Hard coating film
By using a combination of polyimide film and a hard coating of a specific thickness, the problems of bending marks and interference fringes in flexible displays during repeated bending were solved, achieving high bending resistance and scratch resistance, and improving the appearance and visibility of the display.
Patent Information
- Application Number
- CN202410960274.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2016-08-23
- Publication Date
- 2024-11-05
AI Technical Summary
Existing hard coatings are prone to bending marks and whitening when repeatedly bent in flexible displays, resulting in a deterioration in appearance and the appearance of interference fringes, which affects visibility.
A polyimide film is used as the substrate film, and a hard coating with a thickness of 0.5μm to 10μm is laminated on it. The refractive index difference between the hard coating and the substrate film is controlled to be below 0.04. The hard coating is formed by using a composition containing active energy ray curable components and transition metal oxide particles, which ensures the bending resistance and scratch resistance of the hard coating.
It improves the bending and scratch resistance of the hard coating, reduces the generation of interference fringes, and maintains the appearance quality and visibility of the display.
Smart Images

Figure CN118897344A_ABST
Abstract
Description
[0001] The present invention is a divisional application of the Chinese patent application with application number 201680088557.2, application date August 23, 2016, and invention name “Hard Coating Film”. Technical Field
[0002] The present invention relates to a hard coating film having a substrate film and a hard coating layer, and in particular to a hard coating film suitable for use in a flexible display. Background Art
[0003] Various electronic devices widely use various displays such as liquid crystal displays (LCDs), organic EL displays (OELDs), and touch panels. In order to prevent damage, a hard coating film having a hard coating layer on a base film is often provided on the surface of these various displays.
[0004] However, in recent years, as the above-mentioned display, a display that can be bent, that is, a so-called flexible display, has been developed. Flexible displays are expected to have a wide range of uses, for example, as a stationary display that is bent to be set in a cylindrical column, or as a mobile display that can be folded or rolled up to be transported. As a hard coating film for a flexible display, a hard coating film disclosed in Patent Documents 1 and 2 is proposed.
[0005] Here, the flexible display is not formed into a curved surface only once, but may be bent (folded) repeatedly as described in Patent Document 3.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent No. 5468167
[0009] Patent Document 2: Japanese Patent Application Publication No. 2015-69197
[0010] Patent Document 3: Japanese Patent Application Publication No. 2016-2764 Summary of the invention
[0011] 1. Technical issues to be resolved
[0012] However, when conventional hard coat films are used in flexible displays for the above-mentioned applications, bending marks or whitening occur at portions that are repeatedly bent, which deteriorates the appearance and reduces visibility as a display.
[0013] On the other hand, interference fringes may be generated on the hard coating film due to various reasons. When interference fringes are generated on the hard coating film, the appearance is deteriorated and the visibility as a display is reduced.
[0014] The present invention has been made in view of the above-mentioned actual situation, and an object of the present invention is to provide a hard coating film which has bending resistance capable of withstanding repeated bending and is less likely to generate interference fringes.
[0015] (II) Technical solution
[0016] In order to achieve the above-mentioned purpose, first, the present invention provides a hard coating film, which comprises a substrate film and a hard coating layer stacked on at least one main surface side of the substrate film, characterized in that the substrate film is a polyimide film, the difference between the refractive index of the polyimide film and the refractive index of the hard coating layer is less than 0.04 in absolute value, and the thickness of the hard coating layer is greater than 0.5 μm and less than 10 μm (Invention 1).
[0017] The hard coat film of the invention (Invention 1) has excellent bending resistance and scratch resistance by making the base film a polyimide film and making the thickness of the hard coat layer within the above range. In addition, the hard coat film is less likely to generate interference fringes by making the refractive index difference within the above range.
[0018] In the above invention (Invention 1), the refractive index of the hard coat layer is preferably 1.40 or more and 1.85 or less (Invention 2).
[0019] In the above inventions (Inventions 1 and 2), it is preferred that the thickness of the polyimide film is 5 μm or more and 300 μm or less (Invention 3).
[0020] In the above inventions (Inventions 1 to 3), it is preferred that the hard coat layer is formed of a material obtained by curing a composition containing an active energy ray-curable component and transition metal oxide fine particles (Invention 4).
[0021] The hard coat film of the above invention (Inventions 1 to 4) is preferably used as a flexible member constituting a flexible display (Invention 5).
[0022] In the above inventions (Inventions 1 to 5), it is preferable that an adhesive layer is laminated on at least one main surface side of the base film (Invention 6).
[0023] (III) Beneficial effects
[0024] The hard coating film of the present invention has bending resistance capable of withstanding repeated bending and is less likely to generate interference fringes. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a cross-sectional view of a hard coating film according to one embodiment of the present invention.
[0026] Figure 2 This is a cross-sectional view of a hard coating film according to another embodiment of the present invention.
[0027] Figure 3 This is a cross-sectional view of a hard coating film according to still another embodiment of the present invention.
[0028] Description of Reference Numerals
[0029] 1, 1A, 1B: hard coating film; 2: substrate film; 3: hard coating layer; 4: second hard coating layer; 5: adhesive layer. DETAILED DESCRIPTION
[0030] Hereinafter, embodiments of the present invention will be described.
[0031] Figure 1 1 is a cross-sectional view of a hard coating film according to an embodiment of the present invention. The hard coating film 1 of this embodiment comprises a substrate film 2 and a laminated substrate film on one main surface side ( Figure 1 It is composed of a hard coating layer 3 on the upper side of the body.
