Recycled concrete aggregate carbonization treatment
By pressurized carbon dioxide in the airtight sealed chamber, the regenerated concrete aggregate is improved and contamination is reduced, and the mechanical properties of RCA is solved in use and the environmental impact of environmental impact is achieved. Sustainability.
Patent Information
- Application Number
- CN202380019161.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-28
- Filing Date
- 2023-01-27
- Publication Date
- 2024-11-05
AI Technical Summary
Existing recycled concrete aggregates (RCAs) have shortcomings in terms of mechanical properties and environmental impacts, which are inferior to natural aggregates and may cause contamination, limiting their effective use in state or local agencies and groundwater quality.
By building an airtight sealed chamber, loading and pressurizing the carbon dioxide gas, monitoring and controlling the pressure, temperature and relative humidity in the chamber, promoting the reaction between calcium hydroxide and calcium silicate and carbon dioxide, increasing calcium carbonate and The percentage of silica improves the mechanical properties of RCA and reduces contamination.
Significantly improves the mechanical properties of RCA, meets the requirements of alternative natural aggregates, and protects groundwater quality by reducing pH and heavy metal concentrations in the leachate, providing a sustainable solution.
Smart Images

Figure CN118900828A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This patent application claims the benefit of U.S. Provisional Patent Application No. 63 / 304,184, filed on January 28, 2022, which is incorporated by reference in its entirety for all purposes. Background Art
[0003] As infrastructure construction and maintenance continue, the demand for sand, gravel, rock and concrete has increased significantly, consuming huge amounts of natural resources each year. For example, it is estimated that the annual demand for aggregates in the United States exceeds 1.8 billion tons (1.6×10 12 kg). In addition, a large amount of construction and demolition (C&D) waste is generated every year, especially waste concrete. Concrete accounts for about 70% of the entire commercial demolition waste. At the same time, landfill costs continue to increase. In this regard, the recycling and reuse of waste concrete may greatly help to solve these challenges.
[0004] One of the most promising ways to reuse such waste concrete may be to produce recycled concrete aggregate (RCA) through crushing and screening. RCA is a popular alternative to natural stone aggregates for parking lots, backfill, home landscaping, etc. However, due to the large amount of residual paste left over and previous heavy use (including weathering), the mechanical properties of RCA may not be as good as natural aggregates. In addition, due to the potential contamination caused by heavy metal leachate and high pH, there may be environmental issues about the use of RCA. For example, a research team showed the high alkalinity and heavy metal concentration of RCA leachate through laboratory and field tests. The above problems greatly limit the effective use of RCA in state or local agencies. In addition, RCA can potentially damage groundwater quality. Therefore, it may be urgent to develop a means to improve the mechanical properties of RCA while solving environmental problems about the use of RCA. Summary of the invention
[0005] One or more aspects of the present disclosure provide a method for processing recycled concrete aggregate (RCA), comprising: constructing a chamber configured to form an airtight seal; loading the RCA into the chamber; airtightly sealing the chamber; pressurizing the interior of the chamber with carbon dioxide gas; monitoring the pressure and relative humidity of the interior of the chamber; and controlling the pressure and the relative humidity until a predetermined condition is met.
[0006] One or more aspects of the present disclosure provide treated recycled concrete aggregate (RCA), comprising: RCA loaded into a chamber and hermetically sealed within the chamber; and treating the RCA by exposing the RCA to a carbon dioxide-rich atmosphere under high pressure within the chamber, the temperature and relative humidity of the atmosphere being monitored and controlled until predetermined conditions are met, wherein treating the RCA changes the proportions of constituent minerals in the RCA, with the percentages of calcium carbonate and silicon dioxide increasing due to the reaction between calcium hydroxide and calcium silicate hydrates and carbon dioxide.
[0007] One or more aspects of the present disclosure provide a method for carbonizing recycled concrete aggregate (RCA). The method includes: constructing a chamber configured to form an airtight seal; loading the RCA into the chamber; airtightly sealing the chamber; pressurizing the interior of the chamber with carbon dioxide gas; monitoring the pressure, temperature, and relative humidity of the interior of the chamber; and controlling the pressure, the temperature, and the relative humidity until a predetermined condition is met.
[0008] One or more aspects of the present disclosure provide a system for processing recycled concrete aggregate (RCA). The system comprises: a chamber configured to form an airtight seal, the chamber comprising: at least 10 L and no more than 3×10 4 L volume; a door configured to form an airtight seal; at least one dehumidifier installed in the chamber and configured to maintain relative humidity in the chamber; at least one system installed in the chamber and configured to collect water from the at least one dehumidifier; at least one fan installed in the chamber and configured to circulate CO2 gas and moisture in the chamber; at least one heating element; at least one pressure sensor installed and configured to measure the pressure in the chamber; at least one relative humidity / temperature sensor installed and configured to measure the relative humidity and temperature in the chamber; a carbon dioxide gas supply source operably connected to the chamber via an injection valve; and an ejection valve installed on the chamber and configured to allow gas to leave the chamber. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 A chamber for carbonizing RCA is shown according to one or more embodiments.
[0010] Figure 2A and 2B Shown are two laboratory chambers for carbonizing RCA according to one or more embodiments.
[0011] Figure 3 A sealed barrel for percolation testing according to one or more embodiments is shown.
[0012] Figure 4 A sample identification system according to one or more embodiments is presented.
[0013] Figure 5 A bar graph showing all measured aggregate crushing values according to one or more embodiments.
[0014] Fig. 6A and 6B A bar graph showing LA wear mass loss according to one or more embodiments.
[0015] Figure 7 A bar graph showing LA wear mass loss according to one or more embodiments.
[0016] Fig. 8A and 8B A bar graph showing freeze-thaw mass loss according to one or more embodiments.
[0017] Fig. 9 A bar graph showing freeze-thaw mass loss according to one or more embodiments.
[0018] Fig.10 A bar graph showing the compressive strength of concrete samples according to one or more embodiments.
[0019] Fig.11 A bar graph showing a fracture model of a concrete sample according to one or more embodiments.
[0020] Fig.12 A bar graph showing the plasticity module and Poisson's ratio of concrete samples according to one or more embodiments.
[0021] Fig.13 A bar graph showing surface resistivity and volume resistivity of concrete samples according to one or more embodiments.
[0022] Fig.14A and 14B A graph showing mass of carbon dioxide per mass of RCA over time for different pressures according to one or more embodiments.
[0023] Fig.15 A graph showing mass of carbon dioxide per mass of RCA over time for different pressures according to one or more embodiments.
[0024] Fig.16A and 16B Graphs showing CO2 mass consumption per RCA mass for different pressures and CO2 mass variation over time according to one or more embodiments.
[0025] Fig.17A and 17BGraphs showing CO2 mass consumption per RCA mass for different pressures and CO2 mass variation over time according to one or more embodiments.
[0026] Fig.18A and 18B Graphs showing carbon dioxide mass consumption per RCA mass for different relative humidities and carbon dioxide mass variation over time in accordance with one or more embodiments.
[0027] Fig.19A and 19B Graphs showing carbon dioxide mass consumption per RCA mass for different temperatures and carbon dioxide mass variation over time according to one or more embodiments.
