, wide particle size regulation window, high unit production capacity and low processing cost in the aqueous phase. It can flexibly regulate particle size in the range of 5 to 700 nm and achieve excellent sintering at low temperatures. performance.
Smart Images

Figure CN118893216A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fine chemical industry, and in particular to a monodisperse nano silver powder and a preparation method and application thereof. Background Art
[0002] Metal powder materials, metal pastes, and metal films have long played a vital role in ensuring the performance and reliability of electronic devices. They have been widely used in heat dissipation and electrical management of high-power equipment. Usually, metal powder materials are prepared into patch materials with specific forms such as conductive glue, solder alloy, glass, metal film, and metal paste to facilitate large-scale industrial use. At present, conductive glue and tin-based solder alloy materials are the most commonly used first-level interconnect conductive materials. However, these materials have a low performance index M value (0.1-1.8×10 6 W / m, M=K / α, where K is the thermal conductivity and α is the thermal expansion coefficient) and low melting point (<250°C), which makes this type of material only suitable for applications in the low temperature range. At the same time, as microelectronic systems continue to develop towards high power / ultra-high power, high-density integrated circuits and nanostructure interconnections, people are in urgent need of developing a new type of metal powder conductive material that can achieve low temperature sintering and high temperature application. Furthermore, the packaging process of microelectronic components and microsystems continues to require lead-free, making the application of new metal powder conductive materials in the electronics industry an inevitable trend.
[0003] In recent years, new metallic silver nanoparticles have played a vital role in many fields, including printed electronics, optoelectronics, energy harvesting, catalysis, chemical sensing, biosensing, imaging and biomedicine, due to their excellent physical and chemical properties. At the same time, silver nanoparticles have also been found to be the best platform for surface enhanced Raman scattering (SERS) detection, providing important improvements for sensitive chemical analysis and allowing single molecule detection in some cases. More importantly, metallic silver materials have excellent electrical conductivity, thermal conductivity, low sintering temperature and high operating temperature, which make them ideal components for electrical interconnection and are expected to become the most promising multifunctional conductive material to meet the requirements of the new generation of electronic products. Therefore, designing a universal and reproducible synthesis method to prepare silver nanoparticles with uniform morphology and monodispersity is the basis for fully utilizing the unique properties and promising applications of silver nanoparticles.
[0004] At present, people have developed a variety of different synthetic preparation technologies to produce uniform silver nanoparticles. According to different reaction conditions, the preparation methods of silver nanoparticles can be divided into chemical reduction method, microemulsion method, template method, electrochemical method, light-induced reduction method, photocatalytic reduction method, microwave-assisted method, ultrasound-assisted method and radiation reduction method. Among them, the liquid phase chemical reduction method has become a commonly used method for preparing silver nanoparticles with different particle sizes and controllable morphologies because the preparation method is simple and rapid, and can be controlled by changing experimental parameters such as the concentration of reactants, temperature, pH value, silver seeds, stabilizers, oxidants, reducing agents, polymers, etc. The preparation reduction mechanism of metallic silver nanoparticles in liquid phase solution is mainly that the silver metal species in the oxidized state are reduced to form electrically neutral silver atoms, and the silver atoms aggregate to form atomic clusters and then further grow into the final silver nanoparticles. This is the result of redox reaction. In the redox reaction, the electrons from the reducing agent are transferred to the metallic silver according to the chemical equation (1):
[0005] mMe n+ +nRed→mMe 0 +nO x+ (1)
[0006] The driving force for a chemical reaction (1) to occur comes from the difference ΔE between the redox potentials of the two half-cell reactions. According to the classic Nernst equation (2), the size of ΔE determines the equilibrium constant of the reaction. The larger ΔE is, the larger the equilibrium constant K is. e The bigger.
[0007] lnKe=nFΔE / RT (2)
[0008] From the Nernst equation (2), it can be seen that the reaction is thermodynamically possible only when the ΔE of the redox reaction is positive. Therefore, the redox potential of the reducing agent must be more negative than the redox potential of the metallic silver species. Furthermore, ΔE should be greater than 0.4 V; otherwise, the reaction may not proceed or proceed too slowly to have any practical significance. However, metallic silver is a strongly electropositive metal with a very strong reaction activity. Its redox potential E 0It is about 0.8V, and it can react rapidly under normal conditions even when mixed with a mild reducing agent, resulting in the difficulty in regulating the morphology, size and nanostructure of the synthesized silver product. Therefore, an effective synthesis strategy is to react the metallic silver species with a complexing agent / metal chelator to form a complex precursor containing a silver substance, thereby reducing the standard redox potential of the silver precursor. Under the redox potential, since the complex formed by silver ions has an increasingly high stability, by cleverly manipulating the chemical properties of the metallic silver complex to change the ΔE value of the redox reaction, the reactivity of the chemical substances in the established metallic silver reducing agent system can be effectively regulated, thereby achieving the purpose of synthesizing high-quality silver nanoparticles.
[0009] Traditionally, people can synthesize silver nanoparticles with uniform particle size and morphology through direct liquid phase chemical reduction methods. However, a single synthesis formula usually only provides a narrow particle size control window. Therefore, if silver nanoparticles of various sizes need to be synthesized, people often need to switch back and forth between many different synthesis steps, which makes it difficult to apply the industrial batch synthesis and preparation of silver nanoparticles, because different reaction conditions often lead to different metallic silver surface properties and particle morphology / size distribution. In order to prepare silver nanoparticles with flexible and precise adjustable particle size, people have explored seed growth synthesis methods, which can effectively avoid heterogeneous nucleation of silver ions in solution and make silver nanoparticles grow uniformly to the target size. However, in the subsequent seed growth synthesis process, it is not possible to completely eliminate the self-nucleation of silver ions in the silver growth solution, especially when a lower seed / silver ion ratio is used, the self-nucleation of silver ions is particularly significant. As an important optimization synthesis scheme, a multi-step method based on kinetic control has been established, which is achieved by maintaining low concentrations and appropriate ratios of seeds and silver ion precursors in each round of growth, thereby ensuring a low reaction rate of single silver nanoparticles, successfully preparing silver nanoparticles of different particle sizes and uniform morphology, and becoming a recognized synthesis strategy. However, multi-step synthesis requires a lot of time, energy and labor, and due to the low concentration of reagents required to ensure a low reaction rate, the reproducibility is low and it is difficult to scale up.
[0010] In addition, a large number of existing patent technologies report that silver nanoparticles (less than 20 nm in size) can be obtained by precipitation of silver salt solution through organic liquid phase chemical reduction. Simply put, a reducing agent such as ascorbic acid, hydrazine hydrate, sodium citrate, dehydrated sodium citrate, polyvinylpyrrolidine, ethylenediaminetetraacetic acid, sodium sulfite or sodium borohydride is added to the silver salt solution, and then a chemical reduction reaction is carried out in a polar solvent such as ethanol, methanol or tetrahydrofuran. Finally, the nanoparticles and the solution are separated by centrifugation. Studies have shown that the synthesis of silver nanoparticles by organic liquid phase chemical reduction of silver salts requires polar solvents as the effective medium (electron transport carrier) of the electron conduction of the reducing agent. In non-polar or weakly polar organic solvents, the path of electron transport is blocked or very slow, resulting in the oxidation-reduction reaction not occurring or the reaction proceeding very slowly. At the same time, only a few metal silver salts have good solubility in organic solvents. Therefore, the universal method of preparing silver nanoparticles by organic liquid phase chemical reduction is greatly limited. At the same time, common organic polar solvents are generally expensive, environmentally unfriendly, the prepared nanoparticles are difficult to clean, and even pose industrial problems such as safety hazards.