[0032] In the hard coating film 1, the base film 2 is a polyimide film. When the base film 2 is a polyimide film, when the hard coating film 1 is applied to a flexible display and repeatedly bent, the base film 2 can be prevented from having bending marks or whitening, and the bending resistance is excellent. Therefore, when the flexible display using the hard coating film 1 of the present embodiment is repeatedly bent at a predetermined portion, the appearance deterioration or visibility reduction at the bent portion can be prevented.
[0033] In addition, the difference between the refractive index of the polyimide film and the refractive index of the hard coating layer 3 is 0.04 or less in absolute value. In the hard coating film 1 of the present embodiment, by making the difference between the refractive index of the polyimide film and the refractive index of the hard coating layer 3 0.04 or less in absolute value, the light reflection at the interface between the hard coating layer 3 and the substrate film 2 can be suppressed, and it is not easy to interfere with the reflected light on the surface of the hard coating layer 3, thereby suppressing the generation of interference fringes. In addition, the measurement wavelength of the refractive index in this specification is set to 589nm, and the measurement temperature is set to 25°C. The details of the refractive index measurement method are shown in the test examples described later.
[0034] From the viewpoint of suppressing the generation of interference fringes, the difference in refractive index between the polyimide film and the hard coat layer 3 is preferably 0.03 or less, and particularly preferably 0.02 or less in absolute value.
[0035] Furthermore, the thickness of the hard coating layer 3 is 0.5 μm or more and 10 μm or less. When the thickness of the hard coating layer 3 exceeds 10 μm, the bendability of the hard coating film 1 decreases. On the other hand, when the thickness of the hard coating layer 3 is less than 0.5 μm, the surface hardness of the hard coating layer 3 decreases and the scratch resistance deteriorates. That is, by making the thickness of the hard coating layer 3 within the above range, the bending resistance and scratch resistance of the hard coating film 1 become excellent.
[0036] From the above viewpoints, the thickness of the hard coat layer 3 is preferably 0.75 μm or more, and particularly preferably 1 μm or more. In addition, the thickness of the hard coat layer 3 is preferably 8 μm or less, and particularly preferably 6 μm or less.
[0037] (1) Constituent components of hard coating
[0038] (1-1) Base film
[0039] The base film 2 of the hard coat film 1 of this embodiment is a polyimide film, and when used for a display, a transparent polyimide film with less yellowing is preferred. Thus, a display (particularly a flexible display) that displays transparent images with high color reproducibility can be obtained.
[0040] Specifically, the polyimide film used in this embodiment preferably has a transmittance of 75% or more, more preferably 80% or more, and particularly preferably 85% or more at a wavelength of 550 nm from the viewpoint of transparency. The method for measuring transmittance in this specification is as described in the Examples below.
[0041] In addition, as the polyimide film used in the present embodiment, from the perspective of reducing yellowing, a polyimide film having an absolute value of b* of the L*a*b* colorimetric system based on a transmission measurement method of 10 or less is preferred, a polyimide film having an absolute value of 5 or less is more preferred, and a polyimide film having an absolute value of 3 or less is particularly preferred. The method for measuring b* in this specification is shown in the Examples described later.
[0042] The polyimide film in this specification refers to a film containing preferably 50% by mass or more, particularly preferably 80% by mass or more, and further preferably 90% by mass or more of polyimide, i.e., a polymer having an imide bond in the main chain. In addition, since poly(meth)acrylimide does not have an imide bond in the main chain, it is not a polyimide, and such a poly(meth)acrylimide film will whiten when bent repeatedly.
[0043] The polyimide film can be generally obtained by polymerizing tetracarboxylic anhydride (preferably aromatic tetracarboxylic dianhydride) and diamine (preferably aromatic diamine) in a solution to generate polyamic acid, molding the polyamic acid into a film, and then dehydrating and ring-closing the polyamic acid moiety, but is not limited thereto.
[0044] The polyimide in the polyimide film may be modified. For example, the aromatic ring generally contained in the polyimide may be modified with an aliphatic hydrocarbon, thereby improving the adhesion between the base film 2 and the hard coat layer 3 .
[0045] The lower limit of the refractive index of the polyimide film is usually 1.50 or more, preferably 1.55 or more, and more preferably 1.60 or more. The upper limit of the refractive index of the polyimide film is usually 1.85 or less, preferably 1.80 or less, and more preferably 1.75 or less.
[0046] For the above-mentioned polyimide film, in order to improve the adhesion with the layer (hard coating layer 3 or adhesive layer described later) provided on the surface thereof, surface treatment can be applied to one or both sides by primer treatment, oxidation method, convexification method, etc. as needed. As oxidation method, for example, corona discharge treatment, chromic acid treatment, flame treatment, hot air treatment, ozone ultraviolet treatment, etc. can be listed, and as concave-convex method, for example, sandblasting method, solvent treatment method, etc. can be listed.
[0047] As the lower limit of the thickness of the polyimide film, it is preferably 5 μm or more, particularly preferably 7.5 μm or more, and further preferably 10 μm or more. By making the thickness of the polyimide film above the above, the hard coat 1 can exert the prescribed mechanical strength, and it is not easy to break even when it is repeatedly bent. On the other hand, as the upper limit of the thickness of the polyimide film, it is preferably 300 μm or less, particularly preferably 90 μm or less, and further preferably 50 μm or less. Since the polyimide film is easy to color, by making the thickness of the polyimide film below the above, transparency can be ensured, and the b* value can be suppressed to a lower level, so that it can be suitably used for optical purposes. In addition, when the thickness of the polyimide film is below the above, the hard coat 1 can exert the prescribed flexibility and become easy to bend.
[0048] (1-2) Hard coating
[0049] The hard coating layer 3 of the hard coating film 1 of the present embodiment is laminated on one main surface side ( Figure 1 The upper side in the middle), giving the hard coating film 1 a higher surface hardness.