[0028] Fig. 20A and 20B Graphs showing carbon dioxide mass consumption per RCA mass for different relative humidities and carbon dioxide mass variation over time in accordance with one or more embodiments.
[0029] Fig.21A and 21B Graphs showing CO2 mass consumption per RCA mass and CO2 mass variation over time for different sample preconditioning according to one or more embodiments.
[0030] Fig. 22 is a flow chart of a method of processing recycled concrete aggregate according to one or more embodiments. DETAILED DESCRIPTION
[0031] Applicants have investigated improving the mechanical and chemical properties of older concrete aggregates by introducing carbon dioxide (CO2). Experiments were performed in a laboratory environment, and a mid-scale prototype chamber was developed and tested for suitability for the experiments. The chamber was constructed to handle about one ton (910 kilograms (kg)) of loose volume of source-controlled RCA, but the chamber, system, method, and products produced herein are not intended to require source-controlled RCA. After performing about 40 tests using the prototype chamber and about 30 tests in the laboratory, Applicants have demonstrated the efficacy of improving aggregates through the carbon dioxide treatment process.
[0032] Treating RCA with carbon dioxide (CO2) changes the ratio of constituent minerals in RCA, increasing the percentage of calcium carbonate (CaCO3) and silicon dioxide (SiO2) due to the reaction between calcium hydroxide (Ca(OH)2) and calcium silicate hydrate (CSH) and carbon dioxide (CO2).
[0033] The long-term impact of this research could be enormous. The present disclosure has the potential to disrupt the $19 billion stone aggregate industry in an environmentally beneficial way. By improving RCA to higher value uses, the treated RCA described herein can be diverted from landfills (scrap concrete is the single largest landfill product in the United States by volume). Treated RCA is sustainable, and the disclosed method can provide significant carbon sequestration. Using RCA as a substitute for virgin material can extend the life of quarries and reduce the burden on natural habitats. In addition, reducing pH and heavy metals in RCA leachate can protect groundwater.
[0034] One of the most promising ways to reuse such waste concrete may be to produce recycled concrete aggregate (RCA) through crushing and screening. RCA is a popular alternative to natural stone aggregates for parking lots, backfill, home landscaping, etc. However, due to the large amount of residual paste left over and previous heavy use (including weathering), the mechanical properties of RCA may not be as good as natural aggregates. In addition, due to potential contamination caused by heavy metal leachate and high potential hydrogen ions (pH), there may be environmental issues about the use of RCA. For example, a research team showed high alkalinity and heavy metal concentrations in RCA leachate through laboratory and field tests. The above problems greatly limit the effective use of RCA in state or local agencies. In addition, RCA can potentially damage groundwater quality. Therefore, it may be urgent to develop a means to improve the mechanical properties of RCA while solving environmental problems about the use of RCA.
[0035] Laboratory studies
[0036] A total of twenty-seven separate laboratory-scale carbon dioxide treatments have been implemented using two processing chambers with capacities of 10 liters (L) and 30L. In particular, the effects of the main variables, including carbon dioxide supply pressure, relative humidity (RH), processing temperature, initial gas conditioning (CO2 vacuum and CO2 flushing), and sample pre-conditioning methods, on carbon dioxide consumption for RCA processing were studied in depth. Mechanical and pH test results confirmed that the RCA samples were properly carbonized by carbon dioxide. The calculated carbon dioxide mass consumption showed that consumption would increase with initial carbon dioxide supply pressure, exposure time, and temperature. In addition, the test results showed that the optimal RH for achieving maximum carbon dioxide consumption could be in the range of 50±10%, and in particular 50±5%. Due to the higher volume of supplied carbon dioxide, more significant mechanical improvements in RCA were observed in the processing chamber with a higher capacity (30L).
[0037] Fabrication of commercial scale prototypes
[0038] Manufactured with 500 gallons (1.9 cubic meters (m 3)) as a commercial scale prototype. The prototype chamber 100 has a length (L) of 116 inches and a height (H) of 38 1 / 2 inches. A commercial chamber may have a volume of 1000 cubic feet (28,000 liters) or more. As an example, a commercial chamber may be 8 feet in diameter (or height) and 20 feet in length. The chamber 100 is equipped with a pressure sensor 116 and a relative humidity / temperature (RH / T) sensor 118, a gas injection valve 124 and a blow-off valve 126, tracks for accommodating RCA baskets, a water collection container 114, a fan 122, and a dehumidification system 112. The dehumidification system may be a conventional dehumidifier, a desiccant dehumidifier, or some other suitable system. The chamber door 102 is designed to facilitate loading and unloading of the RCAs and is airtight to prevent any carbon dioxide leakage during processing of the RCAs.
[0039] Carbon dioxide treatment for RCA using prototype
[0040] A total of thirty-five separate CO2 treatments were performed on the RCA using the prototype under various conditions. Test conditions included CO2 pressure, CO2 supply conditions, RCA loading arrangement (simple loose loading vs. individual loading in baskets to ensure better contact with CO2), RCA volume, treatment time, temperature, and initial moisture content of the RCA to determine the effect of each variable on CO2 consumption and the resulting mechanical and environmental improvements of the CO2 treated RCA.
[0041] Test conditions included CO2 pressures: 1, 5, 10, 20, 40 and 60 pounds per square inch gauge (psig, 6.9, 34.5, 68.9, 138, 276 and 414 kilopascals (kPa), respectively); CO2 supply: initial set pressure and continuous CO2 supply; loading arrangement: in basket and simple loose loading; RCA volume: 10% and 20% of the internal chamber volume; treatment time: 1 hour to 24 hours; and initial moisture content of RCA: normal dry and extra dry. Higher pressures (e.g., 80 psig or greater) are expected. Additional testing was performed at 80 psig (552 kPa) until chamber seal failure. A wide range of CO2 mass consumption and mechanical environmental test results have been obtained using those different variables. Analysis of the test results indicates the most effective and optimal parameter ranges.
[0042] Mechanical and environmental testing of CO2 treated RCA using prototypes
[0043] Five different mechanical tests and two environmental related tests were conducted using the original and CO2 treated RCA. In detail, 22 separate specific gravity and absorption capacity tests, 117 separate aggregate crushing value (ACV) index tests, 23 Los Angeles (LA) abrasion tests, and 23 freeze-thaw (FT) resistance tests were conducted on the CO2 treated RCA using the manufactured prototype. In addition, 36 separate phenolphthalein tests and more than 150 leachate water tests were conducted to study the pH and heavy metal concentrations in the leachate of the CO2 treated RCA.
[0044] Mechanical properties showed a wide range of improvements: ACV improvement of up to about 20%, LA abrasion mass loss improvement of up to about 16%, and FT mass loss improvement of up to about 59%. It was observed that all of the RCAs treated with carbon dioxide met the requirements for replacing natural aggregates (i.e., the mass loss of concrete and base due to abrasion was less than 40% and 45%, respectively, according to AASHTO T96 and NDOT specification 1033.02). The base refers to a rock pad that may be 4 to 6 inches (10 to 15 centimeters (cm)) to allow water to drain through it. In addition, concrete samples mixed with RCA treated with carbon dioxide met the requirements for replacing natural aggregates in terms of a minimum strength of 3,500 pounds per square inch (psi, 24 megapascals (MPa)), a minimum modulus of rupture of 600 psi (4 MPa), and FT resistance.
