Weather-resistant full-biodegradable mulching film and preparation method thereof
By adding reinforcement fillers and weathering agents to the full biodegradable mulch, the problems of humidity and heat aging and photoaging are solved, the degradation cycle is extended, and the UV resistance is improved, and better mechanical properties and stability are achieved.
Patent Information
- Application Number
- CN202411056734.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-05
AI Technical Summary
The existing fully biodegradable plastic films are prone to moisture and heat aging and photoaging, resulting in too short degradation cycle and poor UV resistance, which cannot effectively play a role.
Add reinforcement fillers, dispersants, heat stabilizers, ultraviolet absorbers, light stabilizers, antioxidants and anti-hydrolytic agents to the full biodegradable plastic film to extend its degradation cycle by improving the mechanical properties and weather resistance of the plastic film.
It improves the moisture and heat resistance and UV resistance of the plastic film, extends the degradation cycle, and enhances its stability and mechanical properties during use.
Smart Images

Figure BDA0004976659160000051 
Figure BDA0004976659160000061 
Figure BDA0004976659160000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of degradable materials, and in particular to a weather-resistant fully biodegradable ground film and a preparation method thereof. Background Art
[0002] Plastic mulch cultivation technology can significantly increase the yield of agricultural products. Traditional mulch films are not degradable and difficult to recycle. The corresponding residual films accumulate more and more in cultivated land, polluting the agricultural ecological environment. At present, the main solution to the problem of white pollution is recycling and using degradable mulch films. Recycling has the disadvantages of low residual film recovery rate, serious secondary processing pollution and high labor costs. The fully degradable mulch film not only has the same heat preservation and moisture retention effect as the traditional mulch film, but also can be naturally degraded. There is no need for manual recycling after use. Therefore, it is an effective way to solve mulch film pollution.
[0003] At present, degradable mulch mainly includes biodegradable mulch, photodegradable mulch, photo / biodegradable mulch, plant fiber mulch, etc. Due to the large differences in natural environment in different regions and the different growth cycles of different crops, the degradation cycle of fully biodegradable plastic mulch is too short, which makes it unable to play a good role. This has become a major problem in its use, especially the fact that fully biodegradable mulch is easy to hydrolyze and has poor UV resistance, which makes it prone to moisture-heat aging and light aging during use. Summary of the invention
[0004] In order to solve the technical problem that the existing fully biodegradable mulch film is prone to moisture and heat aging and light aging, resulting in a short degradation cycle, the present invention provides a weather-resistant fully biodegradable mulch film and a preparation method thereof. The fully biodegradable mulch film has good moisture and heat resistance and UV resistance, and also has good mechanical properties, so that its degradation cycle can be extended.
[0005] The specific technical scheme of the present invention is: In a first aspect, the present invention provides a weather-resistant fully biodegradable mulch film, comprising the following raw materials in parts by weight: 60-90 parts of fully biodegradable polyester, 10-30 parts of reinforcing filler, 0.1-1 part of dispersant, 0.5-2 parts of heat stabilizer, 0.2-0.5 parts of chain extender, 0.1-1 parts of ultraviolet absorber, 0.1-2 parts of light stabilizer, 0.1-2 parts of antioxidant, and 0.1-2 parts of anti-hydrolysis agent.
[0006] The invention can improve the mechanical properties of the mulch film by adding reinforcing fillers to the fully biodegradable mulch film and using a dispersant to improve the compatibility between the reinforcing fillers and small molecule additives and the fully biodegradable polyester, so that the mulch film has higher tensile strength and elongation at break.
[0007] In addition, the present invention can improve the weather resistance of the fully biodegradable mulch by adding heat stabilizers, chain extenders, ultraviolet absorbers, light stabilizers, antioxidants and anti-hydrolysis agents, so that the mulch has better moisture and heat resistance and ultraviolet resistance, thereby making the mulch less susceptible to moisture and heat aging and light aging during use and extending its degradation cycle.
[0008] Preferably, the weather-resistant fully biodegradable mulch film further comprises the following raw materials in parts by weight: 0.3-1 part of an opening agent and 0-5 parts of a masterbatch.
[0009] Preferably, the anti-hydrolysis agent comprises a polymeric carbodiimide anti-hydrolysis agent and a monomeric carbodiimide anti-hydrolysis agent in a mass ratio of 1:1.5 to 2.1.
[0010] Monomeric carbodiimide anti-hydrolysis agents have high reactivity. In the early stage of aging of the ground film, they can react with the carboxyl groups generated by aging quickly, thereby quickly blocking the carboxyl groups from continuing to catalyze the breakage of the polyester molecular chain; the molecular chain of the polymeric carbodiimide anti-hydrolysis agent carries multiple N=C=N functional groups. After reacting with the carboxyl groups in the polyester, crosslinking can be formed between multiple polyester molecular chains, thereby improving the mechanical properties of the ground film to a greater extent. Compared with the use of polymeric and monomeric carbodiimide anti-hydrolysis agents alone, the present invention can use the above-mentioned characteristics of the two anti-hydrolysis agents to give the ground film better aging resistance after compounding the two in a specific mass ratio. Preferably, the fully biodegradable polyester includes one or more of polybutylene adipate / terephthalate (PBAT), polylactic acid (PLA), polyvinyl alcohol (PVA), polycaprolactone (PCL) and polybutylene succinate (PBS).
