Silica material, ion exchange resin composition, electrolyte membrane, membrane electrode assembly, solid polymer fuel cell, solid polymer electrolysis device, and electrochemical hydrogen compression device

By using a combination of silica material with sulfonic acid groups and ion exchange resin in the electrolyte membrane, the contradiction between proton conductivity and mechanical strength of the electrolyte membrane was resolved, and a balance between proton conductivity and mechanical strength was achieved.

CN118900823APending Publication Date: 2024-11-05TEIJIN LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380028281.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-02-06
Filing Date
2023-03-17
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

There is room for improvement in the proton conductivity of existing electrolyte membranes, and thinning and reducing the dry weight (EW) of each ion exchange group will affect the mechanical strength of the membrane.

Method used

An electrolyte membrane is formed by combining silica material with sulfonic acid groups and ion exchange resin, which improves proton conductivity while maintaining mechanical strength.

Benefits of technology

This improved the proton conductivity of the electrolyte membrane while maintaining its mechanical strength, thus enabling the construction of an efficient proton conduction pathway.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005046898450000101
    Figure BDA0005046898450000101
  • Figure BDA0005046898450000111
    Figure BDA0005046898450000111
  • Figure BDA0005046898450000251
    Figure BDA0005046898450000251
Patent Text Reader

Abstract

A silica material having a silica-containing matrix and having a sulfonic acid group on at least the surface of the matrix, or obtained by bringing a sulfonating agent into contact with the silica-containing matrix.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a silicon dioxide material, an ion exchange resin composition, an electrolyte membrane, a membrane electrode assembly, a solid polymer fuel cell, a solid polymer electrolysis device, and an electrochemical hydrogen compression device. Background Art

[0002] In recent years, there has been an increasing demand for improved performance of electrolyte membranes, especially solid polymer electrolyte membranes. For example, water is electrolyzed using renewable energy sources such as sunlight and wind power to produce hydrogen, the generated hydrogen is compressed and stored at a high density, and the hydrogen is supplied to a fuel cell as needed to generate electricity at a location where electricity is needed. This system has attracted much attention as a very clean energy system that does not produce carbon dioxide. Here, the following water electrolysis method is known: during water electrolysis, the anode and cathode are separated by an electrolyte membrane, so that the protons generated at the anode move to the cathode through the electrolyte membrane and combine with the electrons generated at the cathode to obtain hydrogen. The reaction formula at each pole is as follows.

[0003] Anode: H2O→1 / 2O2+2H + +2e -

[0004] Cathode: 2H + +2e - →H2

[0005] On the other hand, in a fuel cell, protons generated in the hydrogen oxidation reaction at the negative electrode (anode) move through the electrolyte membrane to the positive electrode (cathode), where they generate water through an oxygen reduction reaction to generate electricity. The reaction formulas at each electrode are as follows.

[0006] Negative electrode: H2→2H + +2e -

[0007] Positive electrode: 1 / 2O2+2H + +2e - →H2O

[0008] According to the above working principles, it is known that in either water electrolysis or fuel cells, there is generally a problem of improving the proton conductivity of the electrolyte membrane. In order to improve the proton conductivity of the electrolyte membrane, measures such as reducing the membrane thickness of the electrolyte membrane and reducing the dry mass (equivalent mass: EW) per equivalent ion exchange group of the electrolyte polymer can be considered.

[0009] However, from the viewpoint of the strength required as a separator between electrodes, there is a natural limit to the thinning of the electrolyte membrane. In addition, the reduction in EW may cause the ratio of the skeleton part of the electrolyte polymer to decrease, making it difficult to maintain a solid membrane.

[0010] In order to ensure the strength of the electrolyte membrane, there are the following examples: as a polymer electrolyte for a fuel cell, by making the internal space (voids) of the polymer porous membrane contain a polymer electrolyte, the mechanical strength that cannot be obtained by the electrolyte itself is improved (Patent Document 1). In addition, a suitable porous substrate is proposed for keeping the polymer electrolyte in a polyethylene porous membrane (Patent Document 2). In addition, there is the following prior art: an electrolyte film with excellent mechanical strength is provided by introducing an ion exchange resin into the mesh structure of a porous film of ultra-high molecular weight polyolefin (Patent Document 3). In addition, there is also the following prior art: a thin film electrolyte with excellent mechanical strength is provided by introducing an ion conductor into a solid polymer porous membrane using capillary condensation (Patent Document 4).

[0011] Prior art literature

[0012] Patent Literature

[0013] Patent Document 1: Japanese Patent Application Publication No. 2005-166557

[0014] Patent Document 2: Japanese Patent Application Publication No. 2011-241361

[0015] Patent Document 3: Japanese Patent Application Laid-Open No. 64-22932

[0016] Patent Document 4: Japanese Patent Application Laid-Open No. 1-158051 Summary of the invention

[0017] Although the above-mentioned methods have been studied to improve the proton conductivity of the electrolyte membrane, there is a need to further improve the proton conductivity of the electrolyte membrane.

[0018] The present disclosure is completed in view of the above-mentioned existing situation, and its purpose is to provide: a new silica material useful for improving the proton conductivity of an electrolyte membrane, an ion exchange resin composition containing the silica material, an electrolyte membrane containing the ion exchange resin composition, a membrane electrode assembly obtained by using the electrolyte membrane, a solid polymer fuel cell, a solid polymer electrolysis device and an electrochemical hydrogen compression device.

[0019] Specific methods for achieving the above-mentioned subject include the following aspects.

[0020] <1> A silica material comprising a matrix containing silica, and having a sulfonic acid group on at least a surface of the matrix.

[0021] <2> A silica material obtained by bringing a sulfonating agent into contact with a substrate containing silica.

[0022] <3> The silica material according to <1> or <2>, wherein the substrate is in a granular form.

[0023] <4> The silica material according to <3>, wherein the substrate is silica particles, and the number average particle size of primary particles of the silica particles is 1 nm to 500 nm.

[0024] <5> The silica material according to any one of <1> to <4>, wherein a ratio of a sulfur atom concentration to a total of a silicon atom concentration and a sulfur atom concentration determined by X-ray fluorescence spectrometry (XRF) is 0.01% to 90%.

[0025] <6> An ion exchange resin composition comprising the silica material according to any one of <1> to <5> and an ion exchange resin.

[0026] <7> The ion exchange resin composition according to <6>, wherein a content of the silica material in the solid content of the ion exchange resin composition is 0.01% by mass to 90% by mass.

[0027] <8> An electrolyte membrane comprising the ion exchange resin composition according to <6> or <7>.

[0028] <9> A membrane electrode assembly comprising: the electrolyte membrane according to <8>, a cathode layer stacked on one surface of the electrolyte membrane, and an anode layer stacked on the other surface of the electrolyte membrane.

[0029] <10> A polymer electrolyte fuel cell comprising: the membrane electrode assembly described in <9>, and separators disposed on both surfaces of the membrane electrode assembly.

[0030] <11> A solid polymer electrolysis device comprising: the membrane electrode assembly described in <9>, and separators disposed on both surfaces of the membrane electrode assembly.

[0031] <12> An electrochemical hydrogen compression device comprising the electrolyte membrane described in <8>.

[0032] According to the present disclosure, a novel silica material useful for improving the proton conductivity of an electrolyte membrane, an ion exchange resin composition containing the silica material, an electrolyte membrane containing the ion exchange resin composition, a membrane electrode assembly obtained using the electrolyte membrane, a solid polymer fuel cell, a solid polymer electrolysis device, and an electrochemical hydrogen compression device are provided. DETAILED DESCRIPTION

[0033] Hereinafter, the embodiments of the present disclosure are described in detail. However, the present disclosure is not limited to the following embodiments. In the following embodiments, the constituent elements (including element steps, etc.) are not necessary unless otherwise specified. The numerical values ​​and their ranges are also the same and do not limit the present disclosure.

