3D fabric load-bearing structure node strength test method for parafoil manufacturing

Through multi-axial tensile test method and locking sewing technology, the tensile performance test problem of 3D fabric bearing structure under complex stress is solved, and the node strength test of 3D fabric bearing structure is realized to meet the strength of wing parachute manufacturing Requirements provide guidance for 3D structural testing of other materials.

CN118896836APending Publication Date: 2024-11-05BEIJING RES INST OF SPATIAL MECHANICAL & ELECTRICAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411006050.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The prior art lacks an effective test method for node strength testing of 3D fabric bearing structures, and it is difficult to test the tensile performance of 3D fabrics formed by integrated braiding under complex stresses. Especially in the manufacturing of wing parachutes, the 3D fabric bearing structure faces the extension of the wing surface. Complex failure of extended chord loads.

Method used

Using the multi-axial tensile test method, the 3D fabric load-bearing structure samples are cut and marked, the connecting tape is installed and the locking seam sewing is performed, and the lateral node strength test is carried out in combination with preloading and multi-axial tensile test machine is recorded and calculated. The fracture strength ensures the symmetrical installation and no deflection of the test samples, and realizes the tensile performance test of the 3D fabric bearing structure.

Benefits of technology

The tensile performance test of the 3D fabric bearing structure has been realized, which has expanded the fabric strength test from two-dimensional to three-dimensional, provided an effective method for wing parachute manufacturing, and provided reference for material testing of other similar structures, making up for Blanks in the calculation of 3D fabric break strength analysis in the prior art.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118896836A_ABST
    Figure CN118896836A_ABST
Patent Text Reader

Abstract

The invention discloses a 3D fabric force bearing structure node strength test method for parafoil manufacturing, and relates to the field of flexible textile material strength tests.The method comprises the following steps that a test material is prepared, and tailoring and sampling are conducted according to the design requirement of a test piece; manufacturing the 3D fabric force bearing structure into a node strength test sample piece; marking installation positioning lines on the test sample piece and the test equipment; the method comprises the following steps: mounting a test sample on a biaxial four-direction tensile testing machine; pre-loading after the test sample piece is installed; testing the node strength of the test sample, and recording the breaking strength of each transverse branch when the test sample is broken; determining the final breaking strength of the test sample, calculating the average breaking strength according to the final breaking strength, calculating the unit breaking strength according to the average breaking strength, and determining the validity of the test data; the invention makes up the vacancy of the prior art, provides the test method for detecting the transverse breaking strength of the 3D fabric force-bearing structure, and realizes the tensile property test of the 3D fabric force-bearing structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a strength test method for a node of an integrally woven 3D load-bearing structure used for manufacturing a parafoil, and belongs to the field of strength testing of flexible materials. Background Art

[0002] Scholars at home and abroad have conducted extensive research on the theory of fabric structural mechanics, mainly involving the stretching, tearing, shearing and bending of fabrics, especially the tensile properties of fabrics, which have been expanded from uniaxial to biaxial tensile properties.

[0003] Kawabata et al. studied the biaxial deformation theory of plain-weave fabrics in their article The Finite-deformation Theory of Plain-weave Fabrics Part 1: the BiaxialDeformation Theory published in Journal of the Textile Institute. They first calculated the biaxial force of the fabric structure through a model, and verified the theoretical calculation results of different fabrics through experiments. A biaxial stretching instrument was designed in the experiment. According to its experimental mechanism, this method is called the biaxial stretching experimental method with one direction fixed and the other direction stretched. Quaglin et al. used polyester plain-weave fabric as an orthotropic material in their article Experimental characterization of orthotropic technical Textiles under uniaxial and biaxial loading published in Composites: Part A. They analyzed the experimental characterization under uniaxial and biaxial loading by using the biaxial stretching method of a cross specimen with tension in two directions at the same time. In his graduation thesis on the test and research of bidirectional tensile properties of weft knitted fabrics, Hong Weiya from Donghua University in China studied the bidirectional tensile properties of different weft knitted fabrics. Bidirectional tensile tests with one direction fixed and the other direction tensile and bidirectional tensile tests with two directions tensile at the same time were carried out using a bidirectional electronic strength test machine. Although many test methods have been proposed for the study of the tensile properties of fabrics at home and abroad, they are all for conventional two-dimensional structural textiles or flat woven fabrics. There are few test methods for the tensile properties of one-piece woven 3D fabric load-bearing structures. One-piece woven 3D fabric load-bearing structures can be used to connect the upper and lower wing surfaces of the parafoil and the ribs. In actual use, they are subjected to loads in the span and chord directions along the wing surface and loads along the rib direction. They are often not subjected to a single form of damage, but to the combined action of complex stresses. Summary of the invention

[0004] The technical problem solved by the present invention is: to overcome the deficiencies of the prior art, to provide a 3D fabric load-bearing structure node strength test method for parafoil manufacturing, and to achieve tensile performance testing of the 3D fabric load-bearing structure.