[0045] For the environment, for various CO2 treatment conditions, after 24 hours of immersion, the pH of the leachate water decreased by up to two pH units compared to the original RCA, while the concentration of heavy metals decreased by more than 50%. It is worth noting that the concentration levels of most heavy metals in the collected leachate water are well below the EPA's maximum contamination level (MCL) for drinking water.
[0046] All small-scale and medium-scale CO2 processing data as well as mechanical and environmental test results are compiled and analyzed in detail. Below, the results for each variable are described first, followed by the combined range of variables.
[0047] Carbon dioxide pressure:A wide range of carbon dioxide pressures were studied from 1psig to 60psig (6.9kPa to 410kPa) gauge pressure. The test results show that carbon dioxide is consumed much faster at higher carbon dioxide pressures. The ACV test results do not show a strong correlation between strength increase and CO2 pressure. The ACV index may be more relevant to the overall properties of RCA. The mass loss after LA wear and FT resistance tests shows a very good correlation with carbon dioxide pressure (and therefore carbon dioxide consumption). For RCA treatment, the pH of the leachate water also decreases more with higher carbon dioxide pressure. Finally, heavy metal concentrations do not show a strong correlation with carbon dioxide pressure. However, all heavy metal concentrations are still far below the EPA's maximum contamination level (MCL) for drinking water. Among the test results, FT mass loss shows the strongest correlation with CO2 consumption, with a P value of approximately 0.035 from statistical regression analysis. This is a noteworthy result because FT mass loss is one of the most important indicators of aggregate durability. It may be the case that higher CO2 pressures can induce faster carbonization of RCA and a higher degree of penetration inside the aggregate. Furthermore, the test results showed that the proposed treatment method was most effective for improving the surface-level mechanical properties of RCA.
[0048] Processing time : Various treatment times ranging from 1 hour to 24 hours were examined. Based on the carbon dioxide consumption results of both the medium-scale test and the laboratory-scale test, it was observed that the treatment time can be divided into three zones as follows: 0 to 6 hours: the rate of carbon dioxide treatment of RCA is the fastest, 6 to 12 hours: medium rate, and 12 to 24 hours: slow treatment rate. Therefore, the most effective time for the treatment process may be within 12 hours, especially the first 6 hours. The mass loss of LA wear resistance and FT resistance tests showed a good relationship with the treatment time. Statistical regression analysis showed that all mechanical tests—ACV, LA wear and FT resistance—were statistically highly dependent on the treatment time (P values were approximately 0.003, 0.040 and 0.0001, respectively). In general, the treatment time may be another important factor that can significantly affect the carbon dioxide treatment process.
[0049] RCA Quality Two different RCA masses were evaluated using a mid-scale prototype, 10% and 20% of the total volume of the processing chamber (i.e., approximately 260 kg (570 pounds (lb)) and 730 kg (1610 lb) respectively). Two different RCA masses were also tested in a laboratory scale processing chamber, with amounts of 1.2 kg and 5 kg. In theory, a higher mass (and therefore volume) of RCA can reduce the volume that the carbon dioxide can occupy, and can reduce the contact between the RCA and the carbon dioxide inside the chamber. The main finding here is that the gas flow of carbon dioxide between the aggregates is important.
[0050] Relative humidity :The effect of RH on CO2 consumption, mass gain of RCA and ACV was investigated in depth using a laboratory scale processing chamber (30L). A wide range of RH levels (from about 2% to about 80%) was tested. Data analysis showed that maximum CO2 consumption was achieved when RH was between 50% and 55%. The mass gain of RCA after CO2 treatment also showed higher gain for RH of 50±5%. The ACV index did not show a strong correlation, but in general, the ACV index showed the best improvement when RH was in the range of 50% and 55%. In this regard, the optimal RH range may be 50±5%.
[0051] Processing temperature : The effect of treatment temperature in a limited range was preliminarily studied in the laboratory. Test results show that CO2 consumption improves at higher temperatures. The mass gain of RCA after CO2 treatment also shows that the gain percentage increases with increasing treatment temperature, while the ACV index does not show a strong dependence on treatment temperature. From a geochemical point of view, treatment temperature can play an important role by accelerating / decelerating chemical reactions.
[0052] Preconditioning (initial moisture content, expressed as mass %) : Pre-conditioning of the medium-scale treatments remained similar (actually 3 to 5%) for all tests performed. Despite such a narrow range of initial moisture content (i.e., moisture content before entering the chamber), FT resistance showed a good correlation with it from the statistical regression analysis (P value = 0.0016). That is, the FT resistance test produced less mass loss at lower initial moisture contents. Theoretically, the amount of initial moisture content may play an important role in the carbonization process. That is, moisture may be required to initiate any chemical reaction, however, large amounts of water may prevent carbon dioxide from penetrating into the RCA and therefore prevent the carbonization process. In this regard, pre-conditioning the RCA at an optimal moisture level may be another important factor.
[0053] Based on the observed results of all test variables, the optimal ranges of the test variables can be summarized, as shown in Table 1.
[0054] Table 1. General optimal treatment variables based on experimental results
[0055]
[0056] Fabrication of CO2 Processing Chamber
[0057] A 500-gallon (1900-L) propane tank was used to fabricate the prototype chamber 100. (See Figure 1). The tank was modified to have an outward swing door 102 with six threaded tailgate latches to hold the door 102 closed during processing. To obtain an airtight seal, a 2 inch (″) x 1 / 4″ (5.0 centimeters (cm) x 0.64 cm) flat steel lip was welded to the tank body, and an additional lip and latch support were welded to the door. A natural rubber seal was placed on top of the two inch lip and glued in place, then sealed with a rubber gasket sealant. For additional stability during processing and to support the additional weight of the new door, the base of the tank was widened. A wider bottom support 104 was made using 4 inch x 2 inch (10 cm x 5 cm) rectangular steel tubing. The processing basket 106 is made of expanded metal, angle iron, and flat steel bars. In one or more embodiments, the processing basket may be 26 inches long. A total of 6 rolling baskets 106 are made to hold the rock during processing. Wheels 108 are added to the basket to allow the basket to roll into place on welded tracks 110 inside the processing chamber 100. In addition to the basket 106 and general tank modifications, a mount for a dehumidifier 112 is also installed in the chamber door 102, and a metal box (water collection container 114) is made to contain water collected by the dehumidifier 112 during processing. The carbon dioxide inlet port, sensor port, pressure relief valve (or blow-off valve), and openings for electrical components are made to complete the chamber 100. After the modifications to the new processing chamber design were completed, the chamber 100 was tested to maintain a maximum gauge pressure of 65 psig (450 kPa). (Note that unless otherwise indicated, pressures in this disclosure are gauge pressures). In subsequent testing, the rubber chamber seal failed at 70 psig (480 kPa).
[0058] Recycled concrete aggregate: sources and preparation
[0059] The material used in the experiment was a blended mixture from airports and highways. The material was crushed using two crushers (McCloskey J50 jaw crusher and McCloskey I44 impact crusher) and then screened using a McCloskey S190 screening station to obtain 1 inch (2.5-cm) nominal maximum size aggregate (NMSA) RCA samples.