[0050] The lower limit of the refractive index of the hard coating layer 3 is preferably 1.40 or more, particularly preferably 1.45 or more, and more preferably 1.56 or more. In addition, the upper limit of the refractive index of the hard coating layer 3 is preferably 1.85 or less, particularly preferably 1.80 or less, and more preferably 1.75 or less. By making the refractive index of the hard coating layer 3 within the above range, the absolute value of the difference in the refractive index of the polyimide film becomes easy to become 0.04 or less.
[0051] As long as the hard coating layer 3 satisfies the above-mentioned refractive index difference and has a specified hardness, there is no particular limitation, but it is preferably formed from a material obtained by curing a composition containing an active energy ray-curable component, and is particularly preferably formed from a material obtained by curing a composition containing an active energy ray-curable component and transition metal oxide particles (hereinafter sometimes referred to as a "hard coating composition").
[0052] (1-2-1) Active Energy Ray-Curing Component
[0053] As the active energy ray-curable component, it is preferred that the active energy ray-curable component exhibits a predetermined hardness by being cured by irradiation with active energy rays and that the active energy ray-curable component can achieve the above-mentioned refractive index difference by virtue of its relationship with the transition metal oxide fine particles.
[0054] As specific active energy ray-curable components, polyfunctional (meth)acrylate monomers, (meth)acrylate prepolymers, active energy ray-curable polymers, etc. can be listed, among which polyfunctional (meth)acrylate monomers and / or (meth)acrylate prepolymers are preferred, and polyfunctional (meth)acrylate monomers are more preferred. Polyfunctional (meth)acrylate monomers and (meth)acrylate prepolymers can be used alone or both at the same time. In addition, in this specification, (meth)acrylate refers to both acrylate and methacrylate. Other similar terms are also the same.
[0055] Examples of the polyfunctional (meth)acrylate monomer include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, hydroxypivalate neopentyl glycol di(meth)acrylate, dicyclopentyl di(meth)acrylate, caprolactone-modified dicyclopentenyl di(meth)acrylate, ethylene oxide-modified phosphoric acid di(meth)acrylate, allylated cyclohexyl di(meth)acrylate, isocyanurate di(meth)acrylate, trihydroxylamine di(meth)acrylate, and polyisocyanate. Methylpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, propionic acid-modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, tri(acryloxyethyl)isocyanurate, propionic acid-modified dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ethylene oxide-modified dipentaerythritol hexa(meth)acrylate, caprolactone-modified dipentaerythritol hexa(meth)acrylate and other multifunctional (meth)acrylates. They can be used alone or in combination of two or more. Among the above, from the perspective of dispersibility and scratch resistance of transition metal oxide particles, dipentaerythritol hexa(meth)acrylate, ethylene oxide-modified dipentaerythritol hexa(meth)acrylate, or a mixture thereof is preferred.
[0056] On the other hand, examples of the (meth)acrylate prepolymer include polyester acrylate, epoxy acrylate, urethane acrylate, polyol acrylate and the like prepolymers.
[0057] The polyester acrylate prepolymer can be obtained, for example, by esterifying the hydroxyl groups of a polyester oligomer having hydroxyl groups at both ends obtained by condensation of a polycarboxylic acid and a polyol with (meth)acrylic acid, or by esterifying the terminal hydroxyl groups of an oligomer obtained by adding alkylene oxide to a polycarboxylic acid with (meth)acrylic acid.
[0058] The epoxy acrylate prepolymer can be obtained by, for example, reacting (meth)acrylic acid with an oxirane ring of a bisphenol epoxy resin or a novolac epoxy resin having a relatively low molecular weight to form an ester.
[0059] The urethane acrylate prepolymer can be obtained by esterifying, with (meth)acrylic acid, a polyurethane oligomer obtained by a reaction of a polyether polyol or a polyester polyol with a polyisocyanate.
[0060] The polyol acrylate-based prepolymer can be obtained by esterifying a hydroxyl group of a polyether polyol with (meth)acrylic acid, for example.
[0061] The above prepolymers may be used alone or in combination of two or more.
[0062] (1-2-2) Transition Metal Oxide Microparticles
[0063] The hard coating composition constituting the hard coating layer 3 of the present embodiment preferably contains transition metal oxide particles. By containing transition metal oxide particles, the refractive index of the hard coating layer 3 can be made close to the refractive index of the polyimide film, and the absolute value of the refractive index difference can be easily made to be less than 0.04. In addition, it is also possible to impart a higher surface hardness to the hard coating layer 3.
[0064] As the above-mentioned transition metal oxide particles, for example, particles such as zirconium oxide, titanium oxide, tantalum oxide, zinc oxide, hafnium oxide, cerium oxide, and niobium oxide are preferred. They can be used alone or in combination of two or more. Among the above, oxide particles of the fourth group element that can give a higher refractive index to the hard coating layer 3 and are not easy to increase the haze of the hard coating layer 3 are particularly preferred, and specifically zirconium oxide particles and titanium oxide particles are particularly preferred. The crystal structure of the titanium oxide particles is not particularly limited, but is preferably rutile. By making it rutile, the time-dependent degradation of the hard coating layer 3 caused by the photocatalytic activity can be suppressed.
[0065] Zirconium oxide particles and titanium oxide particles may also be surface treated. For example, they may be covered with oxides of aluminum, silicon, etc., or modified with organic compounds. Examples of organic compounds include polyols, alkanolamines, stearic acid, silane coupling agents, and titanate coupling agents. Such surface treatment can improve dispersibility and the like, and can make the above-mentioned effects more excellent.
[0066] The shape of the transition metal oxide fine particles may be spherical or non-spherical.