[0005] The technical solution of the present invention is: a 3D fabric load-bearing structure node strength test method for parafoil manufacturing, comprising:

[0006] Cut and sample the 3D fabric load-bearing structure according to the required length of the test sample, and mark the center line of the sampled 3D fabric load-bearing structure in the length direction; cut and sample the connecting belt according to the required length of the test sample, and mark the center line of the sampled connecting belt in the width direction;

[0007] The sampled connecting belt is installed on the sampled 3D fabric load-bearing structure by lock-stitching to produce a test sample for node strength test;

[0008] Mark the installation positioning line on the test sample, and mark the installation position positioning line of the test sample on the test fixture of the multi-axial tensile testing machine with a marker pen; install the test sample on the multi-axial tensile testing machine according to the marked positioning line, and select the symmetrical direction for installation according to the structural form of the test sample during installation;

[0009] After the test specimen is installed, preload it and ensure that the test specimen is not skewed; after preloading, perform a transverse node strength test on the test specimen and record the transverse fracture strength F when the test specimen breaks. ij ;

[0010] Select the transverse rupture strength F of each test ij The minimum value minF in ij As the final breaking strength of the test sample in this test, the average breaking strength is calculated based on the selected final breaking strength. Calculate the unit breaking strength based on the average breaking strength obtained If the unit breaking strength obtained by the test It is not less than the design unit breaking strength of the 3D fabric load-bearing structure, indicating that the strength of the 3D fabric load-bearing structure obtained by this test method meets the requirements.

[0011] The structural form of the 3D fabric load-bearing structure is a cross-shaped belt or a T-shaped belt, and its transverse cross-sectional shape is a cross or a T-shaped belt; the cross-shaped belt has four transverse branches up, down, left, and right according to the transverse cross-sectional shape, and the T-shaped belt has three transverse branches down, left, and right according to the transverse cross-sectional shape.

[0012] The connecting belt is made of brocade ribbon, which is used as an auxiliary connecting belt to extend the length in the transverse direction during the transverse test of the 3D fabric load-bearing structure body. Its width is greater than Its strength is 2-3 times the strength of the 3D fabric load-bearing structure itself, where U is the cutting sampling length of the test specimen of the 3D fabric load-bearing structure.

[0013] The method of cutting and sampling the 3D fabric load-bearing structure according to the required length of the test sample includes: laying the 3D fabric load-bearing structure flat on the work surface, placing a weight 1m away from the end of the 3D fabric load-bearing structure, placing another weight at a distance of 1.5L, pressing the 3D fabric load-bearing structure to keep it naturally straight, marking the cutting sampling length L between the two weights with a steel ruler and marking the midpoint of the length L, cutting the sample with scissors and keeping the ends of the sample flush, and marking the center line of the width with a mark table after sampling.

[0014] Loosen the rolled connecting tape and let it stand in a natural state for 24 hours to release stress. Spread it flat on the work surface, place a weight 1m away from the end of the connecting tape, and place another weight at a distance of 1.5V to press the connecting tape to keep it naturally straight. Mark the cutting sampling length V with a steel ruler between the two weights. Use scissors to cut the sample and keep the ends of the sample flush. After sampling, use a mark table to mark the center line of the width.

[0015] The sampled connecting belt is installed on the sampled 3D fabric load-bearing structure, and the installation form adopts the lock-sewing form to produce a test sample for node strength test, including: the X-belt sample is installed in four lateral branch directions, and the T-belt sample is installed in three lateral branch directions; the structural form of the installation of the lateral branch of the 3D fabric load-bearing structure sample and the connecting belt is lock-sewing, the sewing seam width is 15 to 30 cm, and the sewing form is two rows of straight stitches, and the stitches are sewn from one end of the 3D fabric load-bearing structure sample in the L direction to the other end; after the connecting belt is installed on the 3D fabric load-bearing structure sample, ensure that the center line of the marked connecting belt in the width direction is flush with the center line of the 3D fabric load-bearing structure in the L direction, and the center lines of the connecting belts on the two lateral branches in the symmetrical direction of the 3D fabric load-bearing structure are flush; strengthen the sewing at the overlapping position of the 3D fabric load-bearing structure sample and the connecting belt lock-sewing, the sewing form is a rectangular diagonal seam, the sewing length is S and is less than the width of the connecting belt.