[0011] Therefore, it is of great significance to study a method for preparing monodisperse nano-silver powder with simple process and precise control of the size of silver nano-particles, and the application of the prepared monodisperse nano-silver powder in various research fields. Summary of the invention
[0012] In view of this, the present invention provides a monodisperse nano silver powder and a preparation method and application thereof, the purpose of which is to solve the problem that the preparation process of the existing monodisperse nano silver powder is complicated and the size of the nano silver powder cannot be accurately controlled.
[0013] In order to achieve the above object, the present invention adopts the following technical solution:
[0014] The present invention provides a method for preparing monodisperse nano silver powder, comprising the following preparation steps:
[0015] (1) adding a complexing agent to an aqueous solution of a silver salt to regulate the redox potential to obtain a silver salt precursor solution;
[0016] (2) mixing a silver salt precursor solution, a dual surfactant and a morphology control agent to obtain a silver salt precursor mother solution;
[0017] (3) Adding a reducing agent solution and an alkaline reagent solution to the silver salt precursor mother solution and reacting them to obtain monodisperse nano silver powder.
[0018] In step (1) of the present invention, the concentration of the aqueous solution of the silver salt is preferably 0.5 to 12 mol / L, more preferably 3 to 10 mol / L, and more preferably 5 to 8 mol / L, and the silver salt includes one or more of silver nitrate, silver nitrite, silver trifluoroacetate, silver hexafluoroantimonate, silver hexafluorophosphate, silver chloride, silver bromide, silver iodide, silver acetate, silver carbonate, silver sulfate, silver sulfide, and silver cyanate;
[0019] The complexing agent includes water and a solute, and the solute includes one or more of ammonia water, diethanolamine, triethanolamine, tetrasodium iminodisuccinate, 3-dimethylamino-1,2-propylene glycol, ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, sodium thiosulfate and sodium sulfite.
[0020] In the step (1) of the present invention, the temperature for regulating the redox potential is preferably 4 to 80° C., more preferably 15 to 70° C., and more preferably 25 to 50° C.; the redox potential is regulated to make Ag in the silver salt precursor solution + / Ag 0 E 0 <0.8V, so as to reduce the reactivity of silver ions and effectively regulate the reactivity of chemical substances in a given reducing agent system, thereby achieving the purpose of synthesizing high-quality silver nanoparticles.
[0021] In step (2) of the present invention, the dual surfactant includes a nonionic surfactant and an ionic surfactant, the nonionic surfactant includes one or more of polyvinyl pyrrolidone, methyl cellulose, gelatin, polyvinyl alcohol and polyethylene glycol, and the ionic surfactant includes one or more of poly(4-styrene sulfonic acid-co-maleic acid) sodium salt, polydiallyldimethylammonium chloride, polyethyleneimine, sodium polystyrene sulfonate, dodecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, octadecyldimethylbenzylammonium chloride, dodecyldimethylphenylphosphonium bromide, sodium acrylate, N-methylamide carboxylate, dodecylammonium sulfate, dodecyl alcohol polyoxyethylene ether sodium sulfate, sodium dodecyl sulfate, dodecylbenzenesulfonic acid, sodium secondary alkyl sulfonate and dialkyldimethylammonium chloride.
[0022] In step (2) of the present invention, the morphology control agent includes one or more of imidazole, imidazole hydrochloride, 1-methylimidazole, benzimidazole, benzotriazole, methylbenzotriazole, thiazole, 2-aminothiazole and benzothiazole.
[0023] In the present invention, the role of the dual surfactant is to provide surface steric hindrance and high charge density by utilizing the end-capping effect of the surfactant, so that the particles can remain fully dispersed under high concentration unit capacity and high solution ionic strength, wherein the non-ionic surfactant provides anionic surface steric hindrance, and the ionic surfactant provides high charge density on the surface of the silver particles; the role of the morphology control agent is to promote the particles to be spherical and inhibit the appearance of irregular structures such as silver flakes, silver short rod nanoparticles, etc.
[0024] In step (3) of the present invention, the reducing agent solution includes a reducing agent and water, the concentration of the reducing agent solution is 5.5 to 10 mol / L, and the reducing agent includes one or more of formaldehyde, acetaldehyde, glyoxal, glutaraldehyde, benzaldehyde, terephthalaldehyde, formic acid, sodium formate, ethyl formate, propyl formate, glucose, maltose, fructose, galactose and lactose;
[0025] The alkaline reagent solution includes an alkaline reagent and water. The concentration of the alkaline reagent solution is 0.7-1.2 mol / L. The alkaline reagent includes one or more of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, potassium silicate, sodium silicate, potassium carbonate, calcium hydroxide, calcium carbonate, sodium phosphate, sodium metaaluminate, ammonium bicarbonate and sodium hypochlorite.
[0026] In step (3) of the present invention, the addition rate of the reducing agent solution and the alkaline agent solution is independently preferably 0.5 to 20 mL / min, more preferably 3 to 16 mL / min, and more preferably 8 to 12 mL / min;
[0027] The reaction temperature is preferably 4 to 80°C, more preferably 20 to 60°C, more preferably 35 to 55°C, and the reaction time is preferably 20 to 45 min, more preferably 25 to 40°C, more preferably 30 to 35°C;
[0028] The kinetic control of the reduction and precipitation of silver nanoparticles is achieved by controlling the concentration, temperature and injection speed of the reducing agent solution and the alkaline reagent solution.
[0029] The volume ratio of the silver salt aqueous solution, the complexing agent, the reducing agent solution and the alkaline reagent solution of the present invention is preferably 0.1-0.7:0.8-1.5:0.1-0.3:0.1-0.15, more preferably 0.2-0.6:0.9-1.4:0.1-0.3:0.11-0.14, more preferably 0.3-0.5:1-1.2:0.2:0.12-0.13;
[0030] The amount of the dual surfactant is preferably 5-10wt% of the mass of the silver salt, more preferably 6-9wt%, and more preferably 7-8wt%; the amount of the morphology control agent is preferably 0.5-1wt% of the mass of the silver salt, more preferably 0.6-0.9wt%, and more preferably 0.7-0.8wt%.
[0031] In the present invention, after the reaction in step (3), post-treatment is performed, and the post-treatment comprises the following steps:
[0032] The reaction solution is sequentially subjected to the first centrifugal filtration, the first dispersion, washing, the second centrifugal filtration, the second dispersion, surface modification, the third centrifugal filtration, the third dispersion, drying, crushing and sieving to obtain monodisperse nano silver powder.