[0060] Medium Scale CO2 Treatment
[0061] The above describes the fabrication and different parts of the pilot scale prototype chamber 100. The monitoring and control system includes a dehumidifier 112 (to control the relative humidity of the chamber during processing), a pressure transducer sensor 116 (Omega, 0 to 100 psig, i.e., 0 to 690 kPa), a temperature / relative humidity sensor 118 (Vaisala, HMP110), a carbon dioxide high purity cylinder 120 (99.9% purity grade, Matheson) and a data acquisition system (Keysight 34972A) to record the pressure and temperature / RH during processing. Although the experiments were conducted with high purity carbon dioxide, lower purity carbon dioxide, such as carbon dioxide from industrial processes, can also be used. In Figure 1 A prototype chamber 100 is shown in FIG.
[0062] Medium Scale CO2 Treatment
[0063] Testing Procedure
[0064] To achieve consistent ambient temperature and relative humidity, and to reduce the effects of seasonal and hourly temperature / RH fluctuations, the processing chamber was placed inside the machine shop. RCA samples were placed inside the machine shop, spread out on the floor, and dried using an oscillating fan 24 hours prior to the start of the processing process. For all processing embodiments, this process may help to achieve consistent moisture content and temperature of the RCA samples prior to co2 treatment. RCA samples were periodically turned using a spatula to promote drying.
[0065] Two different loading arrangements (basket and simple loose loading) were used to study the effect of the loading arrangement for RCA processing. In this way, in the basket loading arrangement, six rolling baskets 106 were uniformly loaded with pre-dried RCA samples using a shovel, and then the six rolling baskets were placed inside the chamber 100 one after another in two layers, as shown in FIG. Figure 1 For the simple loose load arrangement method, a similar sample volume is first measured by loading six baskets and then dumping the sample volume into the processing chamber and spreading it evenly at the bottom of the chamber 100. In this case, the water collection container 114 is placed at the top of the sample.
[0066] After the RCA sample is loaded inside the processing chamber 100, the dehumidifier 112 is set to 40% relative humidity to ensure that the average relative humidity of the chamber is 50 to 60% during the carbon dioxide treatment process. Then, the chamber door 102 is tightly closed, and the carbon dioxide is pressurized inside the chamber 100 until 1 to 2 psig (6.9 kPa to 13.8 kPa), and then the pressure is released from the pressure relief valve 126 to purge the air inside the chamber 100 and have pure carbon dioxide during the treatment process. The chamber 100 is then pressurized until the desired carbon dioxide pressure is reached, at which time the carbon dioxide inlet valve 124 is closed (i.e., CO2 set pressure). As a second carbon dioxide supply mode, the inlet valve 124 remains open at a certain level to ensure that carbon dioxide gas is continuously supplied to the chamber 100 and the chamber pressure is maintained at a constant level (i.e., CO2 is continuously supplied). During the treatment, the carbon dioxide pressure, temperature, and relative humidity inside the chamber 100 are recorded using sensors 116, 118 connected to the processing chamber and a data acquisition system and computer. The carbon dioxide treatment was stopped after 24 hours, either after all the carbon dioxide gas was consumed (the carbon dioxide pressure inside the chamber reached zero) or if the carbon dioxide pressure did not reach zero after 24 hours of treatment.
[0067] RCA sampling for mechanical and environmental testing in laboratories
[0068] After the carbon dioxide treatment was completed, any remaining carbon dioxide pressure was released using the pressure relief valve 126, and the chamber door 102 was opened. For each treatment embodiment, three buckets (5-gallon (19-L) capacity) were collected and transferred to the laboratory for further mechanical and environmental testing. Due to the importance of the sampling process and having representative samples, the sampling process was kept similar for all treatment embodiments. In this regard, for the basket arrangement method, each sample bucket was filled from each basket by two shovels. For the simple loose loading method, the bucket was filled from the top, middle and bottom of the RCA pile inside the chamber by two shovels. As listed in Table 2, a total of thirty-five separate treatment embodiment tests were conducted under various conditions. For the sake of brevity, each treatment condition is presented with abbreviations as follows: SPB10: initial set pressure, basket, 10% volume; SPB20: initial set pressure, basket, 20% volume; SPD20: initial set pressure, simple loose loading, 20% volume; CPB20: continuous pressure, basket, 20% volume.
[0069] Table 2. Medium-scale CO2 treatment conditions
[0070]
[0071] Note: Hereinafter, processing conditions are abbreviated in context as follows:
[0072] 1:SPB10, 2:SPB20, 3:SPD20, 4:CPB20
[0073] Laboratory scale CO2 treatment
[0074] Test equipment
[0075] The laboratory processing apparatus 200 includes a sealed processing chamber 204 (either 10-L or 30-L capacity), a pressure transducer 208 (Omega, 0 to 200 psig (0 to 1.4 MPa)) connected to the chamber, and a temperature / relative humidity sensor 212 (Vaisala, HMP110). The sensors 208, 212 are connected to a data acquisition system 216 (Keysight; 34972A) to record the pressure, temperature, and RH inside the processing chamber 204 during the processing process. A high purity (99.9%, Matheson) carbon dioxide cylinder 220 is also connected to the processing chamber 204 via a pressure regulator 224 to control the carbon dioxide supply rate into the processing chamber 204. As shown in FIG. Figure 2A and 2B , each processing chamber 204 has two valves at the top, one valve for carbon dioxide inlet 228, and another safety valve 232 for vacuum / decompression purposes. The carbon dioxide inlet valve 228 can be a needle valve. The chamber includes a rack 236 (e.g., two racks in a 10L chamber and four racks in a 30L chamber) to hold the RCA sample 240 and ensure sufficient surface contact between the RCA and the carbon dioxide.
[0076] Testing Procedure
[0077] In the laboratory carbon dioxide treatment method, RCA samples of specific sizes are used to minimize size effects and better control the carbon dioxide treatment process and analysis. In this regard, the same RCA from the medium-scale treatment is additionally screened. Samples that pass through a 1 / 2 inch (1.3-cm) sieve but remain on a 3 / 8 inch (1.0-cm) sieve are collected for laboratory carbon dioxide treatment implementation plans. The sieved RCA samples are first pre-conditioned to ensure that the initial RH and temperature (T) of the samples inside the control chamber (where T = 73.4-77℉ (24±1℃) and RH = 50%±1) remain consistent within 24 hours before starting the treatment process. A specific amount of silica gel 244 (sg; Interra Global) is then placed at the bottom of the chamber (or in some cases in the middle of the chamber as an additional layer in a 30L chamber) to control the RH inside the chamber during the treatment process. Afterwards, a specific amount of pre-conditioned RCA sample (2.6 pounds (1.2 kg) in a 10L chamber and 11 pounds (5 kg) in a 30L chamber) is evenly placed on a rack and then moved to the processing chamber 204. The chamber cap is then tightly closed and a carbon dioxide injection tube is also connected to the chamber. In order to obtain pure carbon dioxide gas inside the chamber, a low carbon dioxide pressure (2 to 3 psig (13.8 to 20.7 kPa)) is applied, and then the injected CO2 is discharged via a pressure reducing valve 232 (i.e., CO2 flushing). Moreover, in the process using a 10L capacity chamber (i.e., CO2 vacuum), three carbon dioxide injection / vacuum (up to 13 psig (90 kPa)) cycles are applied. Evacuation is performed using a vacuum pump 248. Carbon dioxide is then injected into the chamber until a specific pressure level is reached and the valve is closed.