[0016] The installation positioning line on the test sample is marked on the connecting belt on the transverse branch, and the distance from the center point of the test sample is not less than The installation position positioning line on the multi-axial tensile testing machine is marked at the center of the test fixture.

[0017] The method of installing the test sample on the multi-axial tensile testing machine according to the marked positioning lines includes: during installation, the X-belt sample is installed on the testing machine in the order of up and down or left and right symmetry of the transverse cross-sectional shape, and the T-belt is installed on the testing machine in the order of first installing the left and right direction and then installing the downward direction according to the transverse cross-sectional shape, the positioning lines on the connecting belts on each transverse branch of the test sample are flush with the clamping openings of the test fixture on each axis of the testing machine, and the center line of the connecting belt in the width direction is flush with the center line of the test clamp, ensuring that the center position of the sample is at the same distance from the clamping openings of the test fixture on each axis of the testing machine; after installation, the L direction of the test sample is in a vertical state.

[0018] After the test sample is installed, it is preloaded with a preload value of 30 to 50N. The four transverse branches of the X-belt sample are loaded simultaneously, the two symmetrical transverse branches of the T-belt sample are loaded, and the single transverse branch in the lower direction is not loaded. After the loading is completed, a visual inspection is performed to confirm that the test sample has no deflection, the heights of the transverse branches of the sample are in the same horizontal plane, and the symmetrical transverse branches on both sides of the sample are in a straight line.

[0019] The node strength test of the test sample is carried out, and the transverse fracture strength F of each branch when the test sample breaks is recorded. ij ,include:

[0020] The four transverse branch directions of the ten-type belt test specimen are loaded and stretched simultaneously until the test specimen breaks, and the breaking strength value F in each transverse branch direction is recorded. ij ;

[0021] The two symmetrical transverse branches of the T-belt test specimen remain stationary, and the single branch in the downward direction is loaded and stretched until the test specimen breaks, and the breaking strength value F in each transverse branch direction is recorded. ij ;

[0022] Where i is the number of tests, j is the number of transverse branches of the 3D fabric load-bearing structure, j=1 to 4 for the ten-type belt samples, and j=1 to 3 for the T-type belt samples.

[0023] The final breaking strength is the transverse breaking strength F of each branch in each test. ij The minimum value among the tests, n tests have n final breaking strengths; sum up all the final breaking strengths and divide by the total number of tests to calculate the average breaking strength

[0024] Unit breaking strength The calculation process is: the average breaking strength is divided by the sewing length S of the reinforced sewing at the overlapping position of the 3D fabric load-bearing structure sample and the connecting tape lock seam, and then multiplied by the converted length of the unit breaking strength.

[0025] The advantages of the present invention compared with the prior art are:

[0026] (1) The present invention proposes a node strength tensile test method for 3D fabric load-bearing structures. At present, fabric strength tests usually adopt bidirectional stretching in which one direction is fixed and the other direction is tensile, or a planar bidirectional stretching test method in which forces are applied in two directions perpendicular to each other in the plane of the sample, but all of them are for two-dimensional fabric structural materials. The present invention adopts a test method of multi-directional stretching in which two directions are fixed and one direction is tensile, and a test method of bidirectional simultaneous stretching in which two directions are fixed in two directions in the 3D space of the sample for T-shaped and cross-shaped 3D fabric load-bearing structures, respectively. At the same time, a pre-loading method of fixing one direction and symmetrically loading in two directions is adopted for T-shaped 3D fabric load-bearing structures, so as to expand the fabric strength tensile test from two-dimensional fabric structures to three-dimensional fabric structures, and realize the tensile mechanical test of 3D fabric load-bearing structures, which can provide reference for mechanical property testing of other non-textile materials with similar structures, such as films, rubbers and composite materials;

[0027] (2) The present invention proposes a method for making test specimens of 3D fabric load-bearing structures. At present, specimens for testing the strength of fabric seams are usually made by fixed sewing technology, but the test specimens are basically two-dimensional structures. The present invention proposes a method for installing a connecting belt by sewing technology using two rows of straight lines + rectangular diagonal seams to make a 3D test specimen for a 3D fabric load-bearing structure that is woven into one piece. The two rows of straight lines are sewn from one end of the 3D fabric load-bearing structure specimen in the L direction to the other end. The rectangular diagonal seams are sewn at the overlapping position of the 3D fabric load-bearing structure specimen and the connecting belt, and the sewing length is less than the width of the connecting belt, so as to achieve a tensile test of the transverse breaking strength of the 3D fabric load-bearing structure. This can provide guidance for the production of 3D structure specimens made of other materials.