[0011] Preferably, the reinforcing filler includes one or more of calcium carbonate, talc, kaolin and wollastonite; and the dispersant includes one or more of stearic acid, titanate, aluminate and silane coupling agent.
[0012] Preferably, the heat stabilizer includes one or more of calcium stearate, zinc stearate, sodium stearate and tin stearate.
[0013] Preferably, the chain extender comprises a polymeric epoxy functional chain extender.
[0014] Preferably, the light stabilizer includes one or more of the light stabilizer 770 , the light stabilizer 326 and the light stabilizer 292 .
[0015] Preferably, the antioxidant includes one or more of antioxidant 1010 , antioxidant 168 , antioxidant 164 and antioxidant 264 .
[0016] Preferably, the opening agent includes one or more of silicon dioxide, talc, calcium carbonate, oleamide, erucamide and silicone.
[0017] In a second aspect, the present invention provides a method for preparing the weather-resistant fully biodegradable mulch film, comprising the following steps: (1) mixing a reinforcing filler and a dispersant to obtain a powder mixture; (2) blending the powder mixture with other raw materials and extruding and granulating to obtain a masterbatch; (3) The masterbatch is used for film making to obtain a weather-resistant and fully biodegradable ground film.
[0018] In the above preparation process, the reinforcing filler is first mixed with the dispersant and then mixed with other raw materials, so that the dispersant can be better combined with the reinforcing filler, thereby improving the dispersibility of the reinforcing filler in the ground film to a greater extent, and then improving the mechanical properties of the ground film.
[0019] Preferably, step (1) specifically includes the following steps: preheating the mixing device at 80-110°C for 10-30 minutes, adding reinforcing filler, stirring at 80-110°C and 800-2000rpm for 10-30 minutes, adding dispersant, mixing at 80-110°C and 800-2000rpm for 10-60 minutes to obtain a powder mixture.
[0020] After adding the reinforcing filler, the process of mixing at 100-110°C for 10-30 minutes can remove the moisture in the reinforcing filler; then add the dispersant and continue mixing. In this process, the dispersant can adhere to the surface of the reinforcing filler, causing its surface to change and forming an organic film. This film can improve the dispersibility and fluidity of the reinforcing filler.
[0021] Preferably, the anti-hydrolysis agent comprises a polymeric carbodiimide anti-hydrolysis agent and a monomeric carbodiimide anti-hydrolysis agent; step (2) specifically comprises the following steps: mixing the powder mixture with other raw materials except reinforcing filler, dispersant and monomeric carbodiimide anti-hydrolysis agent to obtain a mixture; adding the mixture into a twin-screw extruder for melt blending and extrusion granulation, during which the monomeric carbodiimide anti-hydrolysis agent is added between the mixing section and the exhaust section of the twin-screw extruder to obtain a masterbatch.
[0022] In the mixing process of the present invention, two anti-hydrolysis agents are added in batches, the polymeric carbodiimide anti-hydrolysis agent is first melt-blended with raw materials such as fully biodegradable polyester, and then the monomeric carbodiimide anti-hydrolysis agent is added and melt-blended continuously, which can produce the following effects: the polymeric carbodiimide has better compatibility and dispersibility, is not easy to migrate in the polyester, and can be evenly dispersed in the polyester when added in advance, thereby improving the reaction efficiency with the terminal carboxyl group in the polyester, and the cross-linking reaction in the anti-hydrolysis process is helpful to improve the mechanical properties of the mulch film, although the monomeric carbodiimide has high reaction activity, it is easy to migrate and volatilize, and the latter addition can ensure its effective utilization rate in the processing process, thereby giving the mulch film better aging resistance.
[0023] Furthermore, in step (2), the mixing temperature is 30-60°C, the rotation speed is 800-2000 rpm, and the time is 5-10 min; the barrel temperature of the twin-screw extruder is 170-190°C, and the head temperature is 175-185°C. Preferably, in step (3), the film is made by a film blowing machine, the barrel temperature is 140-150°C, and the head temperature is 140-150°C.
[0024] Compared with the prior art, the present invention has the following advantages: (1) The present invention can improve the moisture-heat aging and light aging resistance of the mulch by adding a heat stabilizer, a chain extender, a UV absorber, a light stabilizer, an antioxidant and an anti-hydrolysis agent to the fully biodegradable mulch, thereby helping to extend its degradation cycle during use.