[0067] As the lower limit of the average particle size of the transition metal oxide particles, it is preferably 1 nm or more, particularly preferably 3 nm or more, and further preferably 5 nm or more. By making the average particle size of the transition metal oxide particles 1 nm or more, the dispersibility is improved, and the obtained hard coating layer 3 has a higher surface hardness. In addition, as the upper limit of the average particle size of the transition metal oxide particles, it is preferably 500 nm or less, particularly preferably 200 nm or less, and further preferably 50 nm or less. By making the average particle size of the transition metal oxide particles 500 nm or less, light scattering is not easy to occur in the obtained hard coating layer 3, and the transparency of the hard coating layer 3 becomes higher. In addition, the average particle size of the transition metal oxide particles is set to the primary particle size measured by the Zeta potential measurement method.
[0068] Regarding the content of the transition metal oxide fine particles in the hard coat layer 3 of the present embodiment, in the hard coat layer 3, it is preferably 5% by mass or more, particularly preferably 10% by mass or more, and further preferably 40% by mass or more, based on the following limit. By making the content of the transition metal oxide fine particles 5% by mass or more, the refractive index of the hard coat layer 3 becomes easy to approach the refractive index of the polyimide film, and it becomes easy to give a high surface hardness to the hard coat layer 3. On the other hand, in the hard coat layer 3, the content of the transition metal oxide fine particles is preferably 95% by mass or less, particularly preferably 85% by mass or less, and further preferably 75% by mass or less, based on the upper limit. By making the content of the transition metal oxide fine particles 95% by mass or less, as described above, the refractive index of the hard coat layer 3 becomes easy to approach the refractive index of the polyimide film, and it becomes easy to form a layer using the hard coat composition.
[0069] The content of the transition metal oxide fine particles can be determined from the blending ratio. If the blending ratio is unknown, it can be determined in the following manner. That is, a portion of the hard coating layer 3 of the hard coating film 1 is separated from the base film 2 in the form of a fragment or the like, and the organic components of the separated hard coating layer 3 are burned in accordance with JIS 7250-1. Then, the mass % of the transition metal oxide fine particles can be determined from the obtained ash content.
[0070] Here, a dispersant may be used to improve the dispersibility of the transition metal oxide fine particles in the hard coat composition. As the dispersant, an acrylic resin is preferred from the viewpoint of compatibility with the active energy ray-curable component.
[0071] (1-2-3) Photopolymerization Initiator
[0072] When ultraviolet rays are used as active energy rays for curing the active energy ray-curable component, the hard coating composition preferably contains a photopolymerization initiator. By containing a photopolymerization initiator, the active energy ray-curable component can be polymerized efficiently, and the polymerization curing time and the amount of ultraviolet rays irradiation can be reduced.
[0073] Examples of such photopolymerization initiators include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholine-propane-1-one, and 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2-propyl)ketone. , benzophenone, p-phenylbenzophenone, 4,4'-diethylaminobenzophenone, dichlorobenzophenone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzyl dimethyl ketal, acetophenone dimethyl ketal, p-dimethylaminobenzoate, oligo[2-hydroxy-2-methyl-1[4-(1-methylvinyl)phenyl]propanone], 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, etc. These may be used alone or in combination of two or more.
[0074] The content of the photopolymerization initiator in the hard coating composition is preferably 0.01 parts by mass or more, particularly preferably 0.1 parts by mass or more, and more preferably 1 parts by mass or more, based on the following limit, relative to 100 parts by mass of the active energy ray-curable component. In addition, based on the upper limit, it is preferably 20 parts by mass or less, particularly preferably 10 parts by mass or less, and more preferably 5 parts by mass or less.
[0075] (1-2-4) Other ingredients
[0076] The hard coating composition constituting the hard coating layer 3 of the present embodiment may contain various additives in addition to the above-mentioned components. Examples of the various additives include ultraviolet absorbers, antioxidants, light stabilizers, antistatic agents, silane coupling agents, anti-aging agents, thermal polymerization inhibitors, colorants, surfactants, storage stabilizers, plasticizers, lubricants, defoamers, organic fillers, wettability improvers, and coating surface improvers.
[0077] (2) Method for producing hard coating film
[0078] The hard coating film 1 of the present embodiment can be preferably produced by the following method. In this method, as an example, a hard coating composition containing an active energy ray-curable component is used.
[0079] First, a composition layer formed of a hard coating composition is formed on one main surface of the substrate film 2. In this case, the hard coating composition may be directly applied to one main surface of the substrate film 2 to form the composition layer, or the hard coating composition may be applied to a cover sheet and then the composition layer with the cover sheet attached may be attached to one main surface of the substrate film 2.
[0080] As the cover sheet, a desired resin film can be used. In addition, a release sheet obtained by subjecting one or both surfaces of these resin films to a release treatment using a release agent can also be used.
[0081] The composition layer can be formed by preparing a coating liquid containing a hard coating composition and, if necessary, a solvent, applying the coating liquid to the substrate film 2 or the cover sheet, and drying the coating liquid. The coating liquid can be applied by a common method, such as a rod coating method, a knife coating method, a Meyer rod method, a roller coating method, a blade coating method, a die coating method, or a gravure coating method. Drying can be performed, for example, by heating at 40 to 180° C. for about 30 seconds to 5 minutes.
[0082] Examples of the solvent include aliphatic hydrocarbons such as hexane and heptane, aromatic hydrocarbons such as toluene and xylene, halogenated hydrocarbons such as methylene chloride and ethylene dichloride, alcohols such as methanol, ethanol, propanol, butanol, and propylene glycol monomethyl ether, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, 2-pentanone, isophorone, and cyclohexanone, esters such as ethyl acetate and butyl acetate, and cellosolve solvents such as ethyl cellosolve. Only one solvent may be used, or two or more solvents may be mixed and used. The concentration and viscosity of the coating liquid are not particularly limited as long as they are within the range that can be coated, and can be appropriately selected according to the situation.