[0034] In the present disclosure, a numerical range expressed using "to" includes the numerical values ​​described before and after "to" as the minimum value and the maximum value, respectively.

[0035] In the numerical range recorded in the present disclosure, the upper limit or lower limit recorded in one numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in another segment. In addition, in the numerical range recorded in the present disclosure, the upper limit or lower limit of its numerical range can also be replaced by the value shown in the embodiment.

[0036] In the present disclosure, each component may include a plurality of corresponding substances. When a plurality of substances corresponding to each component are present in the composition, the content or content of each component refers to the total content or content of the plurality of substances present in the composition unless otherwise specified.

[0037] In the present disclosure, particles corresponding to each component may include multiple types of particles. When multiple types of particles corresponding to each component are present in the composition, the particle size of each component refers to the value of the mixture of the multiple types of particles present in the composition unless otherwise specified.

[0038] In the present disclosure, the term "layer" or "film" includes a case where the layer or film is formed in the entire region or only in a part of the region when observing the region where the layer or film exists.

[0039] In the present disclosure, the term "stacked" means stacking layers, and two or more layers may be combined or two or more layers may be detachable.

[0040] In the present disclosure, the average thickness of a layer or a film is a value obtained by measuring the thickness of five points of the target layer or film and giving the value as the arithmetic mean thereof.

[0041] The thickness of a layer or film can be measured using a micrometer or the like. In the present disclosure, when the thickness of a layer or film can be directly measured, it is measured using a micrometer. On the other hand, when the thickness of one layer or the total thickness of a plurality of layers cannot be measured using a micrometer, it is measured by observing a cross section of the measurement object using an electron microscope.

[0042] In the present disclosure, the “solid content” of the electrolyte membrane refers to the remainder obtained by removing volatile components such as water and organic solvent from the electrolyte membrane.

[0043] <Silica Materials>

[0044] The first silica material disclosed in the present invention has a matrix containing silica, and has sulfonic acid groups on at least the surface of the matrix. The sulfonic acid groups may be chemically bonded to the surface of the matrix.

[0045] In addition, the second silica material disclosed in the present disclosure is obtained by bringing a sulfonating agent into contact with a substrate containing silica.

[0046] Hereinafter, the first silica material of the present disclosure and the second silica material of the present disclosure may be collectively referred to as the silica material of the present disclosure.

[0047] The silica material disclosed herein can improve the proton conductivity of an electrolyte membrane when used in combination with an ion exchange resin composition of various ion exchange resins. The reason for this is not clear, but is presumed as follows.

[0048] The ion exchange resin contains a sulfonic acid group, a carboxyl group, a quaternary ammonium group, or a primary amino group, a secondary amino group or a tertiary amino group as an ion exchange group. In particular, as a preferred ion exchange group contained in the ion exchange resin constituting the solid polymer electrolyte membrane, a sulfonic acid group can be cited. The silica material disclosed in the present invention has a sulfonic acid group on at least the surface of the matrix containing silica, and therefore has a high affinity with the ion exchange group (especially the sulfonic acid group). By dispersing the silica material disclosed in the ion exchange resin, the ion exchange group contained in the ion exchange resin in the electrolyte membrane interacts with the sulfonic acid group contained in the silica material disclosed in the present invention, and it is easy to efficiently construct a proton conductive path in the electrolyte membrane.

[0049] As a result, it is estimated that when an electrolyte membrane is produced by combining the silica material disclosed in the present invention with various ion exchange resins, the proton conductivity of the electrolyte membrane can be improved.

[0050] Hereinafter, the silica material of the present disclosure will be described in detail.

[0051] (Matrix)

[0052] The silica material disclosed herein has a matrix containing silica. The shape of the matrix is ​​not particularly limited, and examples thereof include a granular, fibrous, plate-like, or film-like matrix.

[0053] As a granular matrix containing silicon dioxide, silicon dioxide particles can be cited. The silicon dioxide particles can be crystalline or amorphous. The silicon dioxide particles can be particles made from silicon compounds such as water glass and alkoxysilane as raw materials, or can be particles obtained by crushing quartz.

[0054] Specific examples of the silica particles include silica particles produced by a sol-gel method, colloidal silica particles, fumed silica particles obtained by a gas phase method, and fused silica particles.

[0055] The number average particle size of primary particles of the silica particles is preferably 1 nm to 500 nm, more preferably 5 nm to 300 nm, and even more preferably 10 nm to 200 nm.

[0056] The number average particle size of primary particles of silica particles refers to a value calculated as the arithmetic average of equivalent circle diameters of 50 silica particles obtained by scanning electron microscope observation.

[0057] The primary particles of the silica particles may aggregate to form secondary particles.

[0058] The volume average particle size of the secondary particles of the silica particles is preferably 500 nm to 500 μm, more preferably 1 μm to 300 μm, and further preferably 10 μm to 150 μm.

[0059] The volume average particle size of the secondary particles of the silica particles is a value measured using a laser diffraction particle size distribution measuring device, for example, Mastersizer 2000 manufactured by Sysmex. Specifically, the volume average particle size is the central particle size (D50) under the volume particle size distribution of a dispersion obtained by mixing and dispersing silica particles, water (dispersion medium) and a nonionic surfactant (Igepal CA630; dispersant).

[0060] Examples of the silica-containing fibrous substrate include glass fibers such as long glass fibers (glass fibers) and short glass fibers (glass wool), and silica nanofibers. The glass fibers are preferably made of alkali-free glass (E glass).

[0061] The diameter of the glass fiber is not particularly limited, but is preferably 1 μm to 100 μm, and more preferably 5 μm to 50 μm.

[0062] The fiber length of the glass long fibers is not particularly limited, but the fiber length of the glass short fibers is preferably 0.1 mm to 30 mm, more preferably 0.2 mm to 20 mm.

[0063] The diameter of the glass fiber refers to the number average fiber diameter which represents the average value of the diameters of the glass fibers. The number average fiber diameter is the arithmetic mean value when 50 glass fibers are randomly selected and the fiber diameters are measured using an optical microscope.

[0064] The fiber length of the glass short fibers is a value obtained by visually measuring the length of each of 100 randomly selected fibers to the unit of 0.1 mm and calculating the length as the arithmetic mean.

[0065] Examples of the thin film substrate containing silicon dioxide include flaky glass particles and the like.

[0066] The volume average particle size of the flaky glass particles is preferably 0.1 μm to 200 μm, more preferably 0.2 μm to 150 μm, and even more preferably 0.2 μm to 100 μm. The volume average particle size of the flaky glass particles can be measured in the same manner as the volume average particle size of the silica particles.

[0067] The average thickness of the flaky glass particles is preferably 1 to 20 μm, more preferably 1.5 to 15 μm, and even more preferably 2 to 10 μm. The average thickness of the flaky glass particles refers to the arithmetic mean of the thicknesses of 50 randomly selected glass particles from 100 randomly selected glass particles and measured using an optical microscope.

[0068] The ratio of the average thickness of the flaky glass particles to the volume average particle diameter (aspect ratio: volume average particle diameter / average thickness) is preferably 1.2 to 2000, more preferably 1.5 to 1500, and further preferably 2 to 1000. The aspect ratio of the flaky glass particles can be calculated as the ratio of the volume average particle diameter to the average thickness of the flaky glass particles obtained by the above method.

[0069] In addition to the above-mentioned film-like substrate, a plate-like substrate containing silicon dioxide may be used. Examples of the plate-like substrate include a glass plate and the like.

[0070] As the substrate, from the viewpoint of processability to an electrolyte membrane or the like, silica particles or glass fibers are preferred, and silica particles are more preferred.