[0025] (2) The present invention can effectively improve the mechanical properties of the mulch and give it higher tensile strength and elongation at break by adding reinforcing fillers and dispersants to the fully biodegradable mulch and removing moisture from the reinforcing fillers during the preparation of the mulch before mixing it with the dispersants and then mixing it with other raw materials.
[0026] (3) The present invention adopts a specific ratio of polymeric and monomeric carbodiimide anti-hydrolysis agents, and adopts the order of adding the polymeric type first and then the monomeric type in the melt blending process of preparing the ground film, which can improve the aging resistance of the ground film to a greater extent and make it have better mechanical properties after wet heat aging and light aging. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with the embodiments.
[0028] Overall embodiment A weather-resistant fully biodegradable mulch film comprises the following raw materials in parts by weight: 60-90 parts of fully biodegradable polyester, 10-30 parts of reinforcing filler, 0.1-1 part of dispersant, 0.5-2 parts of heat stabilizer, 0.2-0.5 parts of chain extender, 0.1-1 part of ultraviolet absorber, 0.1-2 parts of light stabilizer, 0.1-2 parts of antioxidant and 0.1-2 parts of anti-hydrolysis agent.
[0029] As a specific implementation, the anti-hydrolysis agent includes a polymeric carbodiimide anti-hydrolysis agent and a monomeric carbodiimide anti-hydrolysis agent in a mass ratio of 1:1.5 to 2.1.
[0030] As a specific embodiment, the fully biodegradable polyester includes one or more of polybutylene adipate / terephthalate (PBAT), polylactic acid (PLA), polyvinyl alcohol (PVA), polycaprolactone (PCL) and polybutylene succinate (PBS).
[0031] As a specific implementation, the reinforcing filler includes one or more of calcium carbonate, talc, kaolin and wollastonite; the dispersant includes one or more of stearic acid, titanate, aluminate and silane coupling agent.
[0032] As a specific embodiment, the heat stabilizer includes one or more of calcium stearate, zinc stearate, sodium stearate and tin stearate; the chain extender includes a polymeric epoxy functional chain extender; the light stabilizer includes one or more of light stabilizer 770, light stabilizer 326 and light stabilizer 292; the antioxidant includes one or more of antioxidant 1010, antioxidant 168, antioxidant 164 and antioxidant 264.
[0033] As a specific implementation, the weather-resistant fully biodegradable mulch film further includes the following raw materials in parts by weight: 0.3-1 parts of an opening agent and 0-5 parts of a masterbatch; the opening agent includes one or more of silicon dioxide, talc, calcium carbonate, oleamide, erucamide and silicone.
[0034] A method for preparing the weather-resistant fully biodegradable mulch film comprises the following steps: (1) mixing a reinforcing filler and a dispersant to obtain a powder mixture; (2) blending the powder mixture with other raw materials and extruding and granulating to obtain a masterbatch; (3) The masterbatch is used for film making to obtain a weather-resistant and fully biodegradable ground film.
[0035] As a specific implementation, step (1) specifically includes the following steps: preheating the mixing device at 80-110°C for 10-30 minutes, adding reinforcing filler, stirring at 80-110°C and 800-2000rpm for 10-30 minutes, then adding dispersant, mixing at 80-110°C and 800-2000rpm for 10-60 minutes to obtain a powder mixture.
[0036] As a specific implementation, the anti-hydrolysis agent includes a polymeric carbodiimide anti-hydrolysis agent and a monomeric carbodiimide anti-hydrolysis agent; step (2) specifically includes the following steps: mixing the powder mixture with other raw materials except reinforcing filler, dispersant and monomeric carbodiimide anti-hydrolysis agent at 30-60°C and 800-2000rpm for 5-10min to obtain a mixture; adding the mixture into a twin-screw extruder for melt blending and extrusion granulation, during which the monomeric carbodiimide anti-hydrolysis agent is added between the mixing section and the exhaust section of the twin-screw extruder, and the barrel temperature of the twin-screw extruder is set to 170-190°C, and the head temperature is set to 175-185°C to obtain a masterbatch.
[0037] As a specific implementation, in step (3), the film forming is carried out by a film blowing machine, the barrel temperature is 140-150°C, and the head temperature is 140-150°C. Specific embodiments The present invention is described below by specific examples. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. Without departing from the spirit and scope of the inventive concept, changes and advantages that can be thought of by those skilled in the art are included in the present invention, and the attached claims and any equivalents thereof are the protection scope of the present invention.
[0039] Unless otherwise defined, all technical terms and scientific terms used in the present invention have the same meanings as those commonly understood by ordinary technicians in the field to which the present disclosure belongs. Unless otherwise specified, the raw materials and equipment used in the present invention are conventional raw materials and equipment in the field and can be obtained from conventional commercial channels; unless otherwise specified, the methods used in the present invention are conventional methods in the field.
[0040] Example 1 A fully biodegradable mulch film is prepared by the following steps: (1) According to the formula in Table 1, weigh each raw material.
