Surface coloring method of magnesium alloy object and surface-colored magnesium alloy object
Through pulsed anodizing treatment and erosion treatment, regular pores and pit structures are formed, which solves the problem of uneven dyeing caused by uneven pore distribution in the anodizing treatment of magnesium alloy surface, and improves the interference color and dyeing effect of magnesium alloy surface. Improves decorativeness and reduces power consumption.
Patent Information
- Application Number
- CN202311779753.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-02
- Filing Date
- 2023-12-20
- Publication Date
- 2024-11-05
AI Technical Summary
The pore distribution formed by the anodizing treatment of existing magnesium alloys is unevenly distributed, resulting in uneven dyeing and insufficient dye depth.
An anodizing layer with multiple openings with regular arrangement is formed by pulsed anodizing treatment, and a pit structure is formed in combination with erosion treatment. The hole sealing treatment is then performed to seal the openings, improving the light interference and dyeing effect.
The interference color intensity and dyeing effect of the magnesium alloy surface are improved, the decorative and appearance color effect is improved, and the power consumption is reduced and the production efficiency is improved.
Smart Images

Figure CN118895546A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a surface coloring method for a light metal object, in particular to a surface coloring method for a magnesium alloy object, and a surface colored magnesium alloy object obtained by the method. Background Art
[0002] Portable electronic products on the market today are mainly thin, light and compact. Magnesium alloy has become a popular material for making housings or other mechanical parts of portable electronic products due to its excellent mechanical properties and light weight.
[0003] In order to meet the product's appearance diversity and functionality, objects made of magnesium alloy are usually treated on the surface, such as anodizing, to form an anodized film to prevent the magnesium alloy from being directly exposed to the air, decorate the surface of the magnesium alloy, and improve the wear resistance and corrosion resistance of the magnesium alloy. In addition, the anodized film has the characteristics of being porous and can absorb dyes to change the appearance color of the product. However, the pore distribution formed by general anodizing treatment is not uniform, which makes the dyeing prone to unevenness; in addition, the pore structure formed by general anodizing treatment prevents the dye from effectively penetrating, resulting in insufficient dyeing depth. Summary of the invention
[0004] The object of the present invention is to provide a method for coloring the surface of a magnesium alloy object, and a magnesium alloy object with a colored surface obtained by the method, so as to solve the problems existing in the above-mentioned prior art.
[0005] The concept of the present invention is to first form an anodized layer with multiple openings arranged regularly and with good uniformity on the outer surface of a magnesium alloy object through an anodizing treatment, and then cooperate with a bite-etching treatment to form a plurality of pits on the surface of the anodized layer away from the magnesium alloy object, and each pit corresponds to and is connected to at least one opening, which is beneficial to improving the light interference coloring effect and the dye dyeing effect.
[0006] Specifically, one of the technical solutions adopted by the present invention is to provide a method for surface coloring of a magnesium alloy object, comprising: providing a magnesium alloy object; performing anodizing treatment on the magnesium alloy object to form an anodized layer on the outer surface of the magnesium alloy object, the anodized layer having a plurality of openings extending toward the outer surface of the magnesium alloy object; performing a bite-etching treatment on the anodized layer to form a plurality of pits on the surface of the anodized layer away from the magnesium alloy object, and each of the pits corresponds to and is connected to at least one of the openings; and performing a sealing treatment on the anodized layer after the bite-etching.
[0007] In an embodiment of the present invention, the anodizing treatment is performed in an electrolyte, and the electrolyte contains an oxidant, a pH regulator, and a film-forming agent. The oxidant is selected from the group consisting of sodium nitrate, potassium nitrate, potassium permanganate, and potassium dichromate, the pH regulator is selected from the group consisting of sodium hydroxide, potassium hydroxide, lithium hydroxide, and magnesium hydroxide, and the film-forming agent is selected from the group consisting of sodium silicate, aluminum hydroxide, ammonium dihydrogen phosphate, sodium hexametaphosphate, and trisodium phosphate.