[0083] Next, the composition layer is irradiated with active energy rays to cure the composition layer, thereby forming the hard coating layer 3 .
[0084] As active energy rays, ultraviolet rays, electron beams, etc. can be used. Ultraviolet irradiation can be performed using a high-pressure mercury lamp, a Fusion H lamp, a xenon lamp, etc. The irradiation amount of ultraviolet rays is preferably 50 to 1000 mW / cm 2 , light intensity is 50~1000mJ / cm 2 On the other hand, electron beam irradiation can be performed by an electron beam accelerator or the like, and the irradiation amount of the electron beam is preferably about 10 to 1000 krad.
[0085] When ultraviolet rays are used as active energy rays, the composition layer is preferably irradiated with ultraviolet rays in a state where oxygen is isolated. This prevents curing from being inhibited by oxygen and effectively forms a hard coating layer 3 having a high surface hardness.
[0086] In order to isolate the above-mentioned composition layer from oxygen, when a covering sheet is attached to the above-mentioned composition layer, the state of being covered with the covering sheet is maintained; when a covering sheet is not attached to the above-mentioned composition layer, the covering sheet is re-laminated on the above-mentioned composition layer, or the laminate of the substrate film 2 and the composition layer is placed in an environment with a low oxygen concentration, preferably in a nitrogen atmosphere.
[0087] (3) Physical properties of hard coating
[0088] (3-1) Maximum reflectivity difference
[0089] As described above, in the hard coating film 1 of the present embodiment, the generation of interference fringes can be suppressed. This effect can be evaluated by visual observation as well as by the measured value of the maximum reflectivity difference. When measuring the maximum reflectivity difference, the normal direction of the film is first set to 0°, and light is irradiated from the direction of the incident angle of 8°. The light reflected by the film is collected by an integrating sphere and detected as reflected light. In addition, the wavelength is changed to irradiate the light, and the reflected light corresponding to each wavelength is detected.
[0090] The reflected light is detected as a relative value (hereinafter referred to as "reflectivity") corresponding to each measurement wavelength when the reflected light based on the barium sulfate crystal is set to 100. That is, a graph can be obtained with the horizontal axis being the measurement wavelength and the vertical axis being the reflectivity. The graph is generally in an undulating shape with a plurality of minimum and maximum values.
[0091] Here, in the graph of the reflectivity at a wavelength of 500 to 600 nm, the largest difference between the differences between the adjacent maximum and minimum values is measured as the "maximum reflectivity difference". The maximum reflectivity difference is preferably 1.5 or less, particularly preferably 1.1 or less, and further preferably 0.6 or less. By setting the reflectivity to 1.5 or less, the generation of interference fringes can be suppressed.
[0092] (3-2) Minimum mandrel diameter
[0093] As described above, the hard coating film 1 of the present embodiment is excellent in bending resistance capable of withstanding repeated bending, and the degree of bending can be determined based on the minimum mandrel diameter.
[0094] For the hard coating film 1 of the present embodiment, in the bending resistance test based on the cylindrical mandrel method according to JIS K5600-5-1, the diameter of the mandrel with the smallest diameter among the mandrels on which no cracking and peeling occur on the hard coating layer 3 (minimum mandrel diameter) is preferably 14 mm or less, particularly preferably 6 mm or less, and further preferably 4 mm or less.
[0095] (3-3) Image clarity
[0096] The interference fringes of the hard coating film 1 of the present embodiment are prevented not by adding micron-sized particles, but by reducing the refractive index difference between the hard coating layer 3 and the base film 2. Therefore, compared with the case where interference fringes are prevented by adding micron-sized particles, the hard coating film 1 of the present embodiment can be a film having a more excellent image clarity.
[0097] When a hard coat film having excellent image clarity is applied to a display, a display having excellent image contrast can be obtained. From this viewpoint, the image clarity is preferably 400% or more, more preferably 430% or more, and particularly preferably 450% or more.
[0098] The image clarity can be determined according to JIS K7374 as the total value of the image clarity measured with five types of slits (slit widths: 0.125 mm, 0.25 mm, 0.5 mm, 1 mm, and 2 mm).
[0099] (3-4) Haze value
[0100] When used in a display, the haze value of the hard coat film 1 measured in accordance with JIS K7136 is preferably 1% or less, more preferably 0.8% or less, and particularly preferably 0.5% or less, from the viewpoint of displaying clearer images.
[0101] (3-5) 60° glossiness
[0102] When applied to a display, the 60° gloss (Gloss value) of the hard coat layer 3 in the hard coat film 1 according to JIS Z8741-1997 is preferably set to a value of 100% or more, more preferably a value of 120% or more, and particularly preferably a value of 140% or more, from the viewpoint of displaying a clearer image.
[0103] (4) Other Implementation Methods-1
[0104] like Figure 2 As shown, a second hard coating layer 4 (a second hard coating layer 4a) may be laminated on the other main surface side (the surface opposite to the surface on which the hard coating layer 3 is laminated) of the substrate film 2 in the hard coating film 1. Figure 2 The hard coating film shown is denoted by "1A"). By laminating the second hard coating layer 4, the scratch resistance of the other main surface of the substrate film 2 is improved, and the curing shrinkage of the hard coating layer 3 is offset by the curing shrinkage of the second hard coating layer 4, so that the warping of the hard coating film 1A can be suppressed.
[0105] The second hard coating layer 4 may be formed of the same material as the hard coating layer 3 or may be formed of a different material. In addition, the thickness of the second hard coating layer 4 may be the same as the hard coating layer 3 or may be different from that of the hard coating layer 3.