[0041] Table 1 Raw material formula of Example 1 (2) Preheat the high-speed mixer at 80° C. for 10 min, add the reinforcing filler into the high-speed mixer, and premix at 80° C. and 800 rpm for 10 min, then add the dispersant into the high-speed mixer, and mix at 80° C. and 800 rpm for 10 min to obtain a powder mixture.
[0042] (3) pouring the powder mixture prepared in step (2) and the remaining raw materials except hymax@1010 into a high-speed mixer, mixing at 30° C. and 800 rpm for 10 min to prepare a mixture; (4) The mixed material obtained in step (3) is added to a twin-screw extruder (a conventional main feeding + side feeding twin-screw extruder is used, which includes five sections: conveying section, melting section, mixing section, exhaust section and homogenizing section, and the side feeding section is set between the mixing section and the exhaust section) for melt blending and extrusion granulation. During this period, hymax@1010 is added between the mixing section and the exhaust section of the twin-screw extruder to obtain masterbatch. The temperature of the twin-screw extruder is set as follows: the barrel temperature is 170°C and the head temperature is 175°C.
[0043] (5) Add the masterbatch prepared in step (4) into a film blowing machine, and set the temperature of the film blowing machine as follows: the barrel temperature is 140° C., and the head temperature is 140° C. The film is blown by the film blowing machine to obtain a fully biodegradable ground film.
[0044] Example 2 A fully biodegradable mulch film is prepared by the following steps: (1) According to the formula in Table 2, weigh each raw material.
[0045] Table 2 Raw material formula of Example 2 (2) Preheat the high-speed mixer at 110° C. for 30 minutes, add the reinforcing filler into the high-speed mixer, and premix at 110° C. and 2000 rpm for 30 minutes. Then add the dispersant into the high-speed mixer, and mix at 80° C. and 2000 rpm for 60 minutes to obtain a powder mixture.
[0046] (3) pouring the powder mixture prepared in step (2) and the remaining raw materials except hymax@1010 into a high-speed mixer, mixing at 60° C. and 2000 rpm for 5 min to prepare a mixture; (4) The mixed material obtained in step (3) is added to a twin-screw extruder (a conventional main feeding + side feeding type twin-screw extruder is used, which includes five sections: conveying section, melting section, mixing section, exhaust section and homogenizing section, and the side feeding section is set between the mixing section and the exhaust section) for melt blending and extrusion granulation. During this period, hymax@1010 is added between the mixing section and the exhaust section of the twin-screw extruder to obtain masterbatch. The temperature of the twin-screw extruder is set as follows: the barrel temperature is 190°C and the head temperature is 185°C.
[0047] (5) Add the masterbatch prepared in step (4) into a film blowing machine, and set the temperature of the film blowing machine as follows: the barrel temperature is 150° C., and the head temperature is 150° C. The film is blown by the film blowing machine to obtain a fully biodegradable ground film.
[0048] Example 3 A fully biodegradable mulch film is prepared by the following steps: (1) According to the formula in Table 3, weigh each raw material.
[0049] Table 3 Raw material formula of Example 3 (2) Preheat the high-speed mixer at 110° C. for 30 minutes, add the reinforcing filler into the high-speed mixer, and premix at 110° C. and 2000 rpm for 30 minutes. Then add the dispersant into the high-speed mixer, and mix at 80° C. and 2000 rpm for 60 minutes to obtain a powder mixture.
[0050] (3) pouring the powder mixture prepared in step (2) and the remaining raw materials except hymax@1010 into a high-speed mixer, mixing at 60° C. and 2000 rpm for 5 min to prepare a mixture; (4) The mixed material obtained in step (3) is added to a twin-screw extruder (a conventional main feeding + side feeding type twin-screw extruder is used, which includes five sections: conveying section, melting section, mixing section, exhaust section and homogenizing section, and the side feeding section is set between the mixing section and the exhaust section) for melt blending and extrusion granulation. During this period, hymax@1010 is added between the mixing section and the exhaust section of the twin-screw extruder to obtain masterbatch. The temperature of the twin-screw extruder is set as follows: the barrel temperature is 190°C and the head temperature is 185°C.
[0051] (5) Add the masterbatch prepared in step (4) into a film blowing machine, and set the temperature of the film blowing machine as follows: the barrel temperature is 150° C., and the head temperature is 150° C. The film is blown by the film blowing machine to obtain a fully biodegradable ground film.
[0052] Example 4 A fully biodegradable mulch film is prepared by the following steps: (1) According to the formula in Table 4, weigh each raw material.
[0053] Table 4 Raw material formula of Example 4 (2) Preheat the high-speed mixer at 80° C. for 10 min, add the reinforcing filler into the high-speed mixer, and premix at 80° C. and 800 rpm for 10 min, then add the dispersant into the high-speed mixer, and mix at 80° C. and 800 rpm for 10 min to obtain a powder mixture.