[0071] (Sulfonic acid group)

[0072] In the first silica material of the present disclosure, the base has a sulfonic acid group on at least the surface thereof. The sulfonic acid group may be chemically bonded to the surface of the base.

[0073] Whether or not at least the surface of the substrate has sulfonic acid groups can be confirmed by, for example, the following method.

[0074] X-ray Photoelectron Spectroscopy (XPS) and X-ray Fluorescence (XRF) are used to confirm whether sulfur atoms exist in the silica material and to quantify the amount of sulfur atoms. Scanning Electron Microscope-Energy Dispersive X-ray Spectrometry (SEM-EDX) is used to confirm whether sulfur atoms exist on the surface of the silica material.

[0075] Separately, 0.1 g of a silica material was dispersed in 1.9 g of deionized water, and the pH of the dispersion (5% by mass dispersion) was measured at 25°C.

[0076] If sulfur atoms exist on the surface of the silica material and the pH of the dispersion is 3 or less, it can be determined that the substrate has sulfonic acid groups on at least the surface.

[0077] In one embodiment, the ratio of sulfur atoms to silicon atoms (S / Si) contained in the silica material of the present disclosure is preferably 0.001 to 0.25, more preferably 0.0015 to 0.2, and even more preferably 0.002 to 0.15.

[0078] In another embodiment, the ratio of sulfur atoms to silicon atoms (S / Si) contained in the silica material of the present disclosure is preferably 0.001 to 0.72, more preferably 0.0015 to 0.67, and even more preferably 0.002 to 0.62. The amounts of sulfur atoms and silicon atoms contained in the silica material for calculating the ratio of sulfur atoms to silicon atoms (S / Si) are determined by XPS measurement.

[0079] In one embodiment, the concentration of sulfur atoms contained in the silica material of the present disclosure is preferably 50 mg / kg to 250 g / kg, more preferably 150 mg / kg to 200 g / kg, and even more preferably 300 mg / kg to 150 g / kg.

[0080] In another embodiment, the concentration of sulfur atoms contained in the silica material of the present disclosure is preferably 50 mg / kg to 50 g / kg, more preferably 150 mg / kg to 30 g / kg, and even more preferably 300 mg / kg to 20 g / kg.

[0081] It should be noted that the concentration of sulfur atoms contained in the silica material refers to the amount of atoms present determined by XRF measurement.

[0082] The sulfonation degree (XRF-based sulfonation degree) of the silica material disclosed herein is preferably 0.01% to 90%, more preferably 0.03% to 80%, and further preferably 0.06% to 60%. The XRF-based sulfonation degree is a value obtained as a ratio of the concentration of sulfur atoms obtained by XRF measurement to the total concentration of silicon atoms and the concentration of sulfur atoms.

[0083] (Method for producing silicon dioxide material)

[0084] In the first silica material of the present disclosure, sulfonic acid groups are present on at least the surface of the substrate. The method for making sulfonic acid groups present on at least the surface of the substrate (i.e., the method for producing the first silica material of the present disclosure) is not particularly limited. For example, the first silica material of the present disclosure can be produced by bringing a sulfonating agent into contact with the substrate.

[0085] The method of bringing the substrate into contact with the sulfonating agent is not particularly limited, and examples thereof include a method of immersing the substrate in the sulfonating agent and a method of spraying the sulfonating agent onto the substrate.

[0086] The temperature of the sulfonating agent when the sulfonating agent is brought into contact with the substrate is preferably 10°C to 90°C, more preferably 15°C to 80°C, and further preferably 20°C to 70°C.

[0087] The immersion time when the substrate is immersed in the sulfonating agent is preferably 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and even more preferably 15 minutes to 60 minutes.

[0088] When the substrate is immersed in the sulfonating agent, the ratio of the substrate to the sulfonating agent is preferably 1,000 to 50,000 parts by mass, more preferably 2,000 to 30,000 parts by mass, and even more preferably 3,000 to 20,000 parts by mass, based on 100 parts by mass of the substrate.

[0089] When the substrate is immersed in the sulfonating agent, stirring treatment may be performed. The stirring method is not particularly limited, and examples thereof include stirring using a stirring blade, stirring using a stirring device having a planetary rotating mechanism, etc. By using a stirring device having a planetary rotating mechanism, the presence of bubbles can be effectively removed.

[0090] After the sulfonating agent is brought into contact with the substrate, the substrate may be washed with ion exchange water, deionized water or the like and filtered, and further washed with an organic solvent such as acetone and filtered as necessary, and the substrate may be dried to obtain the first silica material.

[0091] The second silica material of the present disclosure is obtained by bringing a sulfonating agent into contact with a substrate containing silica. The second silica material of the present disclosure can be produced by the same method as the first silica material of the present disclosure described above.

[0092] Examples of the sulfonating agent include fuming sulfuric acid, concentrated sulfuric acid, dilute sulfuric acid, anhydrous sulfuric acid, and the like. Fuming sulfuric acid or concentrated sulfuric acid is preferred, and fuming sulfuric acid is more preferred.

[0093] The concentration of sulfur trioxide in fuming sulfuric acid is preferably 10% by mass to 80% by mass, more preferably 15% by mass to 75% by mass, and still more preferably 20% by mass to 70% by mass.

[0094] <Ion exchange resin composition>

[0095] The ion exchange resin composition of the present disclosure contains the silica material of the present disclosure and an ion exchange resin. The ion exchange resin composition of the present disclosure may contain other components as needed.

[0096] The silica material of the present disclosure is as described above, and thus the description thereof is omitted here.

[0097] The ion exchange group contained in the ion exchange resin is not particularly limited, and examples thereof include a sulfonic acid group, a carboxyl group, a quaternary ammonium group, or a primary, secondary or tertiary amino group.

[0098] Among them, a sulfonic acid group having excellent proton conductivity is preferred.

[0099] The type of ion exchange resin contained in the ion exchange resin composition of the present disclosure is not particularly limited.

[0100] Examples of the aromatic ion exchange resin include sulfonates of aromatic polymers such as polyphenylene, polyphenylene sulfide, polyphenylene ether, diphenyl-p-phenylene ether, polysulfone, polyethersulfone, polyetherketone, polyetheretherketone, polyetherketoneketone, polyethernitrile, polyamide, polybenzazole, and polyimide.

[0101] More specifically, there can be mentioned sulfonated products of polyphenylene containing a structural unit represented by the general formula (I), sulfonated products of polyphenylene sulfide containing a structural unit represented by the general formula (II), sulfonated products of polyphenylene ether containing a structural unit represented by the general formula (III), sulfonated products of polydiphenylene oxide containing a structural unit represented by the general formula (IV), sulfonated products of polysulfone containing a structural unit represented by the general formula (V), sulfonated products of polyethersulfone containing a structural unit represented by the general formula (VI), and sulfonated products of polyethersulfone containing a structural unit represented by the general formula (VII). sulfonated products of polyether ketones containing structural units represented by the general formula (VIII), sulfonated products of polyether ether ketones containing structural units represented by the general formula (IX), sulfonated products of polyether nitrile containing structural units represented by the general formula (X), sulfonated products of polyamide containing structural units represented by the general formula (XI), sulfonated products of polybenzoxazole containing structural units represented by the general formula (XII), and sulfonated products of polyimide containing structural units represented by the general formula (XIII).

[0102] Among them, preferred are sulfonates of polyethersulfones containing a structural unit represented by the general formula (VI), sulfonates of polyphenylene sulfide containing a structural unit represented by the general formula (II), and sulfonates of polysulfones containing a structural unit represented by the general formula (V), and more preferred are sulfonates of polyethersulfones containing a structural unit represented by the general formula (VI).