[0106] The hard coating film 1A of this embodiment can be manufactured basically in the same manner as the above-mentioned hard coating film 1. However, the hard coating layer 3 and the second hard coating layer 4 may be cured simultaneously, or the composition layer of the second hard coating layer 4 (or the hard coating layer 3) may be formed and cured after the composition layer of the hard coating layer 3 (or the second hard coating layer 4) is formed and cured.
[0107] (5) Other Implementation Methods-2
[0108] like Figure 3 As shown, an adhesive layer 5 may be laminated on the other main surface side (the surface opposite to the surface on which the hard coating layer 3 is laminated) of the substrate film 2 in the hard coating film 1. Figure 3 The hard coating film shown is denoted by "1B"). By laminating such an adhesive layer 5, the hard coating film 1B can be easily attached to a desired adherend. In addition, an adhesive layer can also be laminated on the side of the second hard coating layer 4 in the hard coating film 1A opposite to the substrate film 2 side.
[0109] The adhesive constituting the adhesive layer 5 is not particularly limited, and known adhesives such as acrylic adhesives, rubber adhesives, and silicone adhesives can be used. The thickness of the adhesive layer 5 is not particularly limited, but is usually in the range of 5 to 100 μm, preferably 10 to 60 μm.
[0110] The hard coating film 1B of the present embodiment can be produced basically in the same manner as the above-mentioned hard coating film 1. The adhesive layer 5 may be formed by a common method.
[0111] Moreover, a release sheet may be laminated on the exposed surface (the surface opposite to the base film 2 side) of the pressure-sensitive adhesive layer 5 .
[0112] (6) Other Implementation Methods-3
[0113] The hard coat film 1 of the present embodiment may be laminated with other layers, for example, an adhesive layer, a barrier layer, a conductive layer, a low reflection layer, an easy-printing layer, an antifouling layer, and the like.
[0114] (7) Application of hard coating
[0115] The hard coating films 1, 1A, 1B of the above embodiments can be preferably used as flexible components of the surface layer (protective film) or the middle layer of flexible displays in, for example, various electronic devices, especially mobile electronic devices. Specifically, they can be preferably used as flexible components of the surface layer (protective film) or the middle layer of various flexible displays such as liquid crystal displays (LCDs), organic EL displays (OELDs), and electronic paper modules (film-like electronic paper).
[0116] The embodiments described above are described to facilitate understanding of the present invention, and are not described to limit the present invention. Therefore, the gist of each element disclosed in the above embodiments also includes all design changes and equivalents belonging to the technical scope of the present invention.
[0117] For example, another layer may be present between the base film 2 and the hard coat layer 3 , the second hard coat layer 4 , or the adhesive layer 5 in the hard coat films 1 , 1A, and 1B.
[0118] Example
[0119] Hereinafter, the present invention will be described in more detail with reference to Examples and the like, but the scope of the present invention is not limited to these Examples and the like.
[0120] [Manufacturing Example 1] (Manufacturing 1 of a base film)
[0121] In N,N-dimethylacetamide solvent, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, biphenyltetracarboxylic dianhydride and 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropionic dianhydride were mixed and dissolved under cooling, and then stirred at room temperature for 10 hours to obtain a polyamic acid solution.
[0122] Acetic anhydride and pyridine were added to the obtained polyamic acid solution, and after sufficient stirring, the solution was coated on a glass plate and slowly heated from room temperature to 180°C. After reaching 180°C, the solution was heated for a certain period of time and then vacuumed to completely remove the volatile components. Finally, the solution was cooled to room temperature under vacuum to obtain a polyimide film A having a film thickness of 25 μm. The polyimide film A was measured to have a b* of 0.61, a refractive index of 1.62, and a transmittance of 90% at a wavelength of 550 nm.
[0123] In addition, the film thickness of the polyimide film was measured in accordance with JIS K7130 using a constant pressure thickness gauge (manufactured by Teclock, product name "PG-02").
[0124] Regarding the above b*, b* of the L*a*b* colorimetric system was measured by a transmission measurement method in accordance with JIS Z8722, using a simultaneous measurement spectrophotometer (manufactured by NIPPON DENSHOKU INDUSTRIES Co., LTD., product name "SQ-2000") as a measuring device and a C light source 2° field of view (C / 2) as a light source.
[0125] The transmittance at the wavelength of 550 nm was measured using an ultraviolet-visible-near-infrared spectroscopic transmittance meter (manufactured by Shimadzu Corporation, product name "UV3600").
[0126] [Manufacturing Example 2] (Manufacturing of base film 2)
[0127] A polyimide film B having a film thickness of 15 μm, a b* of 2.25, a refractive index of 1.70, and a transmittance of 87% at a wavelength of 550 nm was obtained by implementing the same manufacturing method as in Manufacturing Example 1, except that the blending ratio of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, biphenyltetracarboxylic dianhydride and 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropionic dianhydride was changed in the N,N-dimethylacetamide solvent and the concentration of the obtained polyimide coating liquid was adjusted (the measurement method is as shown above).
[0128] [Example 1]
[0129] 100 parts by mass of dipentaerythritol hexaacrylate as an active energy ray-curable component (converted as solid content; the same applies hereinafter), 150 parts by mass of surface-modified zirconium oxide fine particles (manufactured by CIK Nanotek, product name "ZRMIBK15WT%-F85", average particle size: 15 nm) as transition metal oxide fine particles, and 5 parts by mass of 1-hydroxycyclohexyl phenyl ketone as a photopolymerization initiator are stirred and mixed in a mixed solvent of methyl isobutyl ketone and cyclohexanone in a mass ratio of 1:1, thereby obtaining a coating liquid of a hard coating composition.