[0054] (3) pouring the powder mixture prepared in step (2) and the remaining raw materials except hymax@1010 into a high-speed mixer, mixing at 30° C. and 800 rpm for 10 min to prepare a mixture; (4) The mixed material obtained in step (3) is added to a twin-screw extruder (a conventional main feeding + side feeding twin-screw extruder is used, which includes five sections: conveying section, melting section, mixing section, exhaust section and homogenizing section, and the side feeding section is set between the mixing section and the exhaust section) for melt blending and extrusion granulation. During this period, hymax@1010 is added between the mixing section and the exhaust section of the twin-screw extruder to obtain masterbatch. The temperature of the twin-screw extruder is set as follows: the barrel temperature is 170°C and the head temperature is 175°C.
[0055] (5) Add the masterbatch prepared in step (4) into a film blowing machine, and set the temperature of the film blowing machine as follows: the barrel temperature is 140° C., and the head temperature is 140° C. The film is blown by the film blowing machine to obtain a fully biodegradable ground film.
[0056] Comparative Example 1 A fully biodegradable mulch film is prepared by the following steps: (1) According to the formula in Table 5, weigh each raw material.
[0057] Table 5 Raw material formula of comparative example 1 (2) Pour all the raw materials except hymax@1010 into a high-speed mixer and mix at 30°C and 800 rpm for 10 min to prepare a mixture; (3) The mixed material obtained in step (2) is added to a twin-screw extruder (a conventional main feeding + side feeding type twin-screw extruder is used, which includes five sections: conveying section, melting section, mixing section, exhaust section and homogenizing section, and the side feeding section is set between the mixing section and the exhaust section) for melt blending and extrusion granulation. During this period, hymax@1010 is added between the mixing section and the exhaust section of the twin-screw extruder to obtain masterbatch. The temperature of the twin-screw extruder is set as follows: the barrel temperature is 170°C and the head temperature is 175°C.
[0058] (4) Add the masterbatch prepared in step (3) into a film blowing machine, and set the temperature of the film blowing machine as follows: the barrel temperature is 140° C., and the head temperature is 140° C. The film is blown by the film blowing machine to obtain a fully biodegradable ground film.
[0059] Comparative Example 2 A fully biodegradable mulch film is prepared by the following steps: (1) According to the formula in Table 6, weigh each raw material.
[0060] Table 6 Raw material formula of comparative example 2 (2) Preheat the high-speed mixer at 80° C. for 10 min, add the reinforcing filler into the high-speed mixer, and premix at 80° C. and 800 rpm for 10 min, then add the dispersant into the high-speed mixer, and mix at 80° C. and 800 rpm for 10 min to obtain a powder mixture.
[0061] (3) pouring the powder mixture prepared in step (2) and the remaining raw materials into a high-speed mixer, mixing at 30° C. and 800 rpm for 10 min to prepare a mixture; (4) Add the mixed material obtained in step (3) into a twin-screw extruder for melt blending and extrusion granulation to obtain masterbatch. The temperature of the twin-screw extruder is set as follows: the barrel temperature is 170°C, and the head temperature is 175°C.
[0062] (5) Add the masterbatch prepared in step (4) into a film blowing machine, and set the temperature of the film blowing machine as follows: the barrel temperature is 140° C., and the head temperature is 140° C. The film is blown by the film blowing machine to obtain a fully biodegradable ground film.
[0063] Comparative Example 3 A fully biodegradable mulch film is prepared by the following steps: (1) According to the formula in Table 1 above, weigh each raw material.
[0064] (2) Pour all the raw materials except hymax@1010 into a high-speed mixer and mix at 30°C and 800 rpm for 10 min to prepare a mixture; (3) The mixed material obtained in step (2) is added to a twin-screw extruder (a conventional main feeding + side feeding type twin-screw extruder is used, which includes five sections: conveying section, melting section, mixing section, exhaust section and homogenizing section, and the side feeding section is set between the mixing section and the exhaust section) for melt blending and extrusion granulation. During this period, hymax@1010 is added between the mixing section and the exhaust section of the twin-screw extruder to obtain masterbatch. The temperature of the twin-screw extruder is set as follows: the barrel temperature is 170°C and the head temperature is 175°C.
[0065] (4) Add the masterbatch prepared in step (3) into a film blowing machine, and set the temperature of the film blowing machine as follows: the barrel temperature is 140° C., and the head temperature is 140° C. The film is blown by the film blowing machine to obtain a fully biodegradable ground film.
[0066] Comparative Example 4 A fully biodegradable mulch film is prepared by the following steps: (1) According to the formula in Table 7, weigh each raw material.
[0067] Table 7 Raw material formula of comparative example 4 (2) Preheat the high-speed mixer at 80° C. for 10 min, add the reinforcing filler into the high-speed mixer, and premix at 80° C. and 800 rpm for 10 min, then add the dispersant into the high-speed mixer, and mix at 80° C. and 800 rpm for 10 min to obtain a powder mixture.