[0008] In an embodiment of the present invention, the anodizing treatment is a pulsed anodizing treatment, which includes a voltage ramp-up stage and a voltage constant voltage stage following the voltage ramp-up stage, wherein the operating voltage of the voltage ramp-up stage is increased from an initial voltage to a target voltage, and the operating voltage of the voltage constant voltage stage is maintained at the target voltage.
[0009] In an embodiment of the present invention, the conditions of the pulsed anodizing treatment include: the initial voltage is 0V and the target voltage is 20V to 600V, the pulse frequency is 500Hz to 2000Hz, and the duty cycle is 1% to 50%. In addition, the duration of the voltage ramp-up phase is 1 minute to 10 minutes, and the duration of the voltage constant phase is 5 minutes to 60 minutes, which is more than four times the duration of the voltage ramp-up phase.
[0010] In an embodiment of the present invention, the etching treatment is to use an etching liquid to corrode the surface of the anodized layer, and the etching liquid is an aqueous solution containing nitric acid, sulfuric acid, phosphoric acid, oxalic acid, citric acid and / or their salts, and the duration of the etching treatment is 10 seconds to 1200 seconds.
[0011] In an embodiment of the present invention, the surface coloring method of the magnesium alloy object of the present invention further comprises: between the step of performing the etching treatment and the step of performing the sealing treatment, filling at least one dye into the plurality of openings of the anodized layer.
[0012] In an embodiment of the present invention, the sealing treatment is to cover the surface of the anodized layer with a sealing layer by electrosealing to seal the plurality of openings.
[0013] In an embodiment of the present invention, the sealing layer is formed of a resin composition, the resin composition comprises an acrylic resin and a solid powder, the solid powder is a powder of a metal, a non-metal or its oxide, and the solid content of the resin composition is 3% to 30%. In addition, the implementation conditions of the electric sealing include: an operating voltage of 1V to 150V, and a duration of 30 seconds to 10 minutes.
[0014] In an embodiment of the present invention, the sealing treatment further comprises baking the resin composition under the following conditions: a baking temperature of 100° C. to 200° C. and a baking time of 15 minutes to 60 minutes.
[0015] In order to solve the above technical problems, another technical solution adopted by the present invention is to provide a magnesium alloy object with a colored surface, which includes a magnesium alloy object, an anodized layer and a sealing layer. The anodized layer is formed on the outer surface of the magnesium alloy object and has a plurality of openings extending toward the outer surface of the magnesium alloy object. In addition, a plurality of pits are formed on the surface of the anodized layer away from the magnesium alloy object, and each of the pits is connected to at least one of the openings. The sealing layer covers the surface of the anodized layer to seal the plurality of openings.
[0016] One of the beneficial effects of the present invention is that the surface coloring method of the magnesium alloy object of the present invention can improve the interference color intensity (the interference color is clear and noticeable) and the dyeing effect of the magnesium alloy surface through the combination of the technical features of "performing anodizing treatment on the magnesium alloy object to form an anodized layer on the outer surface of the magnesium alloy object, and the anodized layer has a plurality of openings extending toward the outer surface of the magnesium alloy object" and "performing a bite treatment on the anodized layer to form a plurality of pits on the surface of the anodized layer away from the magnesium alloy object, and each of the pits is connected to at least one of the openings", so as to improve the decorativeness of the magnesium alloy surface and change the appearance color effect of the magnesium alloy surface.
[0017] In order to further understand the features and technical contents of the present invention, please refer to the following detailed description and drawings of the present invention. However, the drawings provided are only for reference and description and are not intended to limit the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 FIG. 1 is a flow chart of a surface coloring method for a magnesium alloy object according to an embodiment of the present invention.
[0019] Figure 2 Another flow chart of the surface coloring method of a magnesium alloy object according to an embodiment of the present invention.
[0020] Figure 3 Schematic diagram of the processing stages of anodizing treatment used in the surface coloring method of a magnesium alloy object according to an embodiment of the present invention.
[0021] Figure 4 It is a schematic structural diagram of a surface-colored magnesium alloy object according to an embodiment of the present invention.
[0022] Figure 5 for Figure 4 1 is a partial enlarged view of the V portion of , which shows that the surface-colored magnesium alloy object according to the embodiment of the present invention does not have any dye.