[0033] In the present invention, in the first centrifugal filtration, the second centrifugal filtration and the third centrifugal filtration, the centrifugal speed is independently preferably 12000-18000rpm, further preferably 13000-17000rpm, more preferably 14000-15000rpm, the centrifugal time is independently preferably 12-25min, further preferably 14-22min, more preferably 15-20min, the filtration is independently preferably suction filtration or filtration, the vacuum degree of the suction filtration is preferably 50-1000Pa, further preferably 200-900Pa, more preferably 400-600Pa; the first dispersion, the second dispersion and the third dispersion are preferably ultrasonic dispersion in water.
[0034] In the present invention, the cleaning is to mix the product after the first centrifugal filtration with a cleaning agent; the concentration of the product after the first dispersion is preferably 10-15%, more preferably 11-14%, and more preferably 12-13%, the cleaning agent includes one or more of hydrogen peroxide, sodium hydroxide, sodium hypochlorite, ethylenediamine hydrochloride, n-butylamine hydrochloride, ethanolamine and n-propanolamine, and the mass ratio of the cleaning agent to the product after the first centrifugal filtration is preferably 2-30:70-98, more preferably 5-25:75-95, and more preferably 8-20:80-92; the mixing speed is preferably 700-900rpm, more preferably 750-850rpm, and more preferably 800-820rpm, and the mixing time is preferably 20-40min, more preferably 24-48min, and more preferably 28-30min.
[0035] In the present invention, the surface modification is to add a solution of a surface modifier to the product after the second dispersion, wherein the surface modifier in the solution of the surface modifier includes one or more of fatty acids, unsaturated fatty acids, fatty acid salts and unsaturated fatty acid salts, and the solvent includes one or more of methanol, ethanol, propanol, butanol, pentanol, hexanol and ethylene glycol, propylene glycol, butanediol or glycerol; the concentration of the solution of the surface modifier is preferably 15-25wt%, more preferably 16-24wt%, more preferably 18-20wt%, and the mass ratio of the product after the second centrifugal filtration to the surface modifier is preferably 98-99.9:0.1-2, more preferably 98.2-99.2:0.8-1.8, and more preferably 98.6-99:1-1.4.
[0036] In the present invention, the drying is preferably drying, freeze drying or spray drying, the drying temperature is preferably 25-60°C, more preferably 30-55°C, more preferably 35-40°C, the drying time is preferably 10-36h, more preferably 14-32h, more preferably 18-24h; the freeze drying temperature is preferably -30--15°C, more preferably -25--18°C, more preferably -22--20°C, the freeze drying time is preferably >4d, more preferably >5d, more preferably >6d; the spray drying temperature is preferably 60-80°C, more preferably 65-75°C, more preferably 68-72°C, the drying time is preferably 15-30min, more preferably 18-28min, more preferably 20-25min.
[0037] The invention also provides nano silver powder prepared by the method for preparing the monodisperse nano silver powder.
[0038] The present invention also provides an application of the nano silver powder in a continuous conductive thick film, and the application comprises the following steps:
[0039] The nano silver powder is mixed with an organic solvent and then sintered to obtain a continuous conductive thick film;
[0040] The organic solvent includes one or more of ethylene glycol, glycerol, ethanol, terpineol, dipropylene glycol methyl ether acetate, diethylene glycol diethyl ether, n-butanol and 1,2-propylene glycol;
[0041] The mass ratio of the nano silver powder to the organic solvent is 40-95:5-60;
[0042] The sintering temperature is 100-350° C., and the sintering time is 5-60 minutes.
[0043] The coating is carried out after mixing in the present invention, and the coating process includes screen printing, inkjet printing or roll coating molding.
[0044] In the present invention, the mass ratio of the nano silver powder to the organic solvent is preferably 45-90:10-55, more preferably 50-85:15-50, and more preferably 55-80:20-45.
[0045] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0046] The present invention chemically reduces the silver salt solution in the aqueous phase by means of a dual synergistic strategy of thermodynamically regulating the redox potential (E0) of the silver salt precursor and kinetically controlling the growth of silver nanoparticles, thereby realizing the aqueous synthesis of quasi-spherical multifunctional nano silver powder with high monodispersity, wide particle size control window, high unit production capacity concentration, controllable scale, and low processing cost. The size of the prepared silver nanoparticles can be flexibly regulated within the range of 5 to 700 nm, the unit production capacity concentration of the nanoparticles can reach 50 to 300 g / L, and the burning loss of the silver powder after washing and drying is less than 1%; at the same time, after the high-quality silver powder obtained by the present invention is modulated with an organic carrier into a conductive slurry, the slurry also achieves excellent low-temperature sintering performance at 100 to 250° C. The present invention provides a method for preparing monodisperse nano silver powder and its application, which provides a material basis for the application fields of high-power, highly integrated devices and new solar cells.
[0047] The application described in the present invention is to prepare high-quality silver nanoparticles into silver nano-paste and then apply them to microelectronic components and have high-power / ultra-high-power high-density integrated microelectronic systems with structural interconnection and lead-free packaging of new energy solar cell conductive electrodes, thereby achieving rapid low-temperature sintering of silver nanoparticles and having important engineering and commercial application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0049] Figure 1 Schematic diagram of the preparation method of the monodisperse nano silver powder of the present invention;
[0050] Figure 2 The SEM images of the nano silver powder obtained in Example 1 at different magnifications;
[0051] Figure 3 The XRD pattern of the nano silver powder obtained in Example 1;
[0052] Figure 4This is a statistical result diagram of the physical size distribution of the nano silver powder obtained in Example 1;
[0053] Figure 5 The SEM images of the nano silver powder obtained in Example 2 at different magnifications;
[0054] Figure 6 This is a statistical result diagram of the physical size distribution of the nano silver powder obtained in Example 2;
[0055] Figure 7 The SEM images of the nano silver powder obtained in Example 3 at different magnifications;
[0056] Figure 8 This is a statistical result diagram of the physical size distribution of the nano silver powder obtained in Example 3;
[0057] Fig. 9 The SEM images of the nano silver powder obtained in Example 4 at different magnifications;
[0058] Fig.10 This is a statistical result diagram of the physical size distribution of the nano silver powder obtained in Example 4;
[0059] Fig.11 The SEM images of the nano silver powder obtained in Example 5 at different magnifications;
[0060] Fig.12 This is a statistical result diagram of the physical size distribution of the nano silver powder obtained in Example 5;
[0061] Fig.13 The SEM images of the nano silver powder obtained in Example 6 at different magnifications;
[0062] Fig.14 This is a statistical result diagram of the physical size distribution of the nano silver powder obtained in Example 6;
[0063] Fig.15 The SEM images of the nano silver powder obtained in Example 7 at different magnifications;
[0064] Fig.16 This is a statistical result diagram of the physical size distribution of the nano silver powder obtained in Example 7;
[0065] Fig.17 This is the SEM image of the nano silver powder obtained in Comparative Example 1;
[0066] Fig.18 This is the SEM image of the nano silver powder obtained in Comparative Example 2;
[0067] Fig.19 These are SEM images of the nano silver paste obtained in Application Example 1 after different curing times, where a is a curing time of 1 min, b is a curing time of 10 min, and c is a curing time of 30 min. DETAILED DESCRIPTION
[0068] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0069] In Examples 1 to 7, Comparative Examples 1 to 2 and Application Example 1 of the present invention, when performing SEM detection, the scanning electron microscope model used is Zess Crossbeam 350, FIB-SEM, the operating voltage is 15 KV, and the working distance is 7 mm; when performing XRD detection, the instrument used is a PANalyticalAeris desktop X-ray powder diffractometer; when performing physical size distribution statistics, the particle size distribution calculation software (Nano Measurer 1.2) is used for statistics, and the number of statistics is 200 nano silver powder particles.