[0068] (3) pouring the powder mixture prepared in step (2) and the remaining raw materials into a high-speed mixer, mixing at 30° C. and 800 rpm for 10 min to prepare a mixture; (4) Add the mixed material obtained in step (3) into a twin-screw extruder for melt blending and extrusion granulation to obtain masterbatch. The temperature of the twin-screw extruder is set as follows: the barrel temperature is 170°C, and the head temperature is 175°C.
[0069] (5) Add the masterbatch prepared in step (4) into a film blowing machine, and set the temperature of the film blowing machine as follows: the barrel temperature is 140° C., and the head temperature is 140° C. The film is blown by the film blowing machine to obtain a fully biodegradable ground film.
[0070] Comparative Example 5 A fully biodegradable mulch film is prepared by the following steps: (1) According to the formula in Table 8, weigh each raw material.
[0071] Table 8 Raw material formula of comparative example 5 (2) Preheat the high-speed mixer at 110° C. for 30 minutes, add the reinforcing filler into the high-speed mixer, and premix at 110° C. and 2000 rpm for 30 minutes. Then add the dispersant into the high-speed mixer, and mix at 80° C. and 2000 rpm for 60 minutes to obtain a powder mixture.
[0072] (3) pouring the powder mixture prepared in step (2) and the remaining raw materials into a high-speed mixer, mixing at 60° C. and 2000 rpm for 5 min to prepare a mixture; (4) Add the mixed material obtained in step (3) into a twin-screw extruder for melt blending and extrusion granulation to obtain masterbatch. The temperature of the twin-screw extruder is set as follows: the barrel temperature is 190°C and the head temperature is 185°C.
[0073] (5) Add the masterbatch prepared in step (4) into a film blowing machine, and set the temperature of the film blowing machine as follows: the barrel temperature is 150° C., and the head temperature is 150° C. The film is blown by the film blowing machine to obtain a fully biodegradable ground film.
[0074] Comparative Example 6 A fully biodegradable mulch film is prepared by the following steps: (1) According to the formula in Table 9, weigh each raw material.
[0075] Table 9 Raw material formula of comparative example 6 (2) Preheat the high-speed mixer at 80° C. for 10 min, add the reinforcing filler into the high-speed mixer, and premix at 80° C. and 800 rpm for 10 min, then add the dispersant into the high-speed mixer, and mix at 80° C. and 800 rpm for 10 min to obtain a powder mixture.
[0076] (3) pouring the powder mixture prepared in step (2) and the remaining raw materials except hymax@1010 into a high-speed mixer, mixing at 30° C. and 800 rpm for 10 min to prepare a mixture; (4) The mixed material obtained in step (3) is added to a twin-screw extruder (a conventional main feeding + side feeding twin-screw extruder is used, which includes five sections: conveying section, melting section, mixing section, exhaust section and homogenizing section, and the side feeding section is set between the mixing section and the exhaust section) for melt blending and extrusion granulation. During this period, hymax@1010 is added between the mixing section and the exhaust section of the twin-screw extruder to obtain masterbatch. The temperature of the twin-screw extruder is set as follows: the barrel temperature is 170°C and the head temperature is 175°C.
[0077] (5) Add the masterbatch prepared in step (4) into a film blowing machine, and set the temperature of the film blowing machine as follows: the barrel temperature is 140° C., and the head temperature is 140° C. The film is blown by the film blowing machine to obtain a fully biodegradable ground film.
[0078] Comparative Example 7 A fully biodegradable mulch film is prepared by the following steps: (1) According to the formula in Table 10, weigh each raw material.
[0079] Table 10 Raw material formula of comparative example 7 (2) Preheat the high-speed mixer at 110° C. for 30 minutes, add the reinforcing filler into the high-speed mixer, and premix at 110° C. and 2000 rpm for 30 minutes. Then add the dispersant into the high-speed mixer, and mix at 80° C. and 2000 rpm for 60 minutes to obtain a powder mixture.
[0080] (3) pouring the powder mixture prepared in step (2) and the remaining raw materials except hymax@1010 into a high-speed mixer, mixing at 60° C. and 2000 rpm for 5 min to prepare a mixture; (4) The mixed material obtained in step (3) is added to a twin-screw extruder (a conventional main feeding + side feeding type twin-screw extruder is used, which includes five sections: conveying section, melting section, mixing section, exhaust section and homogenizing section, and the side feeding section is set between the mixing section and the exhaust section) for melt blending and extrusion granulation. During this period, hymax@1010 is added between the mixing section and the exhaust section of the twin-screw extruder to obtain masterbatch. The temperature of the twin-screw extruder is set as follows: the barrel temperature is 190°C and the head temperature is 185°C.
[0081] (5) Add the masterbatch prepared in step (4) into a film blowing machine, and set the temperature of the film blowing machine as follows: the barrel temperature is 150° C., and the head temperature is 150° C. The film is blown by the film blowing machine to obtain a fully biodegradable ground film.
[0082] Comparative Example 8 A fully biodegradable mulch film is prepared by the following steps: (1) According to the formula in Table 1 above, weigh each raw material.