[0023] Figure 6 for Figure 5 , which shows that the surface-colored magnesium alloy object according to an embodiment of the present invention has a dye on it. DETAILED DESCRIPTION
[0024] The following is an explanation of the implementation methods of the "surface coloring method of magnesium alloy objects and surface colored magnesium alloy objects" disclosed in the present invention through specific embodiments. Those skilled in the art can understand the advantages and effects of the present invention from the contents disclosed in this specification. The present invention can be implemented or applied through other different specific embodiments, and the details in this specification can also be modified and changed in various ways based on different viewpoints and applications without departing from the concept of the present invention. In addition, the drawings of the present invention are only simple schematic illustrations and are not depicted in actual size. It is stated in advance. The following embodiments will further explain the relevant technical contents of the present invention in detail, but the disclosed contents are not intended to limit the scope of protection of the present invention. In addition, the term "or" used in this article may include any one or more combinations of the associated listed items depending on the actual situation.
[0025] Unless otherwise defined, the terms used herein have the same meanings as those generally understood by those skilled in the art. The materials involved in each embodiment are commercially available or prepared according to the prior art unless otherwise specified. The process methods involved in each embodiment are the process methods commonly used in the art unless otherwise specified.
[0026] It should be understood that although the steps in the method flow chart are described in a specific order in this article, this does not require or imply that the steps must be performed in this specific order, or that all steps must be performed to achieve the desired result. Optionally, multiple steps can be combined into one step for execution, or one step can be decomposed into multiple steps for execution.
[0027] The concept of the present invention is to first form an anodized layer with multiple openings arranged regularly and with good uniformity on the outer surface of a magnesium alloy object through an anodizing treatment, and then cooperate with a bite-etching treatment to form a plurality of pits on the surface of the anodized layer away from the magnesium alloy object, and each pit is connected to at least one opening to improve the intensity of the interference color (the interference color is clear and noticeable) and the dyeing effect.
[0028] See also Figure 1As shown, the concept of the present invention is specifically embodied in a surface coloring method for a magnesium alloy object, which mainly includes: step S100, providing a magnesium alloy object; step S102, performing anodizing treatment; step S104, performing etching treatment; and step S106, performing pore sealing treatment. Figure 4 and Figure 5 As shown, the anodizing treatment in step S102 is to form an anodized layer 2 on the outer surface 100 (surface to be colored) of the magnesium alloy object 1, and the anodized layer 2 has a plurality of openings 210 arranged regularly and with good uniformity, and the plurality of openings 210 extend toward the outer surface 100 of the magnesium alloy object 1. The etching treatment in step S104 is used to form a plurality of pits 220 on the surface 200 of the anodized layer 2 away from the magnesium alloy object 1, and each pit 220 is correspondingly connected to at least one opening 210. The sealing treatment in step S106 is to cover the surface 200 of the anodized layer 2 with a sealing layer 3 to seal the plurality of openings 210.
[0029] Hereinafter, each step of the method for coloring the surface of a magnesium alloy article according to the present invention will be described in detail.
[0030] In step S100, the magnesium alloy object 1 can be formed by various methods, such as die casting, extrusion, forging and cutting, to have a shape required for practical application (such as a sheet shape) to serve as a housing, shield or machine. However, the present invention is not limited to the above examples.
[0031] In step S102, the anodizing treatment of the magnesium alloy object 1 is carried out in an electrolytic cell (not shown), and during the treatment process, the magnesium alloy object 1 is used as an anode and electrically connected to the positive electrode of the high-voltage power supply, and the cathode of the electrolytic cell (such as a stainless steel electrode) is electrically connected to the negative electrode of the high-voltage power supply. The electrolyte used for the anodizing treatment is an alkaline reagent, which may include an oxidant, a pH regulator and a film-forming agent, wherein the content of each component may be adjusted according to the performance requirements of the electrolyte. The oxidant may be selected from the group consisting of sodium nitrate, potassium nitrate, potassium permanganate and potassium dichromate, the pH regulator may be selected from the group consisting of sodium hydroxide, potassium hydroxide, lithium hydroxide and magnesium hydroxide, and the film-forming agent may be selected from the group consisting of sodium silicate, aluminum hydroxide, ammonium dihydrogen phosphate, sodium hexametaphosphate and trisodium phosphate. However, the present invention is not limited to the above examples.