[0103] In the present disclosure, two or more ion exchange resins may be used in combination. When two or more ion exchange resins are used in combination, for example, a sulfonated product of polyethersulfone containing a structural unit represented by general formula (VI) and a sulfonated product of a resin other than the polyethersulfone may be used in combination.

[0104] In the general formulae (I) to (XIII), n represents an integer of 1 or 2 or more.

[0105]

[0106]

[0107] The sulfonation rate of the aromatic ion exchange resin is preferably 5 mol% to 90 mol%, more preferably 8 mol% to 80 mol%, and further preferably 10 mol% to 70 mol%.

[0108] In the present disclosure, the sulfonation rate of the aromatic ion exchange resin refers to the ratio of the structural units substituted with sulfonic acid groups to the total structural units contained in the aromatic ion exchange resin.

[0109] Examples of the fluorine-based ion exchange resin include perfluorosulfonic acid electrolyte polymers such as Nafion (registered trademark), Aciplex (registered trademark), Flemion (registered trademark), Aquivion, and GoreSelect.

[0110] Alternatively, an electrolyte membrane may be prepared by combining a reinforcing material such as a polyethylene porous membrane such as Mirime (registered trademark), an ion exchange resin, and the silica material disclosed herein.

[0111] The EW of the ion exchange resin is preferably 200 or more, more preferably 250 or more, further preferably 300 or more, and particularly preferably 350 or more. In addition, the EW is preferably 2600 or less, more preferably 2300 or less, further preferably 2000 or less, and particularly preferably 1700 or less. By setting the EW to 2600 or less, an electrolyte membrane with excellent power generation performance can be obtained, and by setting the EW to 250 or more, an electrolyte membrane with excellent mechanical strength can be obtained. In addition, the EW of the ion exchange resin is preferably 200 to 2600.

[0112] The EW of the acidic ion exchange resin is measured by the following method.

[0113] About 0.02g to 0.10g of ion exchange resin is immersed in 50mL of 25℃ saturated NaCl aqueous solution (0.26g / mL), and after being left for 10 minutes while stirring, neutralization titration is performed using Fujifilm Wako Pure Chemical Industries, Ltd. special grade phenolphthalein as an indicator and a special grade 0.01N sodium hydroxide aqueous solution as a reagent manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. The Na-type ion exchange membrane obtained after neutralization is rinsed with pure water, vacuum dried and weighed. The equivalent amount of sodium hydroxide required for neutralization is set as M (mmol), and the mass of the Na-type ion exchange membrane is set as W (mg), and the equivalent mass EW (g / eq) is calculated according to the following formula.

[0114] EW=(W / M)-22

[0115] If an ion exchange resin containing fluorine atoms in its molecular structure is used to make an electrolyte membrane, fluoric acid may be generated due to the decomposition of the ion exchange resin when the electrolyte membrane works as a solid polymer electrolyte membrane, etc. Therefore, as the ion exchange resin, an ion exchange resin containing no fluorine atoms in its molecular structure or having a fluorine atom content of 50% by mass or less is preferred.

[0116] The ion exchange resin composition of the present disclosure may be used together with an ion exchange resin and other resins having low or no ion exchange energy (hereinafter sometimes referred to as non-ion exchange resins). In the present disclosure, non-ion exchange resins refer to resins having an EW of 10,000 or more.

[0117] Specific examples of the non-ion exchange resin include resins containing structural units represented by the above-mentioned general formulae (I) to (XIII).

[0118] When the ion exchange resin composition of the present disclosure contains an ion exchange resin and a non-ion exchange resin, the content ratio of the ion exchange resin to the non-ion exchange resin is not particularly limited. For example, the content ratio of the ion exchange resin to the non-ion exchange resin can be adjusted so that the EW of the mixture of the ion exchange resin and the non-ion exchange resin becomes a desired value.

[0119] The EW of the mixture of the ion exchange resin and the non-ion exchange resin is preferably 200 or more, more preferably 250 or more, further preferably 300 or more, and particularly preferably 350 or more. In addition, the EW is preferably 2600 or less, more preferably 2300 or less, further preferably 2000 or less, and particularly preferably 1700 or less. By setting the EW to be 2600 or less, an electrolyte membrane with excellent power generation performance can be obtained, and by setting the EW to be 250 or more, an electrolyte membrane with excellent mechanical strength can be obtained. In addition, the EW of the mixture of the ion exchange resin and the non-ion exchange resin is preferably 200 to 2600.

[0120] In one embodiment, the mass-based content of the ion exchange resin in the mixture of the ion exchange resin and the non-ion exchange resin is preferably 1 to 95% by mass, more preferably 5 to 90% by mass, and even more preferably 10 to 80% by mass.

[0121] In a certain embodiment, the sulfonation rate of the mixture of the ion exchange resin and the non-ion exchange resin is preferably 5 mol% to 90 mol%, more preferably 8 mol% to 80 mol%, and even more preferably 10 mol% to 70 mol%.

[0122] In the present disclosure, the sulfonation rate of a mixture of an ion exchange resin and a non-ion exchange resin when both the ion exchange resin and the non-ion exchange resin are aromatic refers to the ratio of the structural units substituted with sulfonic acid groups to all the structural units contained in the ion exchange resin and the non-ion exchange resin.

[0123] The sulfonation rate of the ion exchange resin (a mixture of the ion exchange resin and the non-ion exchange resin when both the ion exchange resin and the non-ion exchange resin are aromatic) refers to a value obtained from the ratio of structural units having a sulfonic acid group to structural units not having a sulfonic acid group measured by proton NMR measurement.

[0124] When the types and molecular weights (e.g., weight average molecular weight) of the structural units constituting the ion exchange resin and the non-ion exchange resin in the mixture and the sulfonation rate of the ion exchange resin are known, the sulfonation rate calculated based on these values ​​is used as the sulfonation rate of the mixture.

[0125] It should be noted that the durability of the ion exchange resin sometimes decreases as the sulfonation rate increases. Therefore, when using an ion exchange resin with a relatively low sulfonation rate, it is not necessary to use it in combination with a non-ion exchange resin. In addition, when an ion exchange resin with a relatively low sulfonation rate and a non-ion exchange resin are used in combination, the mass-based content of the ion exchange resin in the mixture of the ion exchange resin and the non-ion exchange resin can be relatively high.

[0126] On the other hand, when an ion exchange resin having a relatively high sulfonation rate is used, it is preferred to use the ion exchange resin and a non-ion exchange resin in combination.

[0127] For example, when a sulfonated product of polyethersulfone having a sulfonation rate of 1 to 20 mol % (preferably 3 to 18 mol %, more preferably 5 to 15 mol %) is used as the ion exchange resin, the sulfonated product of polyethersulfone may be used alone as the ion exchange resin.

[0128] On the other hand, when a sulfonated product of polyethersulfone having a sulfonation rate of more than 20 mol% and less than 60 mol% (preferably 25 mol% to 50 mol%, more preferably 30 mol% to 45 mol%) is used as the ion exchange resin, it is preferred to use the sulfonated product of polyethersulfone and a non-ion exchange resin together as the ion exchange resin from the viewpoint of durability of the electrolyte membrane. In this case, the mass-based content of the ion exchange resin in the mixture of the ion exchange resin and the non-ion exchange resin is preferably 10 mass% to 95 mass%, more preferably 20 mass% to 90 mass%, and further preferably 25 mass% to 85 mass%.

[0129] From the viewpoint of durability and mechanical properties of the electrolyte membrane, the weight average molecular weight (Mw) of the ion exchange resin is preferably 30,000 to 1,000,000, more preferably 35,000 to 800,000, and even more preferably 40,000 to 500,000.

[0130] From the viewpoint of durability of the electrolyte membrane, the weight average molecular weight of the non-ion exchange resin is preferably 30,000 to 1,000,000, more preferably 50,000 to 800,000, and even more preferably 80,000 to 500,000.