[0070] Example 1
[0071] Under stirring at 30° C. and 300 rpm, 1.3 L of 6.48 mol / L ammonia water was added to 0.2 L of 11.77 mol / L silver nitrate aqueous solution in the inner layer of a 5 L clean glass reactor to obtain a silver salt precursor solution;
[0072] Under stirring at 300 rpm, polyvinyl pyrrolidone (5% by weight of silver nitrate) and polydiallyl dimethyl ammonium chloride (2.5% by weight of silver nitrate) were added to the silver salt precursor solution. After the solution was dissolved, benzotriazole (0.75% by weight of silver nitrate) was added to obtain a silver salt precursor mother liquor. A cold and hot source circulation was introduced into the interlayer of the glass reactor to control the temperature of the silver salt precursor mother liquor to 15°C for standby use.
[0073] At a rotation speed of 300 rpm, 250 mL of formaldehyde aqueous solution (15° C., concentration of 6.16 mol / L) and 125 mL of sodium hydroxide aqueous solution (15° C., concentration of 0.9 mol / L) were added to the silver salt precursor mother solution at 15° C. at a rate of 2 mL / min. After the addition was completed, the mixture was stirred at 300 rpm for 30 min at 15° C. to obtain an aqueous solution of a first monodisperse nano-silver powder;
[0074] The aqueous solution of the first monodisperse nano-silver powder was centrifuged at a speed of 15000 rpm for 20 minutes to obtain a first monodisperse nano-silver powder, and the obtained first monodisperse nano-silver powder was ultrasonically dispersed in 1675 mL of water to obtain an aqueous solution of a second monodisperse nano-silver powder; a hydrogen peroxide aqueous solution (concentration of 30 wt %) of 6.7% of the volume of the aqueous solution of the second monodisperse nano-silver powder was added to the aqueous solution of the second monodisperse nano-silver powder at a speed of 800 rpm for washing, and the solution was stirred at a speed of 800 rpm for 30 minutes and then centrifuged at a speed of 15000 rpm for 15 minutes to obtain a second monodisperse nano-silver powder, and the obtained second monodisperse nano-silver powder was added to the aqueous solution of the second monodisperse nano-silver powder. The powder is ultrasonically dispersed into 1675 mL of water to obtain an aqueous solution of a third monodisperse nano-silver powder; an ethanol solution of stearic acid (the concentration of stearic acid is 20 wt %) in an amount of 1.4% of the volume of the aqueous solution of the third monodisperse nano-silver powder is added to the aqueous solution of the third monodisperse nano-silver powder at a rotation speed of 800 rpm to perform surface in-situ modification and coating to obtain an aqueous solution of modified nano-silver particles; the obtained aqueous solution of modified nano-silver particles is centrifuged at a rotation speed of 15000 rpm for 20 min and then filtered to obtain nano-silver particles; the obtained nano-silver particles are freeze-dried at a temperature of -20°C for 5 days, and then mechanically crushed and airflow-shaped in sequence to obtain nano-silver powder.
[0075] The SEM images of the nano silver powder obtained in Example 1 at different magnifications are as follows: Figure 2 As shown. Figure 2 It can be seen that the nano silver powder obtained in Example 1 is spherical in shape, has uniform morphology and good dispersibility.
[0076] The XRD pattern of the nano silver powder obtained in Example 1 is as follows Figure 3 As shown. Figure 3 It can be seen that the positions of the diffraction peaks in the XRD spectrum ((111), (200), (220), (311), (222)) are consistent with those of the standard crystalline silver card (JCPDB NO4-0783), the crystal structure belongs to the face-centered cubic lattice, and no obvious diffraction peaks of non-silver impurity phases are found in the XRD spectrum. The typical characteristic diffraction peaks of silver powder are sharp and have high intensity, which also indicates that the nano silver powder has high purity and good crystallinity.
[0077] The statistical results of the physical size distribution of the nano silver powder obtained in Example 1 are shown in the figure below: Figure 4 As shown. Figure 4 It can be seen that the average size of the nano silver powder obtained in Example 1 is about 13.5 nm, and the minimum and maximum sizes are distributed between 8 and 25 nm, indicating that the nano silver powder obtained in Example 1 has uniform particle size and good monodispersity.
[0078] Example 2
[0079] Under stirring at 30° C. and 300 rpm, 1.26 L of 7.35 mol / L ammonia water was added to 0.24 L of 10.79 mol / L silver nitrate aqueous solution in the inner layer of a 5 L clean glass reactor to obtain a silver salt precursor solution;
[0080] Under stirring at 300 rpm, polyvinyl pyrrolidone (5% by weight of silver nitrate) and polydiallyl dimethyl ammonium chloride (2.5% by weight of silver nitrate) were added to the silver salt precursor solution. After the solution was dissolved, benzotriazole (0.75% by weight of silver nitrate) was added to obtain a silver salt precursor mother liquor. A cold and hot source circulation was introduced into the interlayer of the glass reactor to control the temperature of the silver salt precursor mother liquor to 18°C for standby use.
[0081] At a rotation speed of 300 rpm, 250 mL of formaldehyde aqueous solution (18° C., concentration of 7.46 mol / L) and 125 mL of sodium hydroxide aqueous solution (18° C., concentration of 0.99 mol / L) were added to the silver salt precursor mother solution at 18° C. at an addition rate of 3 mL / min. After the addition was completed, the mixture was stirred at 300 rpm for 30 min at 18° C. to obtain an aqueous solution of a first monodisperse nano-silver powder;
[0082] The aqueous solution of the first monodisperse nano-silver powder was centrifuged at a speed of 10000 rpm for 20 minutes to obtain a first monodisperse nano-silver powder, and the obtained first monodisperse nano-silver powder was ultrasonically dispersed in 1675 mL of water to obtain an aqueous solution of a second monodisperse nano-silver powder; a hydrogen peroxide aqueous solution (concentration of 30 wt %) of 5.9% of the aqueous solution volume of the second monodisperse nano-silver powder was added to the aqueous solution of the second monodisperse nano-silver powder at a speed of 800 rpm for washing, and the solution was stirred at a speed of 800 rpm for 30 minutes, and then centrifuged at a speed of 10000 rpm for 15 minutes to obtain a second monodisperse nano-silver powder, and the obtained second monodisperse nano-silver powder was ultrasonically dispersed in 1675 mL of water to obtain an aqueous solution of a second monodisperse nano-silver powder; The method comprises the steps of: dispersing the obtained nano-silver particles into 1675 mL of water to obtain an aqueous solution of a third monodisperse nano-silver powder; adding an ethanol solution of stearic acid (the concentration of stearic acid is 20 wt %) in an amount of 1.3% of the volume of the aqueous solution of the third monodisperse nano-silver powder to the aqueous solution of the third monodisperse nano-silver powder at a rotation speed of 800 rpm for 30 min to perform in-situ surface modification and coating to obtain an aqueous solution of modified nano-silver particles; centrifuging the obtained aqueous solution of modified nano-silver particles at a rotation speed of 10000 rpm for 15 min and then filtering to obtain nano-silver particles; freeze-drying the obtained nano-silver particles at a temperature of -25°C for 5 days, and then successively performing mechanical crushing and airflow shaping to obtain nano-silver powder.