[0032] Preferably, with Figure 3As shown, the anodizing treatment of step S102 is a pulsed anodizing treatment, which may include a voltage ramp-up stage M1 and a voltage constant voltage stage M2 following the voltage ramp-up stage M1, wherein the operating voltage of the voltage ramp-up stage M1 is increased from 0V to the target voltage Vt, and the operating voltage of the voltage constant voltage stage M2 is maintained at the target voltage Vt. Under such operation, the surface smoothness and density of the anodized layer 2 can be improved by controlling the nucleation rate, growth rate and dissolution rate of magnesium oxide, and the opening 210 is formed into a configuration that is conducive to improving light interference and dye absorption.
[0033] Further, the conditions of pulsed anodizing treatment include: an initial voltage of 0V and a target voltage of 20V to 600V, a pulse frequency of 500Hz to 2000Hz, and a duty cycle of 1% to 50%. In addition, the duration of the voltage ramp-up phase M1 is 1 minute to 10 minutes, and the duration of the voltage constant voltage phase M2 is 5 minutes to 60 minutes, which is more than four times the duration of the voltage ramp-up phase M1. It is worth mentioning that, compared with general anodizing treatment, the pulsed anodizing treatment adopted in the present invention is also conducive to reducing power consumption and improving production efficiency.
[0034] In an embodiment of the present invention, the target voltage of the pulsed anodizing treatment may be 20V, 50V, 100V, 150V, 200V, 250V, 300V, 350V, 400V, 450V, 500V, 550V or 600V; the pulse frequency may be 500Hz, 600Hz, 700Hz, 800Hz, 900Hz, 1000Hz, 1100Hz, 1200Hz, 1300Hz, 1400Hz, 1500Hz, 1600Hz, 1700Hz, 1800Hz, 1900Hz or 2000Hz; the duty cycle may be 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50%.
[0035] In addition Figure 2 As shown, the surface coloring method of the magnesium alloy object of the present invention may also include a pretreatment step, that is, the magnesium alloy object 1 is pretreated before anodizing (step S101) to remove defects, dirt, natural oxide film, etc. on its outer surface 100, or to obtain a special surface effect. The means of pretreatment vary with different purposes and may include degreasing, decarburization, alkali washing, acid washing, or any combination thereof. Alternatively, in order to obtain a special surface effect, the means of pretreatment may include polishing, sandblasting, or a combination of the two.
[0036] In step S104, the etching treatment is to use an etching liquid to etch a multi-level pit structure on the surface 200 of the anodized layer 2, and then wash and dry. It should be noted that the multi-level pit structure is composed of a plurality of pits 220 arranged in different forms, which is beneficial to improve the intensity of the interference color and the dyeing effect. The "different forms" mentioned here may refer to at least one of the pit diameter, pit depth, pit cross-sectional shape, pit volume, and pit surface area being significantly different. The etching liquid used for the etching treatment may be an aqueous solution containing nitric acid, sulfuric acid, phosphoric acid, oxalic acid, citric acid and / or their salts, and the duration of the etching treatment may be 10 seconds to 1200 seconds. However, the present invention is not limited to the examples given above.
[0037] In step S104, the sealing treatment is to cover the sealing layer 3 on the surface 200 of the anodized layer 2 by electro-deposition coating to seal the opening 210, wherein a portion of the sealing layer 3 is filled in the opening 210. The sealing layer 3 is formed by a resin composition, which includes an acrylic resin and a solid powder, and may further include a colorant as needed. The solid content of the resin composition is 3% to 30%, so that the requirements of gloss, hardness, weather resistance, etc. can be met. The solid powder can be a powder of a metal, a non-metal or its oxide; specific examples of solid powders include: powders of aluminum, gold, silver, iron, and powders of aluminum oxide, titanium oxide, silicon dioxide, iron oxide, and tin oxide. The implementation conditions of the electro-sealing include: an operating voltage of 1V to 150V, and a duration of 30 seconds to 10 minutes. In addition, the resin composition can be hardened by baking, and the baking conditions include: a baking temperature of 100°C to 200°C, and a baking time of 15 minutes to 60 minutes.