[0131] From the viewpoint of durability of the electrolyte membrane, the weight average molecular weight of the mixture of the ion exchange resin and the non-ion exchange resin is preferably 50,000 to 800,000, more preferably 80,000 to 650,000, and even more preferably 100,000 to 500,000.

[0132] In the present disclosure, the weight average molecular weight of a resin refers to a value measured by gel permeation chromatography (GPC).

[0133] In the ion exchange resin composition of the present invention, the content of the silica material of the present invention in the solid content of the ion exchange resin composition is preferably 0.01% by mass to 90% by mass, more preferably 0.1% by mass to 80% by mass, further preferably 0.5% by mass to 60% by mass, and particularly preferably 0.7% by mass to 50% by mass. If the content of the silica particles is within the above range, the film-forming property of the ion exchange resin composition is improved.

[0134] The ion exchange resin composition of the present disclosure can be used as an electrolyte membrane, a binder within an electrode, an acid catalyst in a chemical process, and the like.

[0135] <Electrolyte membrane>

[0136] The electrolyte membrane of the present disclosure contains the ion exchange resin composition of the present disclosure. The electrolyte membrane of the present disclosure may further contain other components as required.

[0137] The ion exchange resin composition of the present disclosure is as described above, and therefore the description in this item is omitted.

[0138] The thickness of the electrolyte membrane may be 0.1 μm to 300 μm, preferably 1 μm to 200 μm, more preferably 2 μm to 150 μm, and further preferably 3 μm to 50 μm.

[0139] The method for producing the electrolyte membrane is not particularly limited.

[0140] For example, it can be formed by applying a liquid composition containing an ion exchange resin, the silica material of the present disclosure, and a solvent onto a substrate, an anode or a cathode described later, and drying the composition.

[0141] As the solvent, a solvent that can dissolve or disperse the ion exchange resin can be used, for example, alcohols such as methanol, ethanol, n-propanol, isopropanol, tert-butanol, glycol solvents such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, aprotic solvents such as dimethyl sulfoxide, N,N-dimethylacetamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, fluorinated alcohols, fluorinated ethers, etc.

[0142] Examples of the substrate to be coated include plastic films such as Teflon (registered trademark), polyester, polyimide, and polycarbonate, metal films such as aluminum, copper, iron, and stainless steel, glass, and the gas diffusion layer (GDL) described below.

[0143] As the coating method of the liquid composition, for example, there are a doctor blade method, a rod coating method, a spin coating method, a screen printing method, etc. as a batch method, and a post-metering method and a front-metering method as a continuous method can be cited. The post-metering method is a method of applying an excessive amount of coating liquid and then removing the coating liquid in a manner to obtain a specified film thickness. The front-metering method is a method of applying a coating liquid for obtaining the amount required for a specified film thickness. As the post-metering method, an air knife coating method, a flat plate coating method, a rod coating method, a doctor blade coating method, an extrusion coating method, an impregnation coating method, a comma coating method, etc. can be cited, and as the front-metering method, a die coating method, a reverse roll coating method, a transfer roll coating method, a gravure coating method, a kiss roll coating method, a cast coating method, a spray coating method, a curtain coating method, a calender coating method (kalendacoder method), an extrusion coating method, etc. can be cited.

[0144] <Membrane electrode assembly>

[0145] The membrane electrode assembly disclosed in the present invention comprises: the electrolyte membrane disclosed in the present invention, a cathode laminated on one surface of the electrolyte membrane, and an anode laminated on the other surface of the electrolyte membrane. The disclosed membrane electrode assembly may also have other structures in addition to the electrolyte membrane, the anode and the cathode. For example, a gas diffusion layer may also be arranged on the surface of the electrolyte membrane opposite to the cathode and on the surface of the electrolyte membrane opposite to the anode.

[0146] The membrane electrode assembly disclosed herein is suitable for use in a solid polymer fuel cell or a solid polymer electrolysis device.

[0147] As a method for manufacturing a membrane electrode assembly, for example, the following methods can be cited: (1) a method in which a coating liquid containing an ion exchange resin or an ion exchange resin composition, a catalyst metal and a solvent is prepared and the coating liquid is directly applied to an electrolyte membrane, and then the solvent contained in the coating liquid is removed by drying to form a catalyst layer, and the catalyst layer is sandwiched from both sides by gas diffusion layers; (2) a method in which the coating liquid is applied to a substrate as a gas diffusion layer, the catalyst layer is dried, and the catalyst layer is bonded to an electrolyte membrane by a method such as heat pressing; (3) a method in which the coating liquid is applied to a membrane (substrate) that exhibits sufficient stability to the solvent contained in the coating liquid, the catalyst layer is dried, the catalyst layer is heat pressed on the electrolyte membrane, and then the substrate membrane is peeled off to sandwich the gas diffusion layer. As the ion exchange resin and ion exchange resin composition contained in the coating liquid, it is preferable to use the same ion exchange resin and ion exchange resin composition as the ion exchange resin composition constituting the electrolyte membrane.

[0148] When the membrane electrode assembly disclosed in the present invention is used in a solid polymer fuel cell, the gas diffusion layer is responsible for supplying hydrogen and air as fuel to the electrode, collecting electrons generated by chemical reactions in the electrode, and moisturizing the electrolyte membrane. As the gas diffusion layer, conventionally known materials such as carbon paper and carbon cloth that are excellent in air permeability, acid resistance, conductivity, and mechanical strength can be used. In addition, in order to promote the discharge of water and moisturizing of the gas diffusion layer, it is also preferable to use a material that configures a microporous layer on the surface of the gas diffusion layer on the electrode side.

[0149] When the membrane electrode assembly disclosed in the present invention is used in a solid polymer electrolysis device, a previously known material composed of a carbon material such as carbon paper or carbon cloth, stainless steel (Fe-Cr alloy, Fe-Ni-Cr alloy, etc.), a metal material such as aluminum, zinc, nickel or titanium can be used as the gas diffusion layer.

[0150] When the membrane electrode assembly disclosed in the present invention is used in a solid polymer fuel cell, the catalyst contained in the catalyst layer may be the same or different on the anode side (hydrogen electrode) and the cathode side (air electrode), and preferably a metal catalyst composed of platinum or a platinum alloy is supported on carbon. In order to make the metal catalyst well dispersed and supported on the carbon carrier, the activity of the electrode reaction is excellent for a long-term stable state, and the carbon used as the carrier preferably has a specific surface area of ​​50 m 2 / g~2000m 2 / g.

[0151] As a metal catalyst, since it is highly active relative to the hydrogen oxidation reaction at the anode in the solid polymer fuel cell and the oxygen reduction reaction at the cathode, a metal catalyst preferably composed of platinum is preferred. Since stability and activity as an electrode catalyst can also be further given sometimes, a metal catalyst preferably composed of a platinum catalyst is also preferred. As the above-mentioned platinum alloy, it is preferably selected from an alloy of one or more metals and platinum in a platinum-based metal (ruthenium, rhodium, palladium, osmium, iridium), gold, silver, chromium, iron, titanium, manganese, cobalt, nickel, molybdenum, tungsten, aluminum, silicon, zinc and tin other than platinum, and the platinum alloy may contain a metal alloyed with platinum and an intermetallic compound of platinum. When a gas containing carbon monoxide is supplied to the anode, if an alloy containing platinum and ruthenium is used, the activity of the catalyst is stable, and thus preferred.

[0152] When the membrane electrode assembly of the present disclosure is used in a solid polymer electrolysis device, a metal catalyst composed of platinum or a platinum alloy is preferably supported on carbon on the cathode side (hydrogen electrode). On the other hand, iridium, platinum, etc. can be used as a catalyst on the anode side (air electrode side).