[0083] The SEM images of the nano silver powder obtained in Example 2 at different magnifications are as follows: Figure 5 As shown. Figure 5 It can be seen that the nano silver powder obtained in Example 2 is spherical in shape, has uniform morphology and good dispersibility.
[0084] The statistical results of the physical size distribution of the nano silver powder obtained in Example 2 are shown in FIG. Figure 6 As shown. Figure 6 It can be seen that the average size of the nano silver powder obtained in Example 2 is about 30 nm, and the minimum and maximum sizes are distributed between 20 and 43 nm, indicating that the nano silver powder obtained in Example 2 has uniform particle size and good monodispersity.
[0085] Example 3
[0086] Under stirring at 30° C. and 300 rpm, 1.2 L of 8.49 mol / L ammonia water was added to 0.3 L of 9.5 mol / L silver nitrate aqueous solution in the inner layer of a 5 L clean glass reactor to obtain a silver salt precursor solution;
[0087] Under stirring at 300 rpm, add polyvinyl pyrrolidone (5% by weight of silver nitrate) and polydiallyl dimethyl ammonium chloride (2.5% by weight of silver nitrate) to the silver salt precursor solution, add methyl benzotriazole (0.65% by weight of silver nitrate) after dissolution to obtain a silver salt precursor mother liquor, introduce a cold and hot source circulation into the interlayer of the glass reactor, and control the temperature of the silver salt precursor mother liquor to 25°C for standby use.
[0088] At a rotation speed of 300 rpm, 250 mL of formaldehyde aqueous solution (18° C., concentration of 6.78 mol / L) and 125 mL of sodium hydroxide aqueous solution (25° C., concentration of 1.09 mol / L) were added to the silver salt precursor mother solution at 25° C. at an addition rate of 3.125 mL / min. After the addition was completed, the mixture was stirred at 300 rpm for 30 min at 25° C. to obtain an aqueous solution of a first monodisperse nano-silver powder;
[0089] The aqueous solution of the first monodisperse nano-silver powder was centrifuged at a speed of 8000 rpm for 20 minutes to obtain a first monodisperse nano-silver powder, and the obtained first monodisperse nano-silver powder was ultrasonically dispersed in 1675 mL of water to obtain an aqueous solution of a second monodisperse nano-silver powder; a hydrogen peroxide aqueous solution (concentration of 30 wt %) of 5% of the volume of the aqueous solution of the second monodisperse nano-silver powder was added to the aqueous solution of the second monodisperse nano-silver powder at a speed of 800 rpm for washing, and the solution was stirred at a speed of 800 rpm for 30 minutes, and then centrifuged at a speed of 8000 rpm for 15 minutes to obtain a second monodisperse nano-silver powder, and the obtained second monodisperse nano-silver powder was ultrasonically dispersed. to 1675mL of water to obtain an aqueous solution of a third monodisperse nano-silver powder; at a rotation speed of 800rpm, an ethanol solution of stearic acid (the concentration of stearic acid is 20wt%) in an amount of 1.28% of the volume of the aqueous solution of the third monodisperse nano-silver powder is added to the aqueous solution of the third monodisperse nano-silver powder for in-situ surface modification and coating for 30min to obtain an aqueous solution of modified nano-silver particles; the obtained aqueous solution of modified nano-silver particles is centrifuged at a rotation speed of 8000rpm for 15min and then filtered to obtain nano-silver particles; the obtained nano-silver particles are freeze-dried at a temperature of -25°C for 5d, and then mechanically crushed and airflow-shaped in sequence to obtain nano-silver powder.
[0090] The SEM images of the nano silver powder obtained in Example 3 at different magnifications are as follows: Figure 7 As shown. Figure 7 It can be seen that the nano silver powder obtained in Example 3 is spherical in shape, has uniform morphology and good dispersibility.
[0091] The statistical results of the physical size distribution of the nano silver powder obtained in Example 3 are shown in the figure below: Figure 8 As shown. Figure 8 It can be seen that the average size of the nano silver powder obtained in Example 3 is about 58 nm, and the minimum and maximum sizes are distributed between 40 and 80 nm, indicating that the nano silver powder obtained in Example 3 has uniform particle size and good monodispersity.
[0092] Example 4
[0093] Under stirring at 30° C. and 400 rpm, 1 L of a complexing agent (the ratio of water, tetrasodium iminodisuccinate and ammonia water is 700 mL: 198.9 g: 300 mL, wherein the mass fraction of ammonia water is 27%) is added to 0.5 L of a 4.71 mol / L silver nitrate aqueous solution in the inner layer of a 5 L clean glass reactor to obtain a silver salt precursor solution;
[0094] Under stirring at 400 rpm, polyethylene glycol (3.5% by weight of silver nitrate) and poly(4-styrenesulfonic acid-co-maleic acid) sodium salt (5% by weight of silver nitrate) were added to the silver salt precursor solution, and after the solution was dissolved, methylbenzotriazole (0.78% by weight of silver nitrate) was added to obtain a silver salt precursor mother liquor. A cold and hot source circulation was introduced into the interlayer of the glass reactor to control the temperature of the silver salt precursor mother liquor to 30°C for standby use.
[0095] At a rotation speed of 400 rpm, 275 mL of formaldehyde aqueous solution (30° C., concentration of 5.6 mol / L) and 150 mL of sodium hydroxide aqueous solution (30° C., concentration of 0.75 mol / L) were added to the silver salt precursor mother solution at 30° C. at an addition rate of 2.83 mL / min. After the addition was completed, the mixture was stirred at 400 rpm for 30 min at 30° C. to obtain an aqueous solution of a first monodisperse nano-silver powder;
[0096] The aqueous solution of the first monodisperse nano-silver powder was centrifuged at a speed of 7000 rpm for 20 minutes to obtain a first monodisperse nano-silver powder, and the obtained first monodisperse nano-silver powder was ultrasonically dispersed in 1925 mL of water to obtain an aqueous solution of a second monodisperse nano-silver powder; a hydrogen peroxide aqueous solution (concentration of 30 wt %) of 5.3% of the aqueous solution volume of the second monodisperse nano-silver powder was added to the aqueous solution of the second monodisperse nano-silver powder at a speed of 800 rpm for washing, and the second monodisperse nano-silver powder was stirred at a speed of 800 rpm for 30 minutes and then centrifuged at a speed of 7000 rpm for 15 minutes to obtain a second monodisperse nano-silver powder, and the obtained second monodisperse nano-silver powder was ultrasonically dispersed in 1925 mL of water to obtain an aqueous solution of a second monodisperse nano-silver powder; The method comprises the following steps: dispersing the obtained nanosilver particles into 1925 mL of water to obtain an aqueous solution of a third monodisperse nanosilver powder; adding an ethanol solution of stearic acid (the concentration of stearic acid is 20 wt %) in an amount of 1.25% of the volume of the aqueous solution of the third monodisperse nanosilver powder to the aqueous solution of the third monodisperse nanosilver powder at a rotation speed of 800 rpm for 30 min of surface in-situ modification and coating to obtain an aqueous solution of modified nanosilver particles; centrifuging the obtained aqueous solution of modified nanosilver particles at a rotation speed of 7000 rpm for 20 min and then filtering to obtain nanosilver particles; freeze-drying the obtained nanosilver particles at a temperature of -25°C for 5 d, and then successively performing mechanical crushing and airflow shaping to obtain nanosilver powder.