[0130] Next, the coating liquid of the hard coating composition was applied onto one side of the polyimide film A as a substrate film using a Meyer bar and dried by heating at 70° C. for 1 minute to form a composition layer of the hard coating composition.
[0131] Then, the composition layer of the hard coat composition was cured by irradiating with ultraviolet rays from the composition layer side under the following conditions to form a hard coat layer (thickness: 3 μm) to obtain a hard coat film.
[0132] <Ultraviolet irradiation conditions>
[0133] ・Ultraviolet irradiation device: Ultraviolet irradiation device manufactured by GS Yuasa Corporation
[0134] Light source: high pressure mercury lamp
[0135] Lamp power: 1.4kW
[0136] Illuminance: 100mW / cm 2
[0137] Light intensity: 240mJ / cm 2
[0138] Conveyor belt speed: 1.2m / min
[0139] ・Ultraviolet irradiation in a nitrogen atmosphere (oxygen concentration is less than 1%)
[0140] [Examples 2 to 8, Comparative Examples 1 to 5]
[0141] A hard coat film was produced in the same manner as in Example 1 except that the types and blending amounts of the components constituting the hard coat composition, the thickness of the hard coat layer, and the type and thickness of the substrate film were changed as shown in Table 1.
[0142] In addition, the details of the abbreviations and the like described in Table 1 are as follows.
[0143] A: Dipentaerythritol hexaacrylate
[0144] B: Ethylene oxide-modified dipentaerythritol hexaacrylate (12 mol of ethylene oxide introduced)
[0145] C: Surface-modified zirconium oxide fine particles (manufactured by CIK Nanotec, product name "ZR MIBK15WT%-F85", average particle size: 15 nm)
[0146] D: Surface-modified titanium oxide fine particles (manufactured by TAYCA, product name "ND139", average particle size: 10 nm)
[0147] E: 1-Hydroxycyclohexyl phenyl ketone
[0148] PI-25: Polyimide Film A
[0149] PI-15: Polyimide film B
[0150] PET: Polyethylene terephthalate film (manufactured by Mitsubishi Plastics, Inc., product name "Diafoil T-60", thickness: 50 μm)
[0151] [Test Example 1] (Measurement of refractive index)
[0152] (1) Refractive index of substrate film
[0153] The refractive index of the substrate films used in Examples and Comparative Examples was measured at a measurement wavelength of 589 nm and a measurement temperature of 25° C. using an Abbe refractometer (manufactured by ATAGO CO., LTD., product name “Multi-wavelength Abbe Refractometer DR-M2”) in accordance with JIS K7142 (2008). The results are shown in Table 2.
[0154] (2) Refractive index of hard coating
[0155] A hard coating layer with a thickness of 200 nm was formed on the untreated surface of a polyethylene terephthalate film (manufactured by TOYOBO CO., LTD., product name "COSMOSHINE A4100", thickness: 50 μm) treated for easy adhesion in the same manner as in the examples and comparative examples. Next, the easy adhesion treated surface of the polyethylene terephthalate film was rubbed with sandpaper and filled with black using an oil pen (manufactured by ZEBRA CO., LTD., product name "Mckee Black").
[0156] Subsequently, the refractive index of the hard coat layer was measured at a measurement wavelength of 589 nm and a measurement temperature of 25° C. using an ellipsometer (manufactured by JA Woollam Co., Inc., product name “M-2000”) in accordance with JIS K7142 (2008).
[0157] (3) Calculation of refractive index difference
[0158] The refractive index difference was calculated by subtracting the refractive index of the hard coat layer from the refractive index of the substrate film measured above.
[0159] [Test Example 2] (Evaluation of interference fringes)
[0160] (1) Visual evaluation
[0161] The hard coating films produced in the examples and comparative examples were attached to a black acrylic plate (manufactured by MITSUBISHI RAYON CO., LTD., product name "Acrylight L502") via a double-sided adhesive sheet (manufactured by Lintec Corporation, product name "OPTERIA MO-3006C", thickness: 25 μm). At this time, the hard coating film was attached so that the base film was in contact with the acrylic plate.
[0162] The obtained laminate was visually observed for interference fringes from the hard coat layer side under a three-wavelength fluorescent lamp, and evaluated based on the following criteria.
[0163] Good (◎): Interference fringes are barely visible
[0164] Generally good (○): Interference fringes are not easily seen
[0165] Slightly bad (△): Interference fringes can be seen
[0166] Poor (×): Interference fringes can be clearly seen
[0167] (2) Determination of maximum reflectivity difference
[0168] The maximum reflectance difference between wavelengths of 500 and 600 nm in the reflectance spectrum of the laminate obtained in (1) was measured using a spectrophotometer under the following conditions.
[0169] <Measurement conditions>
[0170] Spectrophotometer: manufactured by Shimadzu Corporation, product name "UV-3600 UV-Visible Near Infrared Spectrophotometer"
[0171] · Sample holder: manufactured by Shimadzu Corporation, product name "Large Sample Chamber MPC-3100"
[0172] Integrating sphere: manufactured by Shimadzu Corporation, product name "Integrating Sphere Attachment ISR-3100"
[0173] ·Incident angle: 8°
[0174] [Test Example 3] (Evaluation of scratch resistance)
[0175] The hard coating surfaces of the hard coating films prepared in the examples and comparative examples were rubbed with #0000 steel wool at a weight of 125 g / cm 2 The test range was 100 mm in length and 20 mm in width. The number of scratches within the test range was visually confirmed under a three-wavelength fluorescent lamp, and the scratch resistance was evaluated based on the following criteria. The results are shown in Table 2.
[0176] ○: The number of scratches is less than 20.
[0177] ×: The number of scratches is 20 or more.