[0153] <Solid polymer fuel cells, solid polymer electrolyzers, and electrochemical hydrogen compression devices>

[0154] The electrolyte membrane disclosed in the present invention can be used in solid polymer fuel cells, solid polymer electrolysis devices, electrochemical hydrogen compression devices, and the like.

[0155] In a solid polymer electrolysis device, water or an organic solvent can be electrolyzed to produce hydrogen or the like.

[0156] The polymer electrolyte fuel cell and polymer electrolyte electrolysis device disclosed herein include the membrane electrode assembly disclosed herein and separators disposed on both surfaces of the membrane electrode assembly.

[0157] A cell having a separator disposed outside the membrane electrode assembly of the present disclosure can be used as a single cell, or a plurality of cells can be stacked with a cooling plate or the like to form a polymer electrolyte fuel cell or a polymer electrolyte electrolysis device.

[0158] As the separator, since it blocks the fuel and air between the polymer electrolyte fuel cell stacks or the polymer electrolyte electrolyzer stacks and configures the fuel flow path, conventionally known carbon materials, stainless steel and other metal materials can be used.

[0159] In addition, the electrochemical hydrogen compression device of the present disclosure has the electrolyte membrane of the present disclosure.

[0160] The electrochemical hydrogen compression device disclosed in the present invention may, for example, include: the electrolyte membrane disclosed in the present invention, a cathode arranged on one surface of the electrolyte membrane, an anode arranged on the other surface of the electrolyte membrane, an anode supply path for supplying a gas containing hydrogen to the anode, a cathode discharge path for taking out the purified hydrogen gas generated by the cathode, and a power supply for applying voltage to the anode and the cathode.

[0161] Example

[0162] The following examples are given to further illustrate the silica material, ion exchange resin composition and electrolyte membrane of the present disclosure. The materials, usage amounts, proportions, processing steps, etc. shown in the following examples can be appropriately changed as long as they do not deviate from the main purpose of the present disclosure. Therefore, the scope of the silica material, ion exchange resin composition and electrolyte membrane of the present disclosure should not be interpreted as being limited to the specific examples shown below.

[0163] <Example 1A>

[0164] (Manufacturing of silicon dioxide materials)

[0165] 10 parts by mass of silica (manufactured by Sigma-Aldrich, number average particle size of primary particles: 10 nm to 20 nm, silica particles) were added little by little to 400 parts by mass of fuming sulfuric acid (sulfur trioxide concentration: 24% by mass) at 25°C, and stirred with a stirring blade for 10 minutes. The obtained dispersion was added little by little to 4000 parts by mass of deionized water, washed, filtered, and the silica particles obtained as the filtrate were recovered. The recovered silica particles were further washed and filtered with 1000 parts by mass of deionized water, and the filtrate was recovered. The obtained filtrate was washed with 200 parts by mass of acetone and filtered again. The filtrate was dried in a hot air dryer at 80°C to obtain 8.6 parts by mass of silica material A. The sulfonation degree based on XRF of the silica material A was measured according to the method described below, and the result was 0.2%. The pH of the dispersion of the silica material A was measured according to the method described below, and the result was 1.5.

[0166] The pH of the dispersion of silica (manufactured by Sigma-Aldrich, volume average particle size: 10 nm to 20 nm, silica particles) was measured by the method described below and was 4.5. The degree of sulfonation by XRF was measured by the method described below and was 0%.

[0167] <Example 2A>

[0168] (Manufacturing of Electrolyte Membrane 1A)

[0169] 35 parts by mass of N-methyl-2-pyrrolidone (NMP) were added to 15 parts by mass of sulfonated polyethersulfone (s-PES, EW: 1600 g / eq, weight average molecular weight: 50000) having a sulfonation rate of 13.1 mol%, and the mixture was treated at 3500 rpm for 15 minutes using a SpeedMixer DAC150 manufactured by Hauschild, thereby obtaining an NMP solution (stock solution) of s-PES. The silica material A obtained in Example 1A was added thereto in an amount such that the content of the silica material A in the solid content of the ion exchange resin composition was 1.0 mass%, thereby preparing a stock solution in which the silica material A was dispersed.

[0170] The obtained stock solution was degassed with a vacuum pump and then applied to a glass substrate, and cast using a scraper set to 700 μm. The glass substrate was placed in a hot air dryer set to 80° C. and dried for 1 hour to obtain a dry film. The obtained dry film was immersed in ion exchange water, thereby peeling the electrolyte membrane 1A composed of the ion exchange resin composition from the glass substrate. The obtained electrolyte membrane 1A was stored in a state immersed in deionized water.

[0171] <Example 3A>

[0172] An electrolyte membrane 2A was obtained in the same manner as in Example 2A except that the silica material A was added to the NMP solution (stock solution) of s-PES in an amount such that the content of the silica material A in the solid content of the ion exchange resin composition was 2.9 mass %.

[0173] <Example 4A>

[0174] An electrolyte membrane 3A was obtained in the same manner as in Example 2A except that the silica material A was added to the NMP solution (stock solution) of s-PES in such an amount that the content of the silica material A in the solid content of the ion exchange resin composition was 4.8 mass %.

[0175] <Example 5A>

[0176] An electrolyte membrane 4A was obtained in the same manner as in Example 2A except that the silica material A was added to the NMP solution (stock solution) of s-PES in an amount such that the content of the silica material A in the solid content of the ion exchange resin composition was 9.0 mass %.

[0177] <Example 6A>

[0178] An electrolyte membrane 5A was obtained in the same manner as in Example 2A except that the silica material A was added to the NMP solution (stock solution) of s-PES in such an amount that the content of the silica material A in the solid content of the ion exchange resin composition became 23.1% by mass.

[0179] <Example 7A>

[0180] An electrolyte membrane 6A was obtained in the same manner as in Example 2A except that the silica material A was added to the NMP solution (stock solution) of s-PES in an amount such that the content of the silica material A in the solid content of the ion exchange resin composition was 33.3 mass %.

[0181] <Example 8A>

[0182] An electrolyte membrane 7A was obtained in the same manner as in Example 2A except that the silica material A was added to the NMP solution (stock solution) of s-PES in an amount such that the content of the silica material A in the solid content of the ion exchange resin composition was 47.4 mass %.

[0183] <Reference Example 1A>

[0184] A reference electrolyte membrane 1A not containing the silica material A was obtained in the same manner as in Example 2A except that the NMP solution (stock solution) of s-PES was used.

[0185] <Comparative Example 1A>

[0186] A comparative electrolyte membrane 1A was obtained in the same manner as in Example 2A except that silica particles were added to the NMP solution (stock solution) of s-PES in an amount such that the content of silica particles (Silicon dioxide) in the solid content of the ion exchange resin composition was 1.0 mass %.

[0187] <Comparative Example 2A>

[0188] A comparative electrolyte membrane 2A was obtained in the same manner as in Example 2A except that silica particles were added to the NMP solution (stock solution) of s-PES in an amount such that the content of silica particles (Silicon dioxide) in the solid content of the ion exchange resin composition was 2.9 mass %.

[0189] <Comparative Example 3A>

[0190] A comparative electrolyte membrane 3A was obtained in the same manner as in Example 2A except that silica particles were added to the NMP solution (stock solution) of s-PES in an amount such that the content of silica particles (Silicon dioxide) in the solid content of the ion exchange resin composition was 4.8 mass %.

[0191] <Comparative Example 4A>

[0192] A comparative electrolyte membrane 4A was obtained in the same manner as in Example 2A except that silica particles were added to the NMP solution (stock solution) of s-PES in an amount such that the content of silica particles (Silicon dioxide) in the solid content of the ion exchange resin composition was 9.0 mass %.