[0028] (3) The present invention proposes a method for calculating the breaking strength of a 3D fabric load-bearing structure test specimen. Currently, fabric structures usually use the warp and weft breaking strength directly obtained by uniaxial biaxial or biaxial biaxial stretching to confirm the tensile properties of the fabric. The present invention proposes the minimum breaking strength of each test as the final breaking strength for the tensile test performance of the 3D fabric load-bearing structure test specimen, calculates the average breaking strength by the final breaking strength, and then calculates the unit breaking strength by the average breaking strength. This method realizes the performance analysis of multi-directional tensile damage of 3D fabric load-bearing structures, filling the gap of the current lack of a breaking strength analysis and calculation method for 3D fabric load-bearing structures. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the load-bearing structure of type ten 3D fabric;

[0030] Figure 2 It is a schematic diagram of the T-shaped 3D fabric load-bearing structure;

[0031] Figure 3 It is a type 10 3D fabric load-bearing structure test specimen;

[0032] Figure 4 It is a T-shaped 3D fabric load-bearing structure test specimen;

[0033] Figure 5 It is a stitching and sewing form of the horizontal branches and connecting belts of the 3D fabric load-bearing structure;

[0034] Figure 6 Schematic diagram of the loading process of the Type 10 3D fabric load-bearing structure test specimen;

[0035] Figure 7 Schematic diagram of the loading process of the T-shaped 3D fabric load-bearing structure test specimen. DETAILED DESCRIPTION

[0036] The node strength test object of the present invention uses a 3D fabric load-bearing structure, the structural form of which is a flexible textile material integrally woven and formed, including two types of cross-shaped belts 1 and T-shaped belts 2, the design standard unit breaking strength is not less than 3000N / 50mm, the weight is ≤60.0g / m, wherein the width of the cross-shaped belt material is 100mmX100mm, and the width of the T-shaped belt material is 100mmX50mm;

[0037] A 3D fabric load-bearing structure node strength test method for parafoil manufacturing, the steps are as follows:

[0038] (1) Prepare the materials of 3D fabric load-bearing structure and connecting belt 3, cut and sample the 3D fabric load-bearing structure according to the required length of the test sample, and mark the center line of the sampled 3D fabric load-bearing structure in the length direction; cut and sample the connecting belt according to the required length of the test sample, and mark the center line of the sampled connecting belt in the width direction;

[0039] (2) Install the sampled connecting belt onto the sampled 3D fabric load-bearing structure by lock-stitching to produce a test sample for node strength test;

[0040] (3) Mark the installation positioning line on the test specimen and mark the test specimen installation position positioning line on the test fixture of the multi-axial tensile testing machine;

[0041] (4) Install the test specimen on the multi-axial tensile testing machine according to the marked positioning lines, and select the symmetrical direction according to the structural form of the test specimen during installation;

[0042] (5) After the test specimen is installed, preload it and ensure that the test specimen is not deflected;

[0043] (6) Carry out the node strength test of the test specimen and record the transverse fracture strength F of each axis of the testing machine when the test specimen breaks. ij ;

[0044] (7) Select the transverse rupture strength F of each test ij The minimum value min F ij As the final breaking strength of the test sample in this test, the average breaking strength is calculated based on the selected final breaking strength. Calculate the unit breaking strength based on the average breaking strength obtained

[0045] In the step (1), the structural form of the 3D fabric load-bearing structure is a cross-shaped belt or a T-shaped belt, and its transverse cross-sectional shape is a cross or a T-shaped belt. The cross-sectional shape of the cross-shaped belt has four transverse branches, and the T-shaped belt has three transverse branches. The material of the connecting belt is a brocade belt, which is used as an auxiliary connecting belt to extend the transverse length of the 3D fabric load-bearing structure body during the transverse test. The width is greater than Its strength is 2-3 times that of the 3D fabric load-bearing structure itself.

[0046] The cutting and sampling specifically includes laying the 3D fabric load-bearing structure flat on the work surface, placing a 2-5kg weight at a position 1m from the end of the fabric, placing another weight at a distance of 1.5-5L, pressing the fabric to keep it naturally straight, marking the cutting sampling length L between the two weights with a steel ruler and marking the midpoint of the length L, cutting the sample with scissors and keeping the ends of the sample flush; loosening the rolled connecting belt and letting it stand in a natural state for 24 hours to release stress, laying it flat on the work surface, placing a 2-5kg weight at a position 1m from the end of the belt, placing another weight at a distance of 1.5-5V, pressing the connecting belt to keep it naturally straight, marking the cutting sampling length V between the two weights with a steel ruler, cutting the sample with scissors and keeping the ends of the sample flush, and marking the center line of the width with a mark table after sampling.