[0038] See also Figure 2 And cooperate Figure 4 and Figure 6 As shown, the surface coloring method of the magnesium alloy object of the present invention may also include a dyeing step, that is, the magnesium alloy object 1 is dyed before the sealing treatment (step S105) to change the appearance coloring effect of the magnesium alloy surface. The dyeing treatment can be a dyeing method (immersing the magnesium alloy object 1 in the dye 4) so that the dye 4 is attached to the magnesium alloy object 1 and has multiple openings 210 that at least partially penetrate the anodized layer 2, and after completion, it can be washed as needed to remove the dye 4 that is not adsorbed on the anodized layer 2. The dye 4 used for dyeing treatment may include organic pigments or inorganic pigments. It is worth mentioning that the present invention controls the distribution and configuration of multiple openings 210 through the set pulse voltage operation stage, including the voltage slow rise stage M1 and the voltage constant voltage stage M2, and cooperates with the bite treatment to form a multi-level pit structure (arranged by multiple pits 220 of different forms) above the multiple openings 210, which can achieve a deeper and more uniform dyeing effect.
[0039] The surface coloring method of the magnesium alloy article of the present invention will be further described in the following specific examples, but the specific examples are only used as examples and should not be construed as limiting the embodiments of the present invention.
[0040] Specific example 1
[0041] The AZ91D magnesium alloy object is immersed in an electrolyte with a pH of 10, and the electrolyte contains potassium permanganate (as an oxidant), potassium hydroxide (as a pH adjuster) and sodium silicate (as a film-forming agent). With the magnesium alloy object as the anode and the stainless steel as the cathode, pulse anodizing treatment is carried out under the following conditions: the target voltage of the voltage ramp phase is 300V, the frequency is 1000Hz, the duty cycle is 5%, the duration of the voltage ramp phase is 2 minutes, and the duration of the voltage constant phase is 10 minutes. After washing with water, the magnesium alloy object is immersed in a phosphoric acid aqueous solution for 100 seconds of etching treatment. After washing with water, the magnesium alloy object is first immersed in K080 dye (pH value controlled at 8) produced by Yongguang Chemical for dyeing treatment, and then the magnesium alloy object is used as the anode and the stainless steel is used as the cathode. The resin composition (total solid content is 10%) containing acrylic resin and alumina powder is used to seal the hole under the following conditions: the operating voltage is 20V and the duration is 1 minute. Then, the resin composition is hardened by baking at a temperature of 180° C. for 30 minutes. After completion, the magnesium alloy object can obtain a surface with a black appearance.
[0042] Specific example 2
[0043] The AZ31B magnesium alloy object is immersed in an electrolyte with a pH of 11, and the electrolyte contains sodium pernitrate (as an oxidant), sodium hydroxide (as a pH adjuster) and sodium hexametaphosphate (as a film-forming agent). With the magnesium alloy object as the anode and the carbon plate as the cathode, pulse anodizing treatment is carried out under the following conditions: the target voltage of the voltage ramp-up stage is 400V, the frequency is 1200Hz, the duty cycle is 7%, the duration of the voltage ramp-up stage is 1 minute, and the duration of the voltage constant stage is 5 minutes. After washing with water, the magnesium alloy object is immersed in an aqueous sulfuric acid solution for 50 seconds of etching treatment. After washing with water, the magnesium alloy object is first immersed in 503 dye produced by Aoye (pH value is controlled at 9) for dyeing treatment, and then with the magnesium alloy object as the anode and the stainless steel as the cathode, a resin composition containing acrylic resin and silver powder (total solid content is 13%) is used to seal the hole under the following conditions: the operating voltage is 30V and the duration is 30 seconds. Then, the resin composition is hardened by baking at a temperature of 160° C. for 60 minutes. After completion, the magnesium alloy article can obtain a surface with a blue appearance.