[0193] <Comparative Example 5A>

[0194] A comparative electrolyte membrane 5A was obtained in the same manner as in Example 2A except that silica particles were added to the NMP solution (stock solution) of s-PES in an amount such that the content of silica particles (Silicon dioxide) in the solid content of the ion exchange resin composition was 23.1 mass %.

[0195] <Comparative Example 6A>

[0196] Comparative electrolyte membrane 6A was obtained in the same manner as in Example 2A except that silica particles were added to the NMP solution (stock solution) of s-PES in an amount such that the content of silica particles in the solid content of the ion exchange resin composition was 33.3 mass %. However, no membrane was formed.

[0197] <Comparative Example 7A>

[0198] Comparative electrolyte membrane 7A was obtained in the same manner as in Example 2A except that silica particles were added to the NMP solution (stock solution) of s-PES in an amount such that the content of silica particles in the solid content of the ion exchange resin composition was 47.4 mass %. However, no membrane was formed.

[0199] <Example 1B>

[0200] 10 parts by mass of silica (manufactured by Sigma-Aldrich, number average particle size of primary particles: 10 nm to 20 nm, silica particles) were added little by little to 400 parts by mass of concentrated sulfuric acid (concentration: 99.9%) at 25°C, and treated at 1500 rpm for 15 minutes using SpeedMixer DAC400 manufactured by Hauschild, thereby obtaining a dispersion in which silica particles were dispersed in concentrated sulfuric acid. The obtained dispersion was added little by little to 4000 parts by mass of deionized water, filtered after washing, and the silica particles obtained as the filtrate were recovered. The recovered silica particles were further washed and filtered with 4000 parts by mass of deionized water, and the filtrate was recovered. The obtained filtrate was washed with 200 parts by mass of acetone and filtered again. The filtrate was dried in a hot air dryer at 80°C to obtain 14.5 parts by mass of silica material B. The degree of sulfonation of the silica material B based on XRF was measured according to the method described later, and the result was 0.3%. The pH of the dispersion of the silica material B was measured by the method described below and found to be 1.2.

[0201] <Example 2B>

[0202] 35 parts by mass of N-methyl-2-pyrrolidone (NMP) were added to 15 parts by mass of sulfonated polyethersulfone (s-PES, EW: 500 g / eq, weight average molecular weight: 140000) having a sulfonation rate of 34.1 mol%, and the mixture was treated at 3500 rpm for 15 minutes using a SpeedMixer DAC150 manufactured by Hauschild, thereby obtaining an NMP solution (stock solution) of s-PES. The silica material B obtained in Example 1B was added thereto in an amount such that the content of the silica material B in the solid content of the ion exchange resin composition was 10.0% by mass, thereby preparing a stock solution in which the silica material B was dispersed.

[0203] The obtained stock solution was degassed with a vacuum pump and then applied to a glass substrate, and cast using a scraper set to 700 μm. The glass substrate was placed in a hot air dryer set to 80°C and dried for 1 hour to obtain a dry film. The obtained dry film was immersed in ion exchange water, thereby peeling the electrolyte membrane 1B composed of the ion exchange resin composition from the glass substrate. The obtained electrolyte membrane 1B was stored in a state immersed in deionized water.

[0204] <Example 3B>

[0205] 3.0 parts by mass of polyethersulfone (PES, EW: 10000 g / eq or more, weight average molecular weight: 200000) manufactured by Solvay and 35 parts by mass of N-methyl-2-pyrrolidone (NMP) were added to 12.0 parts by mass of sulfonated polyethersulfone (s-PES, EW: 500 g / eq, weight average molecular weight: 140000) having a sulfonation rate of 34.1 mol%, and treated at 3500 rpm for 15 minutes using SpeedMixer DAC150 manufactured by Hauschild to obtain an NMP solution (stock solution) of s-PES and PES. The silica material B obtained in Example 1B was added thereto in an amount such that the content of the silica material B in the solid content of the ion exchange resin composition was 10.0% by mass, thereby preparing a stock solution in which the silica material B was dispersed.

[0206] The obtained stock solution was degassed with a vacuum pump and then applied to a glass substrate, and cast using a scraper set to 700 μm. The glass substrate was placed in a hot air dryer set to 80°C and dried for 1 hour to obtain a dry film. The obtained dry film was immersed in ion exchange water, thereby peeling the electrolyte membrane 2B composed of the ion exchange resin composition from the glass substrate. The obtained electrolyte membrane 2B was stored in a state immersed in deionized water.

[0207] <Example 4B>

[0208] 6.0 parts by mass of polyethersulfone (PES) manufactured by Solvay and 35 parts by mass of N-methyl-2-pyrrolidone (NMP) were added to 9.0 parts by mass of sulfonated polyethersulfone (s-PES, EW: 500 g / eq) having a sulfonation rate of 34.1 mol%, and the mixture was treated at 3500 rpm for 15 minutes using a SpeedMixer DAC150 manufactured by Hauschild, thereby obtaining an NMP solution (stock solution) of s-PES and PES. The silica material B obtained in Example 1B was added thereto in an amount such that the content of the silica material B in the solid content of the ion exchange resin composition was 10.0% by mass, thereby preparing a stock solution in which the silica material B was dispersed.

[0209] An electrolyte membrane 3B was obtained in the same manner as in Example 3B except that the obtained stock solution was used.

[0210] <Example 5B>

[0211] 9.0 parts by mass of polyethersulfone (PES) manufactured by Solvay and 35 parts by mass of N-methyl-2-pyrrolidone (NMP) were added to 6.0 parts by mass of sulfonated polyethersulfone (s-PES, EW: 500 g / eq) having a sulfonation rate of 34.1 mol%, and the mixture was treated at 3500 rpm for 15 minutes using a SpeedMixer DAC150 manufactured by Hauschild, thereby obtaining an NMP solution (stock solution) of s-PES and PES. The silica material B obtained in Example 1B was added thereto in an amount such that the content of the silica material B in the solid content of the ion exchange resin composition was 10.0% by mass, thereby preparing a stock solution in which the silica material B was dispersed.

[0212] An electrolyte membrane 4B was obtained in the same manner as in Example 3B except that the obtained stock solution was used.

[0213] <Example 6B>

[0214] 12.0 parts by mass of polyethersulfone (PES) manufactured by Solvay and 35 parts by mass of N-methyl-2-pyrrolidone (NMP) were added to 3.0 parts by mass of sulfonated polyethersulfone (s-PES, EW: 500 g / eq) having a sulfonation rate of 34.1 mol%, and the mixture was treated at 3500 rpm for 15 minutes using a SpeedMixer DAC150 manufactured by Hauschild, thereby obtaining an NMP solution (stock solution) of s-PES and PES. The stock solution in which the silica material B was dispersed was prepared by adding the silica material B obtained in Example 1B in an amount such that the content of the silica material B in the solid content of the ion exchange resin composition was 10.0% by mass.

[0215] An electrolyte membrane 5B was obtained in the same manner as in Example 3B except that the obtained stock solution was used.

[0216] <Reference Example 1B>

[0217] 35 parts by mass of N-methyl-2-pyrrolidone (NMP) were added to 15 parts by mass of sulfonated polyethersulfone (s-PES, EW: 500 g / eq) having a sulfonation rate of 34.1 mol%, and the mixture was treated at 3500 rpm for 15 minutes using SpeedMixer DAC150 manufactured by Hauschild to obtain an NMP solution (stock solution) of s-PES.

[0218] The obtained stock solution was degassed with a vacuum pump and then applied to a glass substrate, and cast using a scraper set to 650 μm. The glass substrate was placed in a hot air dryer set to 80°C and dried for 1 hour to obtain a dry film. The obtained dry film was immersed in ion exchange water, thereby peeling the electrolytic reference membrane 1B composed of the ion exchange resin composition from the glass substrate. The obtained reference electrolyte membrane 1B was stored in a state immersed in deionized water.