[0097] The SEM images of the nano silver powder obtained in Example 4 at different magnifications are as follows: Fig. 9 As shown. Fig. 9 It can be seen that the nano silver powder obtained in Example 4 is spherical in shape, has uniform morphology and good dispersibility.
[0098] The physical size distribution statistics of the nano silver powder obtained in Example 4 are shown in the figure below: Fig.10 As shown. Fig.10It can be seen that the average size of the nano silver powder obtained in Example 4 is about 72 nm, and the minimum and maximum sizes are distributed between 55 and 90 nm, indicating that the nano silver powder obtained in Example 4 has uniform particle size and good monodispersity.
[0099] Example 5
[0100] Under stirring at 30° C. and 400 rpm, 0.9 L of a complexing agent solution (the amount ratio of water, tetrasodium iminodisuccinate and ammonia water is 600 mL: 200.2 g: 300 mL, wherein the mass fraction of ammonia water is 27%) is added to 0.6 L of a 3.93 mol / L silver nitrate aqueous solution in the inner layer of a 5 L clean glass reactor to obtain a silver salt precursor solution;
[0101] Under stirring at 400 rpm, polyethylene glycol (3.5% by weight of silver nitrate) and poly(4-styrenesulfonic acid-co-maleic acid) sodium salt (5% by weight of silver nitrate) were added to the silver salt precursor solution, and after the solution was dissolved, methylbenzotriazole (0.78% by weight of silver nitrate) was added to obtain a silver salt precursor mother liquor. A cold and hot source circulation was introduced into the interlayer of the glass reactor to control the temperature of the silver salt precursor mother liquor to 50°C for standby use.
[0102] At a rotation speed of 400 rpm, 150 mL of glucose aqueous solution (50° C., concentration of 7.85 mol / L) and 150 mL of sodium hydroxide aqueous solution (50° C., concentration of 0.83 mol / L) were added to the silver salt precursor mother solution at 50° C. at an addition rate of 1.88 mL / min. After the addition was completed, the mixture was stirred at 400 rpm for 30 min at 50° C. to obtain an aqueous solution of a first monodisperse nano-silver powder;
[0103] The aqueous solution of the first monodisperse nano-silver powder was centrifuged at a speed of 6000 rpm for 20 minutes to obtain a first monodisperse nano-silver powder, and the obtained first monodisperse nano-silver powder was ultrasonically dispersed in 1950 mL of water to obtain an aqueous solution of a second monodisperse nano-silver powder; a hydrogen peroxide aqueous solution (with a concentration of 30 wt %) of 4.8% of the volume of the aqueous solution of the second monodisperse nano-silver powder was added to the aqueous solution of the second monodisperse nano-silver powder at a speed of 800 rpm for washing, and the second monodisperse nano-silver powder was centrifuged at a speed of 6000 rpm for 15 minutes after stirring at a speed of 800 rpm for 30 minutes to obtain a second monodisperse nano-silver powder, and the obtained second monodisperse nano-silver powder was ultrasonically dispersed in 1950 mL of water to obtain an aqueous solution of a second monodisperse nano-silver powder; The method comprises the following steps: dispersing the obtained nano-silver particles into 1950 mL of water to obtain an aqueous solution of a third monodisperse nano-silver powder; adding an ethanol solution of stearic acid (the concentration of stearic acid is 20 wt %) in an amount of 1.22% of the volume of the aqueous solution of the third monodisperse nano-silver powder to the aqueous solution of the third monodisperse nano-silver powder at a rotation speed of 800 rpm for 30 min of surface in-situ modification and coating to obtain an aqueous solution of modified nano-silver particles; centrifuging the obtained aqueous solution of modified nano-silver particles at a rotation speed of 6000 rpm for 20 min and then filtering to obtain nano-silver particles; freeze-drying the obtained nano-silver particles at a temperature of -25°C for 5 d, and then successively performing mechanical crushing and airflow shaping to obtain nano-silver powder.
[0104] The SEM images of the nano silver powder obtained in Example 5 at different magnifications are as follows: Fig.11 As shown. Fig.11 It can be seen that the nano silver powder obtained in Example 5 is spherical in shape, has uniform morphology and good dispersibility.
[0105] The physical size distribution statistics of the nano silver powder obtained in Example 5 are shown in the figure below: Fig.12 As shown. Fig.12 It can be seen that the average size of the nano silver powder obtained in Example 5 is about 105 nm, and the minimum and maximum sizes are distributed between 80 and 150 nm, indicating that the nano silver powder obtained in Example 4 has uniform particle size and good monodispersity.
[0106] Example 6
[0107] Under stirring at 30° C. and 400 rpm, 0.87 L of a complexing agent solution (the amount ratio of water, tetrasodium iminodisuccinate and ammonia water is 570 mL: 214.1 g: 300 mL, wherein the mass fraction of ammonia water is 27%) is added to 0.6 L of a 3.93 mol / L silver nitrate aqueous solution in the inner layer of a 5 L clean glass reactor to obtain a silver salt precursor solution;
[0108] Under stirring at 400 rpm, polyethylene glycol (3.5% by weight of silver nitrate) and poly(4-styrenesulfonic acid-co-maleic acid) sodium salt (5% by weight of silver nitrate) were added to the silver salt precursor solution, and after dissolution, methylbenzotriazole (0.78% by weight of silver nitrate) was added to obtain a silver salt precursor mother liquor. A cold and hot source circulation was introduced into the interlayer of the glass reactor to control the temperature of the silver salt precursor mother liquor to 55°C for standby use.