[0178] [Test Example 4] (Mandrel Test)
[0179] For the hard coating films manufactured in the embodiments and comparative examples, a mandrel test according to JIS K5600-5-1 was performed using a cylindrical mandrel bending tester (manufactured by CORTEC). The mandrel test was performed with the hard coating layer of the hard coating film set to the outside. The diameter of the mandrel with the smallest diameter (minimum mandrel diameter) among the mandrels that did not cause undesirable conditions such as cracking and peeling on the hard coating layer was obtained. The results are shown in Table 2.
[0180] [Test Example 5] (Bending resistance test)
[0181] The hard coating films produced in the examples and comparative examples were subjected to repeated bending using a durability tester (manufactured by YUASA SYSTEM Co., Ltd., product name "Plane Body Unloaded U-Shaped Elongation Tester DLDMLH-FS"), with the hard coating layer on the outside, at a test speed of 60 mm / s, with various changes made to the number of tests (number of round trips) and the bending diameter. Next, the occurrence of defects such as cracking and peeling of the hard coating layer, whitening of the hard coating layer, and bending marks was confirmed, and the bending resistance was evaluated based on the following criteria. The results are shown in Table 2.
[0182] ◎: The bending diameter was 5 mm or less, and no defect occurred even when the number of tests was 20,000 or more.
[0183] ○: The bending diameter was 10 mm or less, and no defect occurred even when the number of tests was 20,000 or more.
[0184] ×: Did not meet the standard of ○.
[0185] [Test Example 6] (Evaluation of image clarity)
[0186] The hard coating films produced in the examples and comparative examples were measured for image clarity (%) using an image clarity measuring instrument (manufactured by Suga Test Instruments Co., Ltd., product name "ICM-10P") in accordance with JIS K7374 for the total value of five slits (slit width: 0.125 mm, 0.25 mm, 0.5 mm, 1 mm, and 2 mm). Based on the results, image clarity of less than 400% was evaluated as ×, image clarity of 400% or more and less than 450% was evaluated as ○, and image clarity of 450% or more was evaluated as ◎. The results are shown in Table 2.
[0187] [Test Example 7] (Evaluation of Haze Value)
[0188] The hard coating films produced in the examples and comparative examples were measured for haze value (%) using a haze meter (manufactured by NIPPON DENSHOKU INDUSTRIES Co., LTD, product name "NDH5000") in accordance with JIS K7136. Based on the results, a haze value greater than 1% was evaluated as ×, a haze value less than 1% and more than 0.5% was evaluated as ○, and a haze value less than 0.5% was evaluated as ◎. The results are shown in Table 2.
[0189] [Test Example 8] (Evaluation of 60° glossiness)
[0190] The hard coating films produced in the examples and comparative examples were measured for 60° gloss (gloss value) using a gloss meter (manufactured by NIPPON DENSHOKU INDUSTRIES Co., LTD) in accordance with JIS Z8741-1997. Based on the results, a 60° gloss value of less than 100% was evaluated as ×, a 60° gloss value of 100% or more and less than 140% was evaluated as ○, and a 60° gloss value of 140% or more was evaluated as ◎. The results are shown in Table 2.
[0191] [Table 1]
[0192]
[0193] [Table 2]
[0194]
[0195] As is clear from Table 2, the hard coating films obtained in Examples are excellent in scratch resistance and optical properties, and are also excellent in bending resistance, and interference fringes are less likely to occur.
[0196] Industrial Applicability
[0197] The hard coating film of the present invention is suitable as a flexible member constituting a flexible display that is repeatedly bent, and is particularly suitable as a protective film located on the surface layer.
Claims
1. A flexible display that is repeatedly bent, characterized in that: The flexible display has a hard coating film, The hard coating film comprises a base film and a hard coating layer laminated on at least one main surface side of the base film. The substrate film is a polyimide film, The difference between the refractive index of the polyimide film and the refractive index of the hard coating layer is 0.04 or less in absolute value, The polyimide film has a thickness of 5 μm or more and 50 μm or less. For the hard coating film, in a bending resistance test based on the cylindrical mandrel method in accordance with JIS K5600-5-1, when the hard coating layer is set on the outside compared to the substrate film and the test is performed, the diameter of the mandrel with the smallest diameter among the mandrels that do not cause cracks and peeling on the hard coating layer is less than 8 mm.
2. The repeatedly bent flexible display according to claim 1, characterized in that: The refractive index of the hard coat layer is 1.40 or more and 1.85 or less.
3. The repeatedly bent flexible display according to claim 1, characterized in that: The hard coating layer has a thickness of 0.5 μm or more and 10 μm or less.
4. The repeatedly bent flexible display according to claim 1, characterized in that: The hard coating film is irradiated with light having a changed wavelength from an incident angle of 8°, and reflected light corresponding to the wavelength is detected. When the relative value when the reflected light based on the barium sulfate crystals is set to 100 is detected as the reflectance, in a graph of the reflectance with a measured wavelength of 500 to 600 nm, the maximum difference between adjacent maximum and minimum values is less than 0.
3.
5. The repeatedly bent flexible display according to claim 1, characterized in that: The hard coat layer is formed of a material obtained by curing a composition containing an active energy ray-curable component and transition metal oxide fine particles.
6. The repeatedly bent flexible display according to claim 5, characterized in that: The transition metal oxide fine particles are one or more of zirconium oxide fine particles and titanium oxide fine particles.
7. The repeatedly bent flexible display according to claim 5, characterized in that: The transition metal oxide fine particles are surface-treated with an organic compound.
8. The repeatedly bent flexible display according to claim 5, characterized in that: The content of the transition metal oxide fine particles in the hard coating layer is 5 mass % or more and 95 mass % or less.
9. The repeatedly bent flexible display according to claim 1, characterized in that: An adhesive layer is laminated on at least one main surface of the base film.