[0083] (2) Preheat the high-speed mixer at 80° C. for 10 min, add the reinforcing filler into the high-speed mixer, and premix at 80° C. and 800 rpm for 10 min, then add the dispersant into the high-speed mixer, and mix at 80° C. and 800 rpm for 10 min to obtain a powder mixture.
[0084] (3) pouring the powder mixture prepared in step (2) and the remaining raw materials into a high-speed mixer, mixing at 30° C. and 800 rpm for 10 min to prepare a mixture; (4) Add the mixed material obtained in step (3) into a twin-screw extruder for melt blending and extrusion granulation to obtain masterbatch. The temperature of the twin-screw extruder is set as follows: the barrel temperature is 170°C, and the head temperature is 175°C.
[0085] (5) Add the masterbatch prepared in step (4) into a film blowing machine, and set the temperature of the film blowing machine as follows: the barrel temperature is 140° C., and the head temperature is 140° C. The film is blown by the film blowing machine to obtain a fully biodegradable ground film.
[0086] Comparative Example 9 A fully biodegradable mulch film is prepared by the following steps: (1) According to the formula in Table 1 above, weigh each raw material.
[0087] (2) Preheat the high-speed mixer at 80° C. for 10 min, add the reinforcing filler and the dispersant into the high-speed mixer, and mix at 80° C. and 800 rpm for 20 min to obtain a powder mixture.
[0088] (3) pouring the powder mixture prepared in step (2) and the remaining raw materials except hymax@1010 into a high-speed mixer, mixing at 30° C. and 800 rpm for 10 min to prepare a mixture; (4) The mixed material obtained in step (3) is added to a twin-screw extruder (a conventional main feeding + side feeding twin-screw extruder is used, which includes five sections: conveying section, melting section, mixing section, exhaust section and homogenizing section, and the side feeding section is set between the mixing section and the exhaust section) for melt blending and extrusion granulation. During this period, hymax@1010 is added between the mixing section and the exhaust section of the twin-screw extruder to obtain masterbatch. The temperature of the twin-screw extruder is set as follows: the barrel temperature is 170°C and the head temperature is 175°C.
[0089] (5) Add the masterbatch prepared in step (4) into a film blowing machine, and set the temperature of the film blowing machine as follows: the barrel temperature is 140° C., and the head temperature is 140° C. The film is blown by the film blowing machine to obtain a fully biodegradable ground film.
[0090] Comparative Example 10 This comparative example is a commercially available fully biodegradable agricultural mulch film.
[0091] Test Case Take the fully biodegradable mulch films prepared in the embodiments and comparative examples, and use a manual punching machine to make dumbbell-shaped test specimens in the longitudinal and transverse directions, and perform performance tests according to the following method: (1) Determination of tensile strength and elongation at break: According to the national standard "Determination of Tensile Properties of Plastics" (GB / T 1040.3-2006) Part 3: Test conditions for films and sheets, the dumbbell-shaped specimen length, gauge length 40mm, narrow parallel part width 6mm, thickness 0.020-0.050mm, tensile speed 200mm / min, room temperature 25℃.
[0092] (2) Artificial accelerated photoaging experiment: Use fluorescent UV lamp with wavelength of 365mm and irradiation intensity of 2W / m 2 . Cycle process: 8 hours of light, irradiation intensity 2W / m 2 , 4 hours of condensation. After continuous testing for 240 hours, the tensile mechanical properties of the samples were tested.
[0093] (3) Artificial accelerated heat and humidity aging test: Double "85" constant temperature and humidity test, that is, the temperature is set to 85℃ and the humidity is 85%. After continuous testing for 72 hours, the tensile mechanical properties of the samples are tested.
[0094] The performance test results are shown in Tables 11 and 12.
[0095] Table 11 Light aging performance test results Table 12 Test results of wet heat aging performance By analyzing the test results in Table 7 and Table 8, it can be seen that: (1) The tensile strength and elongation at break of Examples 1-4 before aging are higher than those of Comparative Example 10, and the decrease in tensile strength and elongation at break after light aging and heat and humidity aging is significantly lower than that of Comparative Example 10. This indicates that the use of the formula and method of the present invention to prepare a fully biodegradable mulch can effectively improve the mechanical properties and heat and humidity and UV resistance of the mulch.
[0096] (2) The tensile strength and elongation at break of Example 1 are higher than those of Comparative Example 1 and Comparative Example 3, and Comparative Example 3 is higher than Comparative Example 1. This indicates that the mechanical properties of the mulch film can be improved by adding a dispersant. On this basis, the mechanical properties of the mulch film can be further improved by first mixing the reinforcing filler and the dispersant and then mixing them with other raw materials during the preparation process.
[0097] (3) The decrease in tensile strength and elongation at break of Example 1 after light aging and wet heat aging is significantly lower than that of Comparative Example 3. This indicates that by adding heat stabilizers, chain extenders, ultraviolet absorbers, light stabilizers, antioxidants and anti-hydrolysis agents to the fully biodegradable mulch film, the moisture and heat resistance and ultraviolet resistance of the mulch film can be effectively improved.