[0047] In the step (2), the sampled connecting belt is installed on the sampled 3D fabric load-bearing structure sample to produce a test sample, which specifically includes: the X-belt sample is installed in four lateral branch directions, and the T-belt sample is installed in three lateral branch directions. The structural type of the lateral branches of the 3D fabric load-bearing structure sample and the connecting belt is lock stitching, the sewing seam width is 15 to 30 cm, and the sewing form is two rows of straight stitches, and the stitches are sewn from one end of the 3D fabric load-bearing structure sample in the L direction to the other end. After the connecting belt is installed on the 3D fabric load-bearing structure sample, ensure that the center line of the marked connecting belt in the width direction is flush with the center line of the 3D fabric load-bearing structure in the L direction, and the center lines of the connecting belts on the two lateral branches in the symmetrical direction of the 3D fabric load-bearing structure are flush; strengthen the sewing at the overlapping position of the 3D fabric load-bearing structure sample and the connecting belt lock stitching, and the sewing form is a rectangular diagonal seam, and the sewing length is S and is less than the width of the connecting belt.

[0048] In step (3), the installation positioning line on the test sample is marked on the connecting strip on the transverse branch, and the distance from the center point of the test sample is not less than The mounting position positioning line on the multi-axial tensile testing machine is marked in the center of the test fixture.

[0049] In the step (4), the test sample is installed on the multi-axial tensile testing machine according to the marked positioning lines, specifically including: during installation, the X-belt sample is installed on the testing machine in the order of the up-down or left-right symmetric direction of the transverse cross-sectional shape, and the T-belt is installed on the testing machine in the order of the left-right direction first and the down direction after the transverse cross-sectional shape, the positioning lines on the connecting belts on each transverse branch of the test sample are flush with the clamping openings of the test fixtures on each axis of the testing machine, and the center line of the connecting belt in the width direction is flush with the center line of the test clamp, ensuring that the center position of the sample is at the same distance from the clamping openings of the test fixtures on each axis of the testing machine; after installation, the L direction of the test sample is in a vertical state.

[0050] In the step (5), the preload value of the test sample is 30 to 50N, the four transverse branches of the X-belt sample are loaded simultaneously, the two symmetrical transverse branches of the T-belt sample are loaded, and the single transverse branch in the downward direction is not loaded. After loading is completed, it is confirmed by visual inspection that the test sample has no deflection, the heights of the transverse branches of the sample are in the same horizontal plane, and the symmetrical transverse branches on both sides of the sample are in a straight line.

[0051] In the step (6), the four transverse branch directions of the ten-shaped belt test sample are loaded and stretched simultaneously until the test sample breaks, and the breaking strength value F in each transverse branch direction is recorded. ij The two symmetrical transverse branches of the T-belt test specimen remain stationary, and the single branch in the downward direction is loaded and stretched until the test specimen breaks, and the breaking strength value F of each transverse branch direction is recorded. ij ; Where i is the number of tests, j is the number of transverse branches of the 3D fabric load-bearing structure, j=4 for the ten-type belt sample, and j=3 for the T-type belt sample.

[0052] In the above-mentioned 3D fabric load-bearing structure node strength test method for parafoil manufacturing, in the step (6), the failure form of the test sample is observed. When the 3D fabric load-bearing structure body is destroyed, the fabric test requirements are met and the valid data is retained. When the test sample breaks at the clamp or slips during the test, the fabric test requirements are not met and the invalid data is discarded.

[0053] In step (7), the final breaking strength is the transverse breaking strength F of each branch in each test. ij The minimum value among the tests, n tests have n final breaking strengths; sum up all the final breaking strengths and divide by the total number of tests to calculate the average breaking strength

[0054] In step (7), the unit breaking strength is calculated by dividing the average breaking strength by the sewing length S of the overlapping position of the 3D fabric load-bearing structure sample and the connecting belt lock seam and then multiplying it by the converted length of the unit breaking strength.

[0055] So far, the unit breaking strength obtained from the test is not less than the designed unit breaking strength of the 3D fabric load-bearing structure, indicating that the strength data of the 3D fabric load-bearing structure obtained by this test method meets the requirements and the test method is feasible.