[0044] Specific example 3
[0045] The AM60B magnesium alloy object is immersed in an electrolyte with a pH of 12, and the electrolyte contains potassium pernitrate (as an oxidant), lithium hydroxide (as a pH adjuster) and trisodium phosphate (as a film-forming agent). With the magnesium alloy object as the anode and the carbon plate as the cathode, pulse anodizing treatment is carried out under the following conditions: the target voltage of the voltage ramp-up stage is 380V, the frequency is 800Hz, the duty cycle is 10%, the duration of the voltage ramp-up stage is 5 minutes, and the duration of the voltage constant stage is 20 minutes. After washing with water, the magnesium alloy object is immersed in a nitric acid aqueous solution for 30 seconds of erosion treatment. After washing with water, the magnesium alloy object is first immersed in 102 dye produced by Aoye (pH value is controlled at 10) for dyeing treatment, and then the magnesium alloy object is used as the anode and the stainless steel is used as the cathode. The resin composition (total solid content is 15%) containing acrylic resin and iron oxide powder is used to seal the hole under the following conditions: the operating voltage is 50V and the duration is 2 minutes. Then, the resin composition is hardened by baking at a temperature of 200° C. for 20 minutes. After completion, the magnesium alloy object can obtain a surface with a yellow-red appearance.
[0046] See also Figures 4 to 6 As shown, a surface colored magnesium alloy object Z can be obtained by using the surface coloring method of the magnesium alloy object of the present invention, which includes a magnesium alloy object 1, an anodized layer 2 and a sealing layer 3. The anodized layer 2 is formed on the outer surface 100 of the magnesium alloy object 1, and has a plurality of openings 210 extending toward the outer surface 100 of the magnesium alloy object 1. In addition, a plurality of pits 220 are formed on the surface 200 of the anodized layer 2 away from the magnesium alloy object 1, and each pit 220 is correspondingly connected to at least one opening 210. The sealing layer 3 covers the surface 200 of the anodized layer 2 to seal the plurality of openings 210. In an embodiment of the present invention, a dye 4 (a dye or a combination of multiple dyes) may or may not be present in the opening 210 to change the appearance coloring effect of the magnesium alloy surface.
[0047] Advantageous Effects of Embodiments
[0048] One of the beneficial effects of the present invention is that the surface coloring method of the magnesium alloy object of the present invention can improve the interference color intensity (the interference color is clear and noticeable) and the dyeing effect of the magnesium alloy surface through the combination of the technical features of "performing anodizing treatment on the magnesium alloy object to form an anodized layer on the outer surface of the magnesium alloy object, and the anodized layer has a plurality of openings extending toward the outer surface of the magnesium alloy object" and "performing a bite treatment on the anodized layer to form a plurality of pits on the surface of the anodized layer away from the magnesium alloy object, and each of the pits is connected to at least one of the openings", so as to improve the decorativeness of the magnesium alloy surface and change the appearance color effect of the magnesium alloy surface.
[0049] Furthermore, the anodic oxidation treatment used in the surface coloring method of the magnesium alloy object of the present invention is a pulsed anodic oxidation treatment, which may include a voltage ramp-up phase and a voltage constant voltage phase following the voltage ramp-up phase. Under such operation, the surface smoothness and compactness of the anodic oxide layer can be improved by controlling the nucleation rate, growth rate and dissolution rate of magnesium oxide, and the openings are formed into a configuration that is conducive to improving light interference and dye absorption. Moreover, compared with general anodic oxidation treatment, the anodic oxidation treatment of the present invention is also conducive to reducing power consumption and improving production efficiency.
[0050] Furthermore, the present invention controls the distribution and configuration of multiple openings through set pulse voltage operation stages, including a voltage ramp-up stage and a voltage constant stage, and cooperates with a bite-etching process to form a multi-level pit structure (composed of multiple pits of different forms arranged) above the multiple openings, which can achieve a darker and more uniform dyeing effect.
[0051] The contents disclosed above are only preferred feasible embodiments of the present invention, and are not intended to limit the protection scope of the claims of the present invention. Therefore, all equivalent technical changes made using the contents of the present invention description and drawings are included in the protection scope of the claims of the present invention.