[0078] After 24 hours, the pressure relief valve 232 was opened to release the remaining carbon dioxide gas inside the chamber, and the chamber cap was opened. The processed RCA was collected from the chamber, and the weight of the sample was also measured after the treatment process. Six individual RCA samples were randomly selected to perform phenolphthalein testing on the surface and cross-section of the processed samples. The remaining samples were prepared for ACV testing and water content measurement. Table 3 summarizes the laboratory scale carbon dioxide treatment conditions for the two treatment chambers.
[0079] Table 3. Laboratory scale CO2 treatment conditions
[0080]
[0081] Note: W / C: washed and placed in a controlled room with RH=50% within 24 hours before starting the treatment process, W / O: washed and dried, W / L: washed and laboratory dried for 48 hours, N / L: not washed but laboratory dried for 48 hours.
[0082] *This test is performed in a controlled room with a constant ambient temperature of 3±0.5℃.
[0083] Physical and mechanical testing
[0084] To evaluate the physical and mechanical properties of the RCA samples after CO2 treatment, the untreated (raw) and CO2 treated RCA samples were subjected to appropriate standard physical and mechanical tests as listed in Table 4. The detailed test procedures associated with each laboratory test are described below.
[0085] Table 4. Laboratory mechanical and environmental tests
[0086]
[0087] Specific gravity and absorption capacity
[0088] Specific gravity and absorbency tests were performed based on the ASTM C127 standard. Due to the potential uncertainty caused by the high variability of RCA samples, each sample was re-screened to the same grade for higher accuracy (No. 57 according to ASTM C33). In addition, due to the high absorbency of RCA, in order to ensure complete saturation of the RCA samples, the RCA samples were soaked for 72 hours instead of 24 hours (as recommended by the standard) to ensure complete saturation of the RCA samples. The procedure involves soaking the RCA sample (at least 6.6 pounds (3 kg)) in water, then removing the sample from the water and rolling it in a large absorbent towel to remove surface water. The mass of the saturated surface dry (SSD) sample in air is then obtained, and the mass of the sample in water is then measured to identify the exact volume of the sample. Thereafter, the sample is dried at 230±9℉ (110±5℃) for 24 hours.
[0089] Then use the following equation to calculate the absorbency and specific gravity.
[0090]
[0091] Where A is the mass of the oven-dried test sample in air, B is the mass of the SSD sample in air, and C is the mass of the SSD sample in water.
[0092] Aggregate Crushing Value (ACV)
[0093] The ACV test is performed based on the modified BS110-812 standard. A single-sized RCA sample (1 / 2" to 3 / 8" (1.3cm to 1.0cm)) is placed inside a 6-inch (154mm) inner diameter steel ring, up to 2 inches (5cm) in height, and compacted with 5 / 8" (15.9mm) diameter tamping rod 25 times. The load is applied at a rate of 0.35±0.05 inches / minute (in / min) (0.15±0.02mm / s) until a load of 30,000 pounds force (kips) (133 kilonewtons (kN)) is reached, and then the load is immediately released. The steel ring with the crushed RCA is placed on a vibrating table and vibrated to loosen the compacted RCA sample. The crushed RCA sample is sieved using a No. 8 sieve. The aggregate crushing value (ACV) is calculated as the percentage of particles passing through the No. 8 sieve according to the following equation.
[0094]
[0095] Los Angeles (LA) Wear
[0096] The LA wear test was performed according to ASTM C131. A specific graded sample was prepared by combining 5 pounds (2.5 kg) of 1 / 2 inch (1.3-cm) size RCA and 5 pounds (2.5 kg) of 3 / 8 inch (1.0-cm) size RCA. The sample was then placed in the LA test machine along with a feed consisting of 11 steel balls, each 440 grams. The machine was then rotated 500 times at a speed of 30 to 33 revolutions per minute (rpm). After completing the 500 revolutions, the material was discharged and sieved with a No. 12 sieve. The mass passing through the No. 12 sieve was recorded, and the LA wear mass loss was calculated using the following equation.
[0097]
[0098] Freeze-thaw (FT) resistance
[0099] The freeze-thaw (FT) resistance of aggregates was evaluated based on the CSA A23.2-24A standard. Although the standard requires testing of each particle size, this study only focuses on RCA of 1 / 2 inch (1.3-cm) size. The first step is to carefully prepare the dried sample (2.75 pounds (1.25kg)) by removing any contaminants (such as asphalt bricks, wood and metal). Then, the RCA sample is placed in a container of appropriate size (1L in this case), followed by filling the container with a prepared 3% sodium chloride (NaCl) solution to submerge all aggregate particles. The container is then sealed and kept at room temperature for 24 hours. Afterwards, the solution is removed by inverting the container on a sieve less than 5mm mesh. The container is then sealed and placed in a freezer at 0℉ (-18℃) for 16 hours, which is the freezing cycle stage. The melting cycle is started by removing the container from the freezer and placing it at room temperature for 8 hours. These cycles are repeated five times. After five cycles of freeze-thaw, the aggregate was washed by filling the container with tap water and draining it by inverting it on a No. 4 sieve for 5 seconds. This step was repeated five times to ensure that the RCA particles were thoroughly washed. The samples were then dried at 110°C for 24 hours. Finally, the dried RCA samples were sieved using a suitable sieve (in this case 1 / 2 inch (1.3-cm)) and the mass loss was recorded.
[0100] Environmental Testing
[0101] Laboratory batch percolation testing
[0102] Laboratory batch percolation tests were conducted on untreated (raw) and CO2 treated samples to evaluate the environmental impact of CO2 treatment on RCA sample 240. Figure 3 As shown in FIG. 1 , a 10-pound (4.54-kg) RCA sample 240 (screened with a 1-inch (2.5-cm) screen, similar to the grading in the field-scale treatment) was immersed in 1 gallon (3.79 L) of distilled water 304 in a plastic bucket 300 (5-gallon (18.9-L) capacity) with a sealed door 308. Then, leachate water samples were collected from the bucket 300 after a period of 1 day, 2 days, 4 days, 7 days, 14 days, and 21 days. The pH and total element concentrations of the leachate water samples were measured using a pH meter (Accumet AB15) and an ICP-MS (inductively coupled plasma mass spectrometry) device, respectively. This test procedure was modified from the Ohio DOT 2002 report.
[0103] Concrete mixture with RCA treated with CO2
[0104] Concrete Mix
[0105] Use a 3 cubic foot (ft 3 ,0.0849m 3 ) capacity drum mixer, following the procedure described in ASTM C192 (Standard Practice for Making and Curing Test Specimens in Laboratories). First, the coarse aggregate was mixed with about half of the mixing water containing AEA (air entraining agent) for 30 seconds. Then, sand and gravel, cement and the remaining water were added and mixed for 3 minutes, followed by 3 minutes of standing and an additional 2 minutes of mixing. If workability adjustment was required, WR (water reducing admixture) was added and the concrete was mixed for an additional 3 minutes. During the performance evaluation stage, when the WR dosage for a specific mix was known, it was added along with the other half of the water. Prior to mixing, the aggregate was saturated and the 1.3 ft 3 (0.0368m 3 ) Before batching each mixture, adjust the amount of water according to the moisture condition of the aggregate.