[0056] The present invention is further described in detail below in conjunction with specific embodiments.

[0057] A 3D fabric load-bearing structure node strength test method for parafoil manufacturing, the method specifically comprises the following steps:

[0058] Step (a), such as Figure 1 , 2 As shown, prepare the test materials 3D fabric load-bearing structure cross-belt and T-belt and 43-800A brocade ribbon. Before cutting, the rolled connecting belt is loosened and left to stand for 24 hours in a natural state to release stress. Sampling starts at a position 1000mm away from the end of the 3D fabric load-bearing structure. The fabric is naturally laid flat and two rollers are placed at an interval of 200mm. A steel ruler is used to mark the sampling length of 100mm and the ribbon is cut with scissors. The number of samples of the cross-belt fabric structure is 5, and the number of samples of the T-belt fabric structure is 5; sampling of the 43-800A brocade ribbon starts at a position 1000mm away. The fabric is naturally laid flat and two rollers are placed at an interval of 600mm. A steel ruler is used to mark the sampling length of 350mm and the ribbon is cut with scissors. The number of cuts is 40; the midpoint of the length direction is marked with a marker pen on the 3D fabric load-bearing structure, and the center line of the width is marked with a marker pen on the 43-800A brocade ribbon;

[0059] Step (ii), Step (iii), sew and install the 43-800A brocade ribbon to the horizontal branch of the 3D fabric load-bearing structure sample, and install the ten-type ribbon sample in four directions, such as Figure 3 As shown; T-belt samples are installed in three directions, such as Figure 4 Specifically, the 3D fabric load-bearing structure sample and the 43-800A brocade ribbon are sewn in a lock stitching manner, with a seam width of 20 mm, and two rows of straight lines are sewn from one end of the 3D fabric load-bearing structure sample in the L direction to the other end, and the 43-800A brocade ribbon is fixed on the sample, and the sewing is strengthened at the overlap position of the two. The sewing form is a rectangular diagonal seam, and the sewing length S = 35 mm, as shown in FIG. Figure 5 As shown. The sewing thread is K9# Jinsi thread, and the stitch density is Needle / 100mm; When the 43-800A brocade ribbon is installed on the 3D fabric load-bearing structure, the marked center line of the 43-800A brocade ribbon is aligned with the midpoint of the 3D fabric load-bearing structure, and the center lines of the 43-800A brocade ribbons on both sides of the symmetrical 3D fabric load-bearing structure are flush.

[0060] Step (iv), mark the length installation positioning line with a marker pen on the connecting belt of the transverse branch 225mm away from the center of the test sample, and mark the installation position positioning line at the center position of the test fixture on the multi-axial tensile testing machine. During installation, the X-belt sample is installed on the testing machine in the order of the up-down or left-right symmetry of the transverse cross-sectional shape, and the T-belt is installed on the testing machine in the order of the left-right direction first and the down direction after the transverse cross-sectional shape. The length positioning line on the connecting belt of the test sample is flush with the test fixture clamp on each axis of the testing machine, and the center line of the width direction of the connecting belt is flush with the center line of the test clamp, ensuring that the distance between the center position of the sample and the test fixture clamp on each axis of the testing machine is the same; after installation, the L direction of the test sample is in a vertical state.

[0061] Step (V): After the test specimen is installed, it is preloaded with a loading force of 50N. The four transverse branches of the X-belt specimen are loaded simultaneously, the two symmetrical transverse branches of the T-belt specimen are loaded, and the single branch in the lower direction is not loaded. After the loading is completed, a visual inspection is performed to confirm that the test specimen has no deflection, the heights of the transverse branches of the specimen are in the same horizontal plane, and the symmetrical transverse branches on both sides of the specimen are in a straight line.

[0062] Step (VI): After the preload is confirmed, a strength test is performed. The ten-type belt test specimen is loaded and stretched simultaneously in the four transverse branch directions. Figure 6 As shown, until the test specimen breaks, record the breaking strength value of each transverse branch direction. The first test of the four transverse branches is F 11 、F 12 、F 13 、F 14 , the minimum force value among the four force values ​​is selected as the final breaking strength of the first test of the 3D fabric load-bearing structure test specimen, and the remaining four tests are carried out in the same way to confirm the final breaking strength; the two symmetrical horizontal branches of the T-belt test specimen remain stationary, and the single branch in the lower direction is loaded and stretched, Figure 7 As shown, until the test sample breaks, the final breaking strength of the T-belt test sample after five tests is confirmed according to the final breaking strength selection method of the ten-type belt test sample;

[0063] Step (VII): After selecting and confirming the final breaking strength of the 3D fabric load-bearing structure test sample according to the breaking strength obtained in step (VI), calculate the average breaking strength Then divide the average breaking strength by the sewing length S of the overlapped position of the 3D fabric load-bearing structure sample and the connecting belt lock seam, and then multiply it by the converted length of the unit breaking strength to get the unit breaking strength. Select the conversion length as 50mm.