Claims
1. A method for coloring the surface of a magnesium alloy object, characterized in that: The surface coloring method of the magnesium alloy object comprises: Provide magnesium alloy objects; Performing an anodizing treatment on the magnesium alloy object to form an anodized layer on the outer surface of the magnesium alloy object, wherein the anodized layer has a plurality of openings extending toward the outer surface of the magnesium alloy object; Performing etching treatment on the anodized layer, so that a plurality of pits are formed on the surface of the anodized layer away from the magnesium alloy object, and each of the pits is correspondingly connected to at least one of the openings; and The anodic oxide layer after being corroded is sealed.
2. The surface coloring method of a magnesium alloy object according to claim 1, characterized in that: The anodizing treatment is carried out in an electrolyte, and the electrolyte contains an oxidant, a pH regulator and a film-forming agent; the oxidant is selected from the group consisting of sodium nitrate, potassium nitrate, potassium permanganate and potassium dichromate, the pH regulator is selected from the group consisting of sodium hydroxide, potassium hydroxide, lithium hydroxide and magnesium hydroxide, and the film-forming agent is selected from the group consisting of sodium silicate, aluminum hydroxide, diammonium phosphate, sodium hexametaphosphate and trisodium phosphate.
3. The surface coloring method of a magnesium alloy object according to claim 1, characterized in that: The anodizing treatment is a pulsed anodizing treatment, which includes a voltage ramp-up phase and a voltage constant voltage phase following the voltage ramp-up phase. The operating voltage in the voltage ramp-up phase is increased from an initial voltage to a target voltage, and the operating voltage in the voltage constant voltage phase is maintained at the target voltage.
4. The method for surface coloring of a magnesium alloy object according to claim 3, characterized in that: The conditions for the pulsed anodizing treatment include: the initial voltage is 0V and the target voltage is 20V to 600V, the pulse frequency is 500Hz to 2000Hz, and the duty cycle is 1% to 50%; the duration of the voltage ramp-up phase is 1 minute to 10 minutes, and the duration of the voltage constant phase is 5 minutes to 60 minutes, which is more than four times the duration of the voltage ramp-up phase.
5. The surface coloring method of a magnesium alloy object according to claim 1, characterized in that: The etching treatment is to use an etching liquid to corrode the surface of the anodized layer. The etching liquid is an aqueous solution containing nitric acid, sulfuric acid, phosphoric acid, oxalic acid, citric acid and / or their salts, and the duration of the etching treatment is 10 seconds to 1200 seconds.
6. The method for surface coloring of a magnesium alloy object according to claim 1, characterized in that: Between the step of performing the etching treatment and the step of performing the sealing treatment, the method further includes: filling at least one dye into the plurality of openings of the anodized layer.
7. The method for surface coloring of a magnesium alloy object according to claim 1, characterized in that: The sealing treatment is to cover the surface of the anodized layer with a sealing layer by electric sealing to seal the plurality of open pores.
8. The surface coloring method of a magnesium alloy object according to claim 7, characterized in that: The sealing layer is formed by a resin composition, the resin composition comprises an acrylic resin and a solid powder, the solid powder is a powder of a metal, a non-metal or an oxide thereof, and the solid content of the resin composition is 3% to 30%; The implementation conditions of the electric sealing include: an operating voltage of 1V to 150V and a duration of 30 seconds to 10 minutes.
9. The method for surface coloring of a magnesium alloy object according to claim 8, characterized in that: The sealing treatment further comprises baking the resin composition under the following conditions: a baking temperature of 100° C. to 200° C. and a baking time of 15 minutes to 60 minutes.
10. A surface colored magnesium alloy object, characterized in that: The surface-colored magnesium alloy object comprises: Magnesium alloy articles; an anodized layer formed on the outer surface of the magnesium alloy object and having a plurality of openings extending toward the outer surface of the magnesium alloy object; wherein a plurality of pits are formed on the surface of the anodized layer away from the magnesium alloy object, and each of the pits is correspondingly connected to at least one of the openings; and A sealing layer covers the surface of the anodized layer to seal the plurality of openings.