[0219] <Reference Example 2B>

[0220] 35 parts by mass of N-methyl-2-pyrrolidone (NMP) were added to 15 parts by mass of polyethersulfone (PES) manufactured by Solvay, and the mixture was treated at 3500 rpm for 15 minutes using SpeedMixer DAC150 manufactured by Hauschild to obtain an NMP solution (stock solution) of PES.

[0221] The obtained stock solution was degassed with a vacuum pump and then applied to a glass substrate, and cast using a scraper set to 650 μm. The glass substrate was placed in a hot air dryer set to 80°C and dried for 1 hour to obtain a dry film. The obtained dry film was immersed in ion exchange water, thereby peeling the electrolytic reference membrane 2B composed of the ion exchange resin composition from the glass substrate. The obtained reference electrolyte membrane 2B was stored in a state immersed in deionized water.

[0222] <pH measurement>

[0223] 0.1 g of a silica material was dispersed in 1.9 g of deionized water to prepare a dispersion (5 mass % dispersion). The pH of the dispersion was measured at 25°C using a pH meter (PCE-PH 18).

[0224] <Measurement of weight average molecular weight>

[0225] The weight average molecular weight of each resin was measured by GPC. The measurement conditions were as follows.

[0226] Device name: High performance liquid chromatography LC-20A series

[0227] Column oven: CTO-20A

[0228] Mobile phase: NMP

[0229] Automatic sample injector: SIL-20AHT

[0230] LC workstation: LC solution

[0231] Flow rate: 0.3ml / min

[0232] Differential refractive index detector: RID-10A

[0233] Column oven temperature: 60°C

[0234] Molecular weight standard: polystyrene

[0235] <Determination of sulfonation degree>

[0236] The silica material was weighed into a measuring container under a helium atmosphere and measured using an XRF measuring device (PANalytical AxiosMAX). The concentration of sulfur atoms and the concentration of silicon atoms were determined from the obtained spectrum, and the ratio of the concentration of sulfur atoms to the sum of the concentration of silicon atoms and the concentration of sulfur atoms was taken as the degree of sulfonation.

[0237] <Film-forming property>

[0238] The film forming properties of each electrolyte membrane obtained as described above were evaluated according to the following criteria.

[0239] A: When a flawless film can be produced, the film-forming property is judged to be good.

[0240] B: The membrane was formed without any problem in appearance, but cracks occurred in the membrane when the sample for measuring proton conductivity was cut out. It was judged that the membrane was brittle but the membrane could be formed.

[0241] C: When numerous cracks appeared during the drying of the solvent in the dryer and the film shape could not be maintained, it was judged that the film could not be formed.

[0242] <Proton conductivity evaluation>

[0243] Each electrolyte membrane obtained as described above was measured using an electrochemical impedance spectroscopy device (TSC Battery manufactured by RHD Instruments) at a frequency of 50 Hz to 10 7 The impedance of the electrolyte membrane in the thickness direction was measured in the Hz region, and the proton conductivity was measured as an index of proton conductivity. It should be noted that each electrolyte membrane used in the above measurement was provided for the proton conductivity measurement in a state where the electrolyte membrane stored in deionized water was heated to 80°C in the measurement cell. The obtained results are shown in Tables 1 to 3.

[0244] <Fenton test>

[0245] The Fenton test was performed according to the method described in EU harmonized protocols for testing of low temperature water electrolysers (ISBN 978-92-76-39266-8).

[0246] That is, the sample was cut into a size of 4 cm × 4 cm, dried in a vacuum dryer at 50°C for 4 hours, and the dry mass before the Fenton test was measured. Then, a solution containing 4 ppm of divalent iron ions was prepared using 3% by mass of hydrogen peroxide and ferric chloride, and 50 mL of the solution was placed in a water bath at 80°C to adjust the temperature of the solution. The dried sample was placed therein, and a 2-hour Fenton test was performed. After 2 hours, the sample was taken out, dried in a vacuum dryer at 50°C for 4 hours, and the mass was measured. Based on the mass after the test and the mass before the test, the residual rate (%) was calculated. The results obtained are shown in Tables 1 to 3.

[0247] In Tables 1 to 3, EW, sulfonation ratio, and Mw indicate values ​​of an ion exchange resin when the ion exchange resin is used alone, and indicate values ​​of a mixture of the ion exchange resin and a non-ion exchange resin when the ion exchange resin and the non-ion exchange resin are used together.

[0248] In addition, the “silicon dioxide content” in Table 1 indicates the content of the silica material A, the “silicon dioxide content” in Table 2 indicates the content of the silica particles (Silicon dioxide), and the “silicon dioxide content” in Table 3 indicates the content of the silica material B.

[0249] [Table 1]

[0250] [Table 2]

[0251]

[0252] [Table 3]

[0253]

[0254] As shown in Tables 1 to 3, it can be seen that the proton conductivity of the electrolyte membranes 1A-7A and 1B-5B containing the silica material of the present disclosure is higher than that of the comparative electrolyte membrane 1A-7A not containing the silica material of the present disclosure. In addition, it can be seen that the film forming properties of the electrolyte membranes 1A-7A and 1B-5B are excellent regardless of the content of the silica material.

[0255] The disclosures of Japanese Patent Application No. 2022-047494 filed on March 23, 2022 and Japanese Patent Application No. 2023-016458 filed on February 6, 2023 are incorporated herein by reference in their entirety.

[0256] All documents, patent applications, and technical standards described in this specification are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually described as being incorporated by reference.

Claims

1. A silica material comprising a matrix containing silica, and having a sulfonic acid group on at least a surface of the matrix.

2. A silica material obtained by bringing a sulfonating agent into contact with a substrate containing silica.

3. The silicon dioxide material according to claim 1 or 2, wherein The matrix is ​​in granular form.

4. The silicon dioxide material according to claim 3, wherein The matrix is ​​silicon dioxide particles, and the number average particle size of primary particles of the silicon dioxide particles is 1 nm to 500 nm.

5. The silicon dioxide material according to claim 1 or 2, wherein: The ratio of the concentration of sulfur atoms to the total concentration of silicon atoms and the concentration of sulfur atoms determined by XRF measurement, which is an X-ray fluorescence spectrometry, is 0.01% to 90%.

6. An ion exchange resin composition comprising the silica material according to claim 1 or 2 and an ion exchange resin.

7. The ion exchange resin composition according to claim 6, wherein The content of the silica material in the solid content of the ion exchange resin composition is 0.01% by mass to 90% by mass.

8. An electrolyte membrane comprising the ion exchange resin composition according to claim 6. 9 . A membrane electrode assembly comprising: the electrolyte membrane according to claim 8 , a cathode layer stacked on one surface of the electrolyte membrane, and an anode layer stacked on the other surface of the electrolyte membrane. 10 . A polymer electrolyte fuel cell comprising: the membrane electrode assembly according to claim 9 , and separators disposed on both surfaces of the membrane electrode assembly.

11. A solid polymer electrolysis device comprising: the membrane electrode assembly according to claim 9, and separators arranged on both surfaces of the membrane electrode assembly.

12. An electrochemical hydrogen compression device comprising the electrolyte membrane according to claim 8.

Citation Information

Patent Citations

  • Thin membrane electrolyte

    JP1989158051A

  • Polymer electrolyte composite membrane, its manufacturing method and solid polymer type fuel cell using it

    JP2005166557A

  • Polyethylene microporous film

    JP2011241361A

  • Stainless steel powders for additive manufacturing

    JP2022047494A

  • Electrolytic plating solution additive, production method thereof, and production method of electrolytic plating solution and electroplated member