[0109] At a rotation speed of 400 rpm, 150 mL of glucose aqueous solution (55° C., concentration of 8.635 mol / L) and 150 mL of sodium hydroxide aqueous solution (30° C., concentration of 0.91 mol / L) were added to the silver salt precursor mother solution at 55° C. at an addition rate of 1.5 mL / min. After the addition was completed, the mixture was stirred at 400 rpm for 30 min at 55° C. to obtain an aqueous solution of a first monodisperse nano-silver powder;
[0110] The aqueous solution of the first monodisperse nano-silver powder was centrifuged at a speed of 5500 rpm for 20 minutes to obtain a first monodisperse nano-silver powder, and the obtained first monodisperse nano-silver powder was ultrasonically dispersed in 1975 mL of water to obtain an aqueous solution of a second monodisperse nano-silver powder; a hydrogen peroxide aqueous solution (with a concentration of 30 wt %) of 4.3% of the volume of the aqueous solution of the second monodisperse nano-silver powder was added to the aqueous solution of the second monodisperse nano-silver powder at a speed of 800 rpm for washing, and the second monodisperse nano-silver powder was centrifuged at a speed of 5500 rpm for 15 minutes after stirring at a speed of 800 rpm for 30 minutes to obtain a second monodisperse nano-silver powder, and the obtained second monodisperse nano-silver powder was ultrasonically dispersed in 1975 mL of water to obtain an aqueous solution of a second monodisperse nano-silver powder; The invention discloses a method for preparing a nano-silver powder having a surface area of about 5000 nm and a surface area of about 1000 nm. The method comprises the steps of: dispersing the nano-silver powder into 1975 mL of water to obtain an aqueous solution of a third monodisperse nano-silver powder; adding an ethanol solution of stearic acid (the concentration of stearic acid is 20 wt %) in an amount of 1.19% of the volume of the aqueous solution of the third monodisperse nano-silver powder to the aqueous solution of the third monodisperse nano-silver powder at a rotation speed of 800 rpm for 30 min to perform surface in-situ modification and coating to obtain an aqueous solution of modified nano-silver particles; centrifuging the obtained aqueous solution of modified nano-silver particles at a rotation speed of 5500 rpm for 20 min and then filtering to obtain nano-silver particles; freeze-drying the obtained nano-silver particles at a temperature of -25°C for 5 d, and then successively performing mechanical crushing and airflow shaping to obtain nano-silver powder.
[0111] The SEM images of the nano silver powder obtained in Example 6 at different magnifications are as follows: Fig.13 As shown. Fig.13 It can be seen that the nano silver powder obtained in Example 6 is spherical in shape, has uniform morphology and good dispersibility.
[0112] The physical size distribution statistics of the nano silver powder obtained in Example 6 are shown in the figure below: Fig.14 As shown. Fig.14It can be seen that the average size of the nano silver powder obtained in Example 6 is about 200 nm, and the minimum and maximum sizes are distributed between 130 and 310 nm, indicating that the nano silver powder obtained in Example 6 has uniform particle size and good monodispersity.
[0113] Example 7
[0114] Under stirring at 30° C. and 400 rpm, 0.85 L of a complexing agent solution (the amount ratio of water, tetrasodium iminodisuccinate and ammonia water is 550 mL: 237.8 g: 300 mL, wherein the mass fraction of ammonia water is 27%) is added to 0.62 L of a 4.18 mol / L silver nitrate aqueous solution in the inner layer of a 5 L clean glass reactor to obtain a silver salt precursor solution;
[0115] Under stirring at 400 rpm, polyethylene glycol (3.5% by weight of silver nitrate) and poly(4-styrenesulfonic acid-co-maleic acid) sodium salt (5% by weight of silver nitrate) were added to the silver salt precursor solution, and after the solution was dissolved, methylbenzotriazole (0.78% by weight of silver nitrate) was added to obtain a silver salt precursor mother liquor. A cold and hot source circulation was introduced into the interlayer of the glass reactor to control the temperature of the silver salt precursor mother liquor to 60°C for standby use.
[0116] At a rotation speed of 400 rpm, 150 mL of glucose aqueous solution (60° C., concentration of 9.5 mol / L) and 150 mL of sodium hydroxide aqueous solution (60° C., concentration of 1 mol / L) were added to the silver salt precursor mother solution at 60° C. at a rate of 1.25 mL / min. After the addition was completed, the mixture was stirred at 400 rpm for 30 min at 60° C. to obtain an aqueous solution of a first monodisperse nano-silver powder;
[0117] The aqueous solution of the first monodisperse nano-silver powder was centrifuged at a speed of 5000 rpm for 20 minutes to obtain a first monodisperse nano-silver powder, and the obtained first monodisperse nano-silver powder was ultrasonically dispersed in 2000 mL of water to obtain an aqueous solution of a second monodisperse nano-silver powder; a hydrogen peroxide aqueous solution (with a concentration of 30 wt %) of 4% of the volume of the aqueous solution of the second monodisperse nano-silver powder was added to the aqueous solution of the second monodisperse nano-silver powder at a speed of 800 rpm for washing, and the solution was stirred at a speed of 800 rpm for 30 minutes, and then centrifuged at a speed of 5000 rpm for 15 minutes to obtain a second monodisperse nano-silver powder, and the obtained second monodisperse nano-silver powder was ultrasonically dispersed. to 2000mL of water to obtain an aqueous solution of a third monodisperse nano-silver powder; adding an ethanol solution of stearic acid (the concentration of stearic acid is 20wt%) in an amount of 1.16% of the volume of the aqueous solution of the third monodisperse nano-silver powder to the aqueous solution of the third monodisperse nano-silver powder at a rotation speed of 800rpm for 30min to carry out surface in-situ modification and coating to obtain an aqueous solution of modified nano-silver particles; centrifuging the obtained aqueous solution of modified nano-silver particles at a rotation speed of 5000rpm for 20min and then filtering to obtain nano-silver particles; freeze-drying the obtained nano-silver particles at a temperature of -25°C for 5d, and then successively performing mechanical crushing and airflow shaping to obtain nano-silver powder.
[0118] The SEM images of the nano silver powder obtained in Example 7 at different magnifications are as follows: Fig.15 As shown. Fig.15 It can be seen that the nano silver powder obtained in Example 7 is spherical in shape, has uniform morphology and good dispersibility.
[0119] The physical size distribution statistics of the nano silver powder obtained in Example 7 are shown in the figure below: Fig.16 As shown. Fig.16 It can be seen that the average size of the nano silver powder obtained in Example 7 is about 340 nm, and the minimum and maximum sizes are distributed between 200 and 600 nm, indicating that the nano silver powder obtained in Example 7 has uniform particle size and good monodispersity.
[0120] Comparative Example 1
[0121] The step “adding 5% by weight of polyvinyl pyrrolidone and 2.5% by weight of polydiallyl dimethyl ammonium chloride to the silver salt precursor solution” in Example 2 was replaced by “adding 7.5% by weight of polyvinyl pyrrolidone to the silver salt precursor solution”. The other steps were the same as those in Example 2 to obtain nano silver powder.
[0122] The SEM image of the nano silver powder obtained in Comparative Example 1 is as follows: Fig.17 As shown. Fig.17It can be seen that the nano silver powder obtained in Comparative Example 1 shows agglomeration, aggregation or branched growth, which cannot meet the dispersion of single nano silver particles. Therefore, by comparing Example 2 with Comparative Example 1, the use of dual surfactants is fully demonstrated, especially when facing a complex high-concentration synthesis system, the nano silver particles can still maintain colloidal stability in the high ionic strength environment of the solution, which provides a solid synthetic material technical means for preparing high-quality nano silver powder, thereby illustrating the technical superiority of the patented technology of the present invention.
[0123] Comparative Example 2
[0124] The step "adding 0.78% by weight of methylbenzotriazole of silver nitrate after dissolution" in Example 5 is deleted, and the other steps are the same as those in Example 5 to obtain nano silver powder.