[0106] Tables 5 and 6 show the mix designs and mix proportions for the mixtures under study, where pcy is pounds per cubic yard and cwt is hundredweight, or 100 pounds (45 kg). Therefore, fluid ounces per 100 pounds are abbreviated as fl oz / cwt. Mix identification is based on three parameters, namely, the processing pressure 404 (T for treated or U for untreated) and the fractions of RCA or NA (natural aggregate) 408 and river sand (RS) 412. For example, T5_RCA30-RS70 represents a mixture of RCA processed at 5 psig (34.5 kPa) with RCA and RS fractions of 30 and 70, respectively ( Figure 4 ). Note that since the specific gravity of RCA was almost the same before and after CO2 treatment, the mix design was the same for all RCA mixes. Due to the lower specific gravity of RCA (compared to NA), a lower amount of coarse aggregate was used in the RCA mixes.
[0107] Table 5. Mix design of concrete prepared with RCA
[0108]
[0109] Table 6. Properties of concrete prepared with RCA
[0110]
[0111] Results: Medium-Scale CO2 Processing
[0112] Various CO2 treatment conditions were applied to evaluate the impact of each variable on the CO2 treatment process and RCA mechanical and environmental properties, and ultimately the optimal variable range was found based on mechanical, environmental and cost analysis of the results. Table 7 lists the recorded parameters for all thirty-five individual pilot scale CO2 treatment implementations under various conditions.
[0113] Table 7. CO2 treatment conditions and recorded data before, during and after the CO2 treatment process for all treatment embodiments
[0114]
[0115]
[0116] Physical and mechanical testing
[0117] Specific gravity and absorption
[0118] Table 8 lists the specific gravity and absorption capacity of untreated and carbon dioxide treated RCA samples under all treatment conditions in accordance with ASTM C127. Pressure is expressed in pounds per square inch gauge (psig). The results show that under various treatment conditions, the specific gravity and absorption capacity of the RCA samples did not change significantly after carbon dioxide treatment.
[0119] Table 8. Specific gravity and absorption capacity of untreated and CO2 treated RCA samples
[0120]
[0121]
[0122] Aggregate Crushing Value (ACV)
[0123] Based on the modified BS110-812 standard, the ACV index of untreated and CO2-treated RCA samples under different treatment conditions was measured. Figure 5 All measured ACV indices for all treatment conditions were combined. The results show that the ACV index decreased in the RCA samples treated with CO2 under all treatment conditions. Among all the results, the ACV values of SPB10 and SPB20 showed relatively low values, mainly related to the higher contact surface between the RCA samples and the carbon dioxide in the basket and the longer treatment time.
[0124] LA Wear
[0125] The mass loss of the untreated and CO2 treated RCA samples after LA abrasion testing was measured using ASTM C131 standard. Fig. 6A ,6B 7 show this mass loss for RCA samples treated for SPB10 & 20 and CPB20 conditions, respectively. Note that the LA abrasion mass loss for limestone aggregate is about 26.8%. The results clearly show the effect of carbonization treatment of RCA on the reduction of mass loss.
[0126] Freeze-thaw (FT) resistance
[0127] The mass loss of untreated and carbon dioxide treated RCA samples after freeze-thaw (FT) resistance testing was measured based on CSA A23.2-24A standard. Fig. 8A , 8B 9 show this mass loss for RCA samples treated under SPB10 & 20 and CPB20 treatment conditions for various CO2 pressures, respectively. The dashed line depicts the FT mass loss of limestone aggregate (2.63%). A clear trend of decreasing mass loss as higher treatment pressures are applied is shown in the results.
[0128] Chemical and Environmental Testing
[0129] As environmental tests, phenolphthalein pH indicator test and batch percolation test were performed on untreated and CO2 treated RCA samples. These tests were designed to evaluate the environmental improvement effect of CO2 treatment process on RCA samples under various conditions. In the following sections, the results of phenolphthalein test, leachate pH and leachate ion concentration are presented respectively.
[0130] pH of RCA treated with CO2 (phenolphthalein test)
[0131] The phenolphthalein test is a quick and easy method to roughly evaluate the acidity or alkalinity of the surface and cross-section of RCA samples. In this way, six RCA samples were randomly selected, and then phenolphthalein solution was dropped on the surface of three samples, and the other three samples were broken with a hammer and phenolphthalein was dropped on the freshly cut surface to evaluate the penetration depth of carbon dioxide treatment.
[0132] Leachate water: pH
[0133] For each treatment condition, 6 RCA leachate water samples were collected after 1 day, 2 days, 4 days, 7 days, 14 days and 21 days. The water samples were all alkaline (basic) and showed a trend of increasing pH over time, although the original (untreated) sample had the highest pH for a given time and treatment pressure. Based on the EPA National Secondary Drinking Water Regulations (NSDWR), the standard pH for drinking water is between 6.5 and 8.5.
[0134] Leachate water: heavy metals
[0135] ICP-MS analysis was used to measure total elemental concentrations in RCA leachate water samples from day 1 to day 21. Heavy metal concentrations in leachate water from both untreated and CO2 treated samples from day 1 to day 21 were well below EPA Maximum Contaminant Levels (MCLs) for drinking water under all conditions.
[0136] Properties of concrete with CO2-treated RCA
[0137] Fresh concrete testing
[0138] (1) Slump test
[0139] Concrete slump is measured according to ASTM C143 (Standard Test Method for Slump of Hydraulic Cement Concrete) to measure the consistency of concrete. The test is performed immediately after the concrete is mixed.
[0140] (2) Air content test
[0141] The air content of the mixture was measured and determined according to ASTM C138 (Standard Test Method for Density (Unit Weight), Yield, and Air Content (Specific Gravity) of Concrete).
[0142] Table 9 summarizes the fresh concrete properties of the different concrete mixes. The results show that all mixes exhibit comparable properties regardless of whether natural aggregate or treated / untreated RCA is used. The mixes also exhibit reasonable workability and air content that meet Nebraska Department of Transportation specifications. Unit weights are expressed in pounds per cubic foot (pcf) in Table 9.
[0143] Table 9. Fresh concrete test results
[0144]
[0145]
[0146] *Specific gravity to determine air content
[0147] Hardened concrete testing
[0148] 1) Compressive strength
[0149] Based on ASTM C39 (Standard Test Method for Compressive Strength of Cylindrical Concrete Specimens), three 4-inch by 8-inch (10 cm×20 cm) cylinders of each mix were tested for compressive strength at 28 days of age. All samples were mechanically end-grounded before each test. A compressor with a capacity of 400 kips (1,779 kN) was used.
[0150] Fig.10 The compressive strength of different mixes was demonstrated. The results show that for pavement concrete applications, all mixes had a minimum compressive strength of 3500 psi (24 MPa) at 28 days. The use of RCA resulted in a slight decrease in compressive strength. However, a clear trend of increasing compressive strength with increasing CO2 treatment pressure was observed, with the 20 psig, 40 psig, and 60 psig (138 kPa, 276 kPa, and 414 kPa, respectively) treatment pressures used in this study resulting in compressive strengths comparable to the reference mix with natural aggregate.