[0064] Finally, the average transverse breaking strength of the cross-shaped 3D fabric load-bearing structure after five tests is The unit breaking strength is The unit breaking strength is greater than the design requirement of 3000N / 50mm, and the data is valid; the average transverse breaking strength of the T-shaped 3D fabric load-bearing structure after five tests is The unit breaking strength is The unit breaking strength is greater than the design requirement of 3000N / 50mm, and the data is valid. The strength of the 3D fabric bearing structure obtained by this test method meets the requirements, and the test method is feasible.

[0065] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Any person skilled in the art can make possible changes and modifications to the technical solution of the present invention by using the technical contents disclosed above without departing from the spirit and scope of the present invention. Therefore, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention shall fall within the protection scope of the technical solution of the present invention.

Claims

1. A 3D fabric load-bearing structure node strength test method for parafoil manufacturing, characterized in that: include: Cut and sample the 3D fabric load-bearing structure according to the required length of the test sample, and mark the center line of the sampled 3D fabric load-bearing structure in the length direction; cut and sample the connecting belt according to the required length of the test sample, and mark the center line of the sampled connecting belt in the width direction; The sampled connecting belt is installed on the sampled 3D fabric load-bearing structure by lock-stitching to produce a test sample for node strength test; Mark the installation positioning line on the test sample, and mark the test sample installation position positioning line on the test fixture of the multi-axial tensile testing machine; install the test sample on the multi-axial tensile testing machine according to the marked positioning line, and select the symmetrical direction for installation according to the structural form of the test sample during installation; After the test specimen is installed, preload it and ensure that the test specimen is not skewed; after preloading, perform a transverse node strength test on the test specimen and record the transverse fracture strength F when the test specimen breaks. ij ; Select the transverse rupture strength F of each test ij The minimum value minF in ij The final breaking strength of the test specimen is used as the final breaking strength of the test. The average breaking strength is calculated based on the selected final breaking strength. Calculate the unit breaking strength based on the average breaking strength obtained If the unit breaking strength obtained by the test It is not less than the design unit breaking strength of the 3D fabric load-bearing structure, indicating that the strength of the 3D fabric load-bearing structure obtained by this test method meets the requirements.

2. A 3D fabric load-bearing structure node strength test method for parafoil manufacturing according to claim 1, characterized in that: The structural form of the 3D fabric load-bearing structure is a cross-shaped belt or a T-shaped belt, and its transverse cross-sectional shape is a cross or a T-shaped belt; the cross-shaped belt has four transverse branches up, down, left, and right according to the transverse cross-sectional shape, and the T-shaped belt has three transverse branches down, left, and right according to the transverse cross-sectional shape.

3. A 3D fabric load-bearing structure node strength test method for parafoil manufacturing according to claim 2, characterized in that: The connecting belt is made of brocade ribbon, which is used as an auxiliary connecting belt to extend the length in the transverse direction during the transverse test of the 3D fabric load-bearing structure body. Its width is greater than Its strength is 2-3 times the strength of the 3D fabric load-bearing structure itself, where U is the cutting sampling length of the test specimen of the 3D fabric load-bearing structure.

4. A 3D fabric load-bearing structure node strength test method for parafoil manufacturing according to claim 3, characterized in that: The method of cutting and sampling the 3D fabric load-bearing structure according to the required length of the test sample includes: laying the 3D fabric load-bearing structure flat on the work surface, placing a weight 1m away from the end of the 3D fabric load-bearing structure, placing another weight at a distance of 1.5L, pressing the 3D fabric load-bearing structure to keep it naturally straight, marking the cutting sampling length L between the two weights with a steel ruler and marking the midpoint of the length L, cutting the sample with scissors and keeping the ends of the sample flush, and marking the center line of the width with a mark table after sampling.

5. A 3D fabric load-bearing structure node strength test method for parafoil manufacturing according to claim 4, characterized in that: Loosen the rolled connecting tape and let it stand in a natural state for 24 hours to release stress. Spread it flat on the work surface, place a weight 1m away from the end of the connecting tape, and place another weight at a distance of 1.5V to press the connecting tape to keep it naturally straight. Mark the cutting sampling length V with a steel ruler between the two weights. Use scissors to cut the sample and keep the ends of the sample flush. After sampling, use a mark table to mark the center line of the width.