[0098] (4) The decrease in tensile strength and elongation at break of Example 1 after light aging and wet heat aging is lower than that of Comparative Examples 4 and 6, and the decrease in Example 2 is lower than that of Comparative Examples 5 and 7. This indicates that compared with the use of polymeric and monomeric carbodiimide anti-hydrolysis agents alone, the use of the two in a specific ratio can improve the moisture and heat resistance and UV resistance of the mulch film.
[0099] (5) The decrease in tensile strength and elongation at break of Example 1 after light aging and wet heat aging is lower than that of Comparative Example 8. This indicates that in the melt blending process, compared with adding the polymeric and monomeric carbodiimide anti-hydrolysis agents together, the order of adding the polymeric and monomeric carbodiimide anti-hydrolysis agents first can improve the moisture and heat resistance and UV resistance of the mulch film.
[0100] (6) The tensile strength and elongation at break of Example 1 are higher than those of Comparative Example 9. This indicates that in the mixing process, the mechanical properties of the ground film can be improved by first heating and stirring the reinforcing filler to remove moisture and then blending it with the dispersant.
[0101] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A weather-resistant fully biodegradable mulch film, characterized in that: The invention comprises the following raw materials in parts by weight: 60-90 parts of fully biodegradable polyester, 10-30 parts of reinforcing filler, 0.1-1 parts of dispersant, 0.5-2 parts of heat stabilizer, 0.2-0.5 parts of chain extender, 0.1-1 parts of ultraviolet absorber, 0.1-2 parts of light stabilizer, 0.1-2 parts of antioxidant and 0.1-2 parts of anti-hydrolysis agent.
2. The weather-resistant fully biodegradable mulch film according to claim 1, characterized in that: The invention also comprises the following raw materials in parts by weight: 0.3-1 part of an opening agent and 0-5 parts of a color masterbatch.
3. The weather-resistant fully biodegradable mulch film according to claim 1, characterized in that: The anti-hydrolysis agent includes a polymeric carbodiimide anti-hydrolysis agent and a monomeric carbodiimide anti-hydrolysis agent in a mass ratio of 1:1.5-2.
1.
4. The weather-resistant fully biodegradable mulch film according to claim 1, characterized in that: The fully biodegradable polyester includes one or more of polybutylene adipate / terephthalate, polylactic acid, polyvinyl alcohol, polycaprolactone and polybutylene succinate.
5. The weather-resistant fully biodegradable mulch film according to claim 1, characterized in that: The reinforcing filler includes one or more of calcium carbonate, talc, kaolin and wollastonite; the dispersant includes one or more of stearic acid, titanate, aluminate and silane coupling agent.
6. The weather-resistant fully biodegradable mulch film according to claim 2, characterized in that: The opening agent includes one or more of silicon dioxide, talc, calcium carbonate, oleamide, erucamide and silicone.
7. A method for preparing the weather-resistant fully biodegradable mulch film according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) Mixing a reinforcing filler and a dispersant to obtain a powder mixture; (2) Blending the powder mixture with other raw materials and extruding and granulating to obtain a masterbatch; (3) Masterbatch is used to make film to obtain weather-resistant and fully biodegradable ground film.
8. The preparation method according to claim 7, characterized in that: Step (1) specifically includes the following steps: preheating the mixing device at 80-110° C. for 10-30 minutes, adding reinforcing filler, stirring at 80-110° C. and 800-2000 rpm for 10-30 minutes, adding dispersant, mixing at 80-110° C. and 800-2000 rpm for 10-60 minutes, and obtaining a powder mixture.
9. The preparation method according to claim 7, characterized in that: The anti-hydrolysis agent includes a polymeric carbodiimide anti-hydrolysis agent and a monomeric carbodiimide anti-hydrolysis agent; step (2) specifically includes the following steps: mixing the powder mixture with other raw materials except the reinforcing filler, the dispersant and the monomeric carbodiimide anti-hydrolysis agent to obtain a mixture; adding the mixture into a twin-screw extruder for melt blending and extrusion granulation, during which the monomeric carbodiimide anti-hydrolysis agent is added between the mixing section and the exhaust section of the twin-screw extruder to obtain a masterbatch.
10. The preparation method according to claim 9, characterized in that: In step (2), the mixing temperature is 30-60°C, the rotation speed is 800-2000 rpm, and the time is 5-10 min; the barrel temperature of the twin-screw extruder is 170-190°C, and the head temperature is 175-185°C.
Citation Information
Cited By
Waterproof breathable film with thermal insulation performance and preparation method thereof
CN120775223A
Hydrolysis-resistant master batch, functional period adjustable degradable mulching film and preparation method
CN121379070A
Degradable lithium ion battery cell coating base material and preparation method thereof
CN122521096A