[0151] 2) Flexural strength (modulus of rupture)
[0152] One 6-inch by 6-inch by 20-inch (15-cm×15-cm×51-cm) beam of each mix was tested for modulus of rupture at 28 days of age in accordance with ASTM C78 (Standard Test Method for Flexural Strength of Concrete (Using a Simply Supported Beam with Third Point Loading)). A flexural testing machine with a 30 kips (133 kN) capacity was used.
[0153] Fig.11 Demonstration of flexural strength (modulus of rupture) of different mixtures. The results show that for pavement concrete applications, all mixtures, except for the mixture with untreated RCA, have a minimum modulus of rupture of 600psi (4MPa) at 28 days. Similar to the results from the compressive strength test, the use of RCA results in a slight decrease in compressive strength. However, a trend of significant increase in flexural strength with the increase of CO2 treatment pressure was observed, with the 40psig (276kPa) and 60psig (414kPa) treatment pressures used in this study resulting in flexural strength comparable to the reference mixture with natural aggregate.
[0154] 3) Static elastic modulus and Poisson’s ratio test
[0155] The elastic modulus test was performed at 28 days of age according to ASTM C469 (Standard Test Method for Static Elastic Modulus and Poisson's Ratio of Compressed Concrete). A frame with two dial gauges to monitor both axial and radial deformations was used. Each test was recorded and later used to construct a graph from which the corresponding properties were calculated.
[0156] Fig.12 The elastic modulus and Poisson's ratio of different mixes are presented. The results show that the use of RCA leads to a slight decrease in the elastic modulus and Poisson's ratio. It is noteworthy that the properties do not have any significant impact on the design of concrete. Unlike the compressive strength and flexural strength, no clear trend of the effect of CO2 treatment was observed.
[0157] 4) Surface and volume resistivity
[0158] Based on AASHTO TP95 (Standard Test Method for Surface Resistivity Indication of Concrete's Resistance to Chloride Ion Penetration), a 4 inch by 8 inch (10 cm x 20 cm) cylindrical sample was randomly selected from each mix for surface and volume resistivity testing using a Proceq Resipod test device at 28 days. Resipod works on the Wenner probe principle and measures the resistivity of concrete. Before testing, the sample is fully saturated. Current is applied through the outer probe, while the inner probe measures the voltage.
[0159] Fig.13 Surface and volume resistivities of all mixes are demonstrated. The use of RCA resulted in a slight decrease in surface and volume resistivities, with the untreated RCA mix showing the lowest resistivities. However, a clear trend of increasing surface and volume resistivities with increasing CO2 treatment pressure was observed, with the 20 psig, 40 psig, and 60 psig (138 kPa, 276 kPa, and 414 kPa, respectively) treatment pressures used in this study resulting in surface and volume resistivities comparable to those of the reference mix with natural aggregate.
[0160] Analysis and Discussion
[0161] A detailed analysis based on experimental data during the CO2 treatment process and subsequent mechanical and environmentally relevant laboratory tests on CO2 treated samples is presented here. In the following sections, the treatment and laboratory results are analyzed based on CO2 mass consumption calculations, operational statistical analysis, cost analysis and CO2 footprint.
[0162] CO2 mass consumption
[0163] Individual carbon dioxide pressure drop data may not be a comprehensive indicator of carbon dioxide gas consumption. Temperature and RCA volume may be key factors to be considered when considering gas consumption. Therefore, carbon dioxide mass consumption is calculated to evaluate the amount and rate of carbon dioxide gas consumption during the treatment process under different treatment conditions, and then the carbon dioxide mass consumption is normalized by the initial RCA mass under each treatment condition. Carbon dioxide mass consumption may be one of the main indicators of the intensity and magnitude of the quantified carbon dioxide treatment process. In this regard, the density of carbon dioxide at the beginning of the test (Equations 6 to 12) is calculated using the Peng and Robinson equations of state based on the initial carbon dioxide pressure and temperature inside the treatment. Then, the initial mass of carbon dioxide in the chamber is calculated by multiplying the carbon dioxide density by its volume, wherein the initial CO2 volume is obtained using the internal chamber volume and the RCA volume. Similarly, the carbon dioxide mass at any time after the treatment process begins is also calculated using the same procedure. The carbon dioxide mass difference between the initial (t_0) and the time (t_1 to t_n) after the start of the test can represent the carbon dioxide mass consumption during the RCA treatment. In all the medium-scale and laboratory-scale processing tests, the initial volume of the RCA sample in the chamber may not be the same. Therefore, the amount of carbon dioxide gas consumption is normalized by the initial mass of RCA in the chamber. In this way, the amount and rate of carbon dioxide gas consumption under all processing conditions can be easily compared. In this section, carbon dioxide consumption graphs related to various medium-scale and laboratory-scale processing conditions are presented.
[0164]
[0165] Z 3 -(1-B)Z 2 +(A-3B 2 -2B)Z-(AB-B 2 -B 3 )=O (11)
[0166]
[0167] Where P is the chamber pressure [Pa], R is the universal gas constant = 8.3145 [J.mol -1 .k -1 ], T is the chamber temperature [K], Tr is the relative humidity (=T / T crit ), α is the attraction parameter, and Z is the compressibility factor [-]. For pure carbon dioxide gas, p crit =73.8[bar], T crit =304.2[K], m=0.6877, n=0.3813, ρ is the CO2 density [kg / m 3] and M is the molar mass of CO2 = 0.04401 [kg / mol].
[0168] Medium Scale CO2 Treatment
[0169] Various treatment conditions were applied using the prototype to evaluate the effect of each parameter on the physical / mechanical properties and CO2 consumption potential of the RCA samples. Fig.14A , 14B 15 show the normalized carbon dioxide gas consumption under SPB10, SPB20 and SPD20 processing conditions, respectively. Due to the continuous supply of carbon dioxide to the chamber, the exact amount of carbon dioxide mass consumption for the processing condition with continuous carbon dioxide pressure supply (CPB20) cannot be accurately calculated. However, based on the results calculated for the SPB condition, the carbon dioxide consumption is roughly estimated for the CPB20 condition.
[0170] The results of carbon dioxide mass consumption for different processing conditions show that the gas consumption increases in the order of SPB10, SPB20, and SPD20. It can be explained that the initial volume of carbon dioxide in the chamber and the contact area between the RCA sample and the carbon dioxide play an important role in the gas consumption during the processing process. Under the condition SPB10 with a lower volume of RCA and a higher amount of carbon dioxide gas, carbon dioxide can be more easily absorbed into the RCA, and therefore, faster carbonization can occur ( Fig.14A and 14B On the other hand, in addition to the CO2 / RCA volume, the arrangement of the RCA sample in the chamber can play an important role during the CO2 treatment process and CO2 mass consumption. Under conditions with a simple loose loading arrangement ( Fig.15 ), the gas consumption was lower, which may be attributed to the limited contact area between the RCA sample and CO2 in the chamber.
[0171] Since the carbon dioxide / RCA volume ratios for conditions SPB20 and CPB20 were similar, the carbon dioxide consumption at CPB20 was roughly calculated based on the SPB20 data, as shown in Table 10.