6. A 3D fabric load-bearing structure node strength test method for parafoil manufacturing according to claim 5, characterized in that: The sampled connecting belt is installed on the sampled 3D fabric load-bearing structure, and the installation form adopts the lock-sewing form to produce a test sample for node strength test, including: the X-belt sample is installed in four lateral branch directions, and the T-belt sample is installed in three lateral branch directions; the structural form of the installation of the lateral branch of the 3D fabric load-bearing structure sample and the connecting belt is lock-sewing, the sewing seam width is 15 to 30 cm, and the sewing form is two rows of straight stitches, and the stitches are sewn from one end of the 3D fabric load-bearing structure sample in the L direction to the other end; after the connecting belt is installed on the 3D fabric load-bearing structure sample, ensure that the center line of the marked connecting belt in the width direction is flush with the center line of the 3D fabric load-bearing structure in the L direction, and the center lines of the connecting belts on the two lateral branches in the symmetrical direction of the 3D fabric load-bearing structure are flush; strengthen the sewing at the overlapping position of the 3D fabric load-bearing structure sample and the connecting belt lock-sewing, the sewing form is a rectangular diagonal seam, the sewing length is S and is less than the width of the connecting belt.

7. A 3D fabric load-bearing structure node strength test method for parafoil manufacturing according to claim 5, characterized in that: The installation positioning line on the test sample is marked on the connecting belt on the transverse branch, and the distance from the center point of the test sample is not less than The installation position positioning line on the multi-axial tensile testing machine is marked at the center of the test fixture.

8. A 3D fabric load-bearing structure node strength test method for parafoil manufacturing according to claim 5, characterized in that: The method of installing the test sample on the multi-axial tensile testing machine according to the marked positioning lines includes: during installation, the X-belt sample is installed on the testing machine in the order of up and down or left and right symmetry of the transverse cross-sectional shape, and the T-belt is installed on the testing machine in the order of first installing the left and right direction and then installing the downward direction according to the transverse cross-sectional shape, the positioning lines on the connecting belts on each transverse branch of the test sample are flush with the clamping openings of the test fixture on each axis of the testing machine, and the center line of the connecting belt in the width direction is flush with the center line of the test clamp, ensuring that the center position of the sample is at the same distance from the clamping openings of the test fixture on each axis of the testing machine; after installation, the L direction of the test sample is in a vertical state.

9. A 3D fabric load-bearing structure node strength test method for parafoil manufacturing according to claim 8, characterized in that: After the test sample is installed, it is preloaded with a preload value of 30 to 50N. The four transverse branches of the X-belt sample are loaded simultaneously, the two symmetrical transverse branches of the T-belt sample are loaded, and the single transverse branch in the lower direction is not loaded. After the loading is completed, a visual inspection is performed to confirm that the test sample has no deflection, the heights of the transverse branches of the sample are in the same horizontal plane, and the symmetrical transverse branches on both sides of the sample are in a straight line.

10. A 3D fabric load-bearing structure node strength test method for parafoil manufacturing according to claim 9, characterized in that: The node strength test of the test sample is carried out, and the transverse fracture strength F of each branch when the test sample breaks is recorded. ij ,include: The four transverse branch directions of the ten-type belt test specimen are loaded and stretched simultaneously until the test specimen breaks, and the breaking strength value F in each transverse branch direction is recorded. ij ; The two symmetrical transverse branches of the T-belt test specimen remain stationary, and the single branch in the downward direction is loaded and stretched until the test specimen breaks, and the breaking strength value F in each transverse branch direction is recorded. ij ; Where i is the number of tests, j is the number of transverse branches of the 3D fabric load-bearing structure, j=1 to 4 for the ten-type belt samples, and j=1 to 3 for the T-type belt samples.

11. A 3D fabric load-bearing structure node strength test method for parafoil manufacturing according to claim 1, characterized in that: The final breaking strength is the transverse breaking strength F of each branch in each test. ij The minimum value among the tests, n tests have n final breaking strengths; sum up all the final breaking strengths and divide by the total number of tests to calculate the average breaking strength 12. A 3D fabric load-bearing structure node strength test method for parafoil manufacturing according to claim 1, characterized in that: Unit breaking strength The calculation process is: the average breaking strength is divided by the sewing length S of the reinforced sewing at the overlapping position of the 3D fabric load-bearing structure sample and the connecting tape lock seam, and then multiplied by the converted length of the unit breaking strength.