[0125] The SEM image of the nano silver powder obtained in Comparative Example 2 is as follows: Fig.18 As shown. Fig.18 It can be seen that the nano silver powder obtained in Comparative Example 2 has a large number of non-spherical nano silver particle impurities, such as nanowires, nanosheet structures, etc. Therefore, by comparing Example 5 with Comparative Example 2, it can be seen that adding a morphology control agent to the synthesis system is an important control factor for preparing a uniform morphology, which is of great significance for obtaining a nano silver powder preparation technology with controllable morphology.
[0126] Application Example 1
[0127] The nano silver powder obtained in Example 2 was mixed with pine alcohol at a mass ratio of 80:20 to obtain a nano silver paste, and the obtained nano silver paste was coated on three glass substrates by screen printing, and the three glass substrates coated with the nano silver paste were sintered at a sintering temperature of 130° C. for 1 min, 10 min and 30 min, respectively, to obtain glass substrates after sintering. The glass substrates after sintering were observed by electron microscope, and the results were as follows: Fig.19 shown.
[0128] The SEM images of the nano silver paste obtained in Application Example 1 after different curing times are shown in the figure below: Fig.19 As shown, a is the curing time of 1 minute, b is the curing time of 10 minutes, and c is the curing time of 30 minutes. Fig.19It can be seen that when the solidification time is 1 min, it can be seen from the SEM image that the nanosilver particles still maintain good monodispersity, and there is no interconnection or mutual melting between the nanosilver particles; when the solidification time is 10 min, it can be clearly found from the SEM image that the nanosilver particles are interconnected and melted together, and there are multiple independent nanosilver particles sintered into nanosilver particles of larger size, and the nanosilver particles are still granular; when the solidification time is 30 min, it can be clearly found from the SEM image that the nanosilver particles are transformed into a low-porosity continuous conductive silver thick film, indicating that the nanosilver powder obtained by the present invention has good low-temperature sintering activity.
[0129] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing monodisperse nano silver powder, characterized in that: The method comprises the following preparation steps: (1) adding a complexing agent to an aqueous solution of a silver salt to regulate the redox potential to obtain a silver salt precursor solution; (2) mixing a silver salt precursor solution, a dual surfactant and a morphology control agent to obtain a silver salt precursor mother solution; (3) Adding a reducing agent solution and an alkaline reagent solution to the silver salt precursor mother solution and reacting them to obtain monodisperse nano silver powder.
2. The method for preparing monodisperse nano silver powder according to claim 1, characterized in that: In the step (1), the concentration of the aqueous solution of the silver salt is 0.5 to 12 mol / L, and the silver salt includes one or more of silver nitrate, silver nitrite, silver trifluoroacetate, silver hexafluoroantimonate, silver hexafluorophosphate, silver chloride, silver bromide, silver iodide, silver acetate, silver carbonate, silver sulfate, silver sulfide and silver cyanate; The complexing agent includes one or more of water, ammonia water, diethanolamine, triethanolamine, tetrasodium iminodisuccinate, 3-dimethylamino-1,2-propylene glycol, ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, sodium thiosulfate and sodium sulfite.
3. The method for preparing a monodisperse nano silver powder according to claim 1 or 2, characterized in that: In the step (1), the temperature for regulating the redox potential is 4 to 80° C. The redox potential is regulated to make Ag in the silver salt precursor solution + / Ag 0 E 0 <0.8V.
4. The method for preparing monodisperse nano silver powder according to claim 3, characterized in that: In the step (2), the dual surfactant includes a nonionic surfactant and an ionic surfactant, the nonionic surfactant includes one or more of polyvinyl pyrrolidone, methyl cellulose, gelatin, polyvinyl alcohol and polyethylene glycol, and the ionic surfactant includes one or more of poly(4-styrene sulfonic acid-co-maleic acid) sodium salt, polydiallyldimethylammonium chloride, polyethyleneimine, sodium polystyrene sulfonate, dodecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, octadecyldimethylbenzylammonium chloride, dodecyldimethylphenylphosphonium bromide, sodium acrylate, N-methylamide carboxylate, dodecylammonium sulfate, sodium dodecyl alcohol polyoxyethylene ether sulfate, sodium dodecyl sulfate, dodecylbenzenesulfonic acid, sodium secondary alkyl sulfonate and dialkyldimethylammonium chloride.
5. The method for preparing monodisperse nano silver powder according to claim 4, characterized in that: In the step (2), the morphology control agent includes one or more of imidazole, imidazole hydrochloride, 1-methylimidazole, benzimidazole, benzotriazole, methylbenzotriazole, thiazole, 2-aminothiazole and benzothiazole.
6. The method for preparing monodisperse nano silver powder according to claim 2 or 4, characterized in that: In the step (3), the reducing agent solution includes a reducing agent and water, the concentration of the reducing agent solution is 5.5 to 10 mol / L, and the reducing agent includes one or more of formaldehyde, acetaldehyde, glyoxal, glutaraldehyde, benzaldehyde, terephthalaldehyde, formic acid, sodium formate, ethyl formate, propyl formate, glucose, maltose, fructose, galactose and lactose; The alkaline reagent solution includes an alkaline reagent and water. The concentration of the alkaline reagent solution is 0.7-1.2 mol / L. The alkaline reagent includes one or more of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, potassium silicate, sodium silicate, potassium carbonate, calcium hydroxide, calcium carbonate, sodium phosphate, sodium metaaluminate, ammonium bicarbonate and sodium hypochlorite.
7. The method for preparing monodisperse nano silver powder according to claim 6, characterized in that: In the step (3), the adding rates of the reducing agent solution and the alkaline agent solution are independently 0.5 to 20 mL / min; the reaction temperature is 4 to 80° C., and the reaction time is 20 to 45 min.
8. The method for preparing monodisperse nano silver powder according to claim 1, characterized in that: The volume ratio of the silver salt aqueous solution, the complexing agent, the reducing agent solution and the alkaline reagent solution is 0.1-0.7:0.8-1.5:0.1-0.3:0.1-0.15; The dosage of the dual surfactant is 5-10wt% of the mass of the silver salt; the dosage of the morphology control agent is 0.5-1wt% of the mass of the silver salt.
9. Nano silver powder obtained by the method for preparing monodisperse nano silver powder according to any one of claims 1 to 8.
10. The use of the nano silver powder in continuous conductive thick film according to claim 9, characterized in that: The application comprises the following steps: The nano silver powder is mixed with an organic solvent and then sintered to obtain a continuous conductive thick film; The organic solvent includes one or more of ethylene glycol, glycerol, ethanol, terpineol, dipropylene glycol methyl ether acetate, diethylene glycol diethyl ether, n-butanol and 1,2-propylene glycol; The mass ratio of the nano silver powder to the organic solvent is 40-95:5-60; The sintering temperature is 100-350° C., and the sintering time is 5-60 minutes.
Citation Information
Cited By
Ultra-long silver nanowire and preparation method and application thereof
CN120551414A
Preparation method of nano silver powder with single particle dispersion
CN121223101A
A method for preparing a nano-silver powder with single particle dispersion
CN121223101B
Preparation method of high-specific-surface-form monodisperse nano silver powder for semiconductor packaging
CN122480325A