[0172] Table 10. CO2 gas consumption estimates for CPB20 processing conditions based on mass consumption calculated for SPB20 processing conditions
[0173]
[0174] Laboratory scale CO2 treatment
[0175] The Peng & Robinson equation of state (EOS) was also used to evaluate the carbon dioxide mass consumption for various processing conditions using the two sized chambers.
[0176] 10L capacity chamber
[0177] Similar calculations were used to calculate the CO2 mass consumption for the smaller laboratory scale chamber. The initialization method was the only variable examined using the smaller chamber. Fig.16A , 16B , 17A and 17B show the carbon dioxide mass consumption during carbon dioxide treatment of the RCA for different initial set pressures with initial CO 2 vacuum and CO 2 flush, respectively. Fig.16A and 16B Carbon dioxide mass consumption for all process pressures using the CO2 vacuum initialization method is shown and normalized by the RCA mass. Fig.17A and 17B Carbon dioxide mass consumption for all treatment pressures using the CO2 flushing initialization method is shown and normalized by the RCA mass.
[0178] The carbon dioxide consumption results for both the CO2 vacuum initialization method and the CO2 flushing initialization method are relatively similar. Therefore, the CO2 flushing method is selected as the initialization method for the processing chamber with a 30L capacity chamber.
[0179] 30L capacity chamber
[0180] At laboratory scale, various treatment conditions were evaluated using a 30 L capacity chamber (see Table 3). Carbon dioxide mass consumption plots for each treatment variable are presented here to facilitate evaluation of the effectiveness of each treatment condition on carbon dioxide mass consumption.
[0181] Fig.18A and 18B The carbon dioxide mass consumption is shown for all treatment conditions with different average RH during treatment and normalized by the RCA mass. The solid line shows the increase in carbon dioxide mass consumption as the RH is increased from 1.88% up to 55.1%, and then the profile long dashed line shows the decrease in carbon dioxide mass consumption as the RH is increased above 55.1% until a maximum of 76.7%. At normal laboratory temperatures, the chamber does not allow the average RH to increase above 76.7%, and this is the maximum RH achieved.
[0182] The results showed that the maximum carbon dioxide consumption was achieved at a relative humidity of 50±5° C. These results confirm the optimal RH range for carbonization of RCA using carbon dioxide.
[0183] Fig.19A and 19BCarbon dioxide mass consumption for similar processing conditions (i.e., no silica gel and initial set pressure of 40 psig (276 kPa)) is shown at different processing temperatures and normalized by RCA mass. The solid line shows carbon dioxide mass consumption at typical laboratory temperature (21°C to 25°C), and the dashed and long dashed contour lines represent carbon dioxide mass consumption at a cooler temperature of about 3°C.
[0184] Temperature can be another key factor that affects chemical reactions and thus the carbonization process. In general geochemistry, chemical reactions become faster as ambient temperature increases. The results can indicate that the carbonization process and carbon dioxide consumption may be limited at lower temperatures (e.g., 3°C).
[0185] although Fig.19A and 19B The test conditions for all treatment embodiments presented in are similar (i.e., without silica gel), but the average RH inside the control chamber during treatment is different (3 ± 0.5 °C) due to the different dew points at different temperatures. Fig. 20A and 20B In FIG. 5 , the continuous solid line shows the carbon dioxide mass consumption for the treatment at laboratory temperature and using 150 g SG at the middle layer, and the dotted and dashed lines represent the carbon dioxide mass consumption for the treatment in a control chamber at a constant temperature of 3±0.5° C. and without silica gel (no SG). Fig. 20A and 20B Results for CO2 consumption for treatments with similar mean RH are presented in . This comparison supports that the CO2 consumption rate is still valid; therefore the carbonization process of RCA is slower at cooler temperatures.
[0186] Fig.21A and 21BThe carbon dioxide consumption of treatments with different sample preconditioning is presented in Figure 2 (W: washed, and N: RCA not washed. C: RCA placed in a control room for 24 hours before treatment, where RH = 50 ± 2%, and T = 22 ± 1 ° C, 24 hours, L: RCA placed in a laboratory, where RH = 58 ± 2% and T = 22 ± 1 ° C, O: RCA dried at 105 ° C for 24 hours before treatment). The lowest carbon dioxide consumption was obtained for the dried RCA sample. As is well known, the carbonization reaction requires the presence of moisture, in which CO2 can be dissolved, and the carbonization of RCA (and therefore carbon dioxide consumption) is limited when drying the RCA. Comparing these conditions with washing and drying in a control room (WC) and in a laboratory (WL), it is shown that the carbon dioxide consumption is lower for the WL conditions, which may be due to the higher initial moisture content and average RH. The results of washing and drying in the control room (WC) and not washing and drying in the laboratory (NL) show similar carbon dioxide consumption, which may be due to the similar average RH during treatment and the cleaned samples. Therefore, washing does not seem to affect the CO2 permeation and consumption rates.
[0187] refer to Fig. 22 One or more embodiments of the present disclosure may provide a method of processing recycled concrete aggregate (RCA). The method may include: loading the RCA into a chamber configured to form an airtight seal; airtightly sealing the chamber; flushing the interior of the chamber with a non-carbon dioxide gas; pressurizing the interior of the chamber with carbon dioxide gas; and monitoring and maintaining the temperature and relative humidity of the interior of the chamber until a predetermined condition is met.
[0188] In one or more embodiments, the method may further include at least one member of the group consisting of: washing the RCA by immersing the RCA in water at least once before loading the RCA; drying the RCA before loading the RCA, and stabilizing the temperature of the RCA before loading the RCA. Drying of the RCA may include blowing air over the RCA.
[0189] In one or more embodiments, flushing may include performing one or more of the following: pressurizing the chamber with carbon dioxide (at a low pressure of 2 to 3 psig (13.8 to 20.7 kPa)), followed by releasing the pressure by opening a purge valve to the exterior of the container, or evacuating the chamber. Pressurizing may include injecting an initial volume of carbon dioxide gas sufficient to raise the pressure inside the chamber to a predetermined level. In addition, additional carbon dioxide gas may be injected into the chamber to maintain the pressure inside the chamber at a predetermined level. In one or more embodiments, the purity of the carbon dioxide gas may be at least 99%.
[0190] In one or more embodiments, the predetermined condition may be the processing time or the pressure inside the chamber.
[0191] In one or more embodiments, the pressure inside the chamber can be maintained at a gauge pressure between 20 and 60 psig (138 and 414 kPa), the processing time can be between 4 and 12 hours, loading the RCA can include filling 10% to 20% of the volume of the chamber with RCA, the relative humidity within the chamber can be maintained between 40% and 60%, and the temperature within the chamber can be maintained between 20°C and 30°C.
[0192] In one or more embodiments, the treated recycled concrete aggregate (RCA) may be treated according to all or part of the methods described above.
[0193] One or more of the methods described above may be performed using a chamber as disclosed herein.
[0194] One or more embodiments of the present invention may provide a method for optimizing carbonization of recycled concrete aggregate (RCA). The method may include: performing multiple experiments on the carbonization of RCA while varying input parameters between consecutive experiments. Varying the input parameters may include: varying sample preconditioning to include or not include washing and drying the RCA before placing the RCA in a carbonization chamber; varying the carbonization temperature between 10 L and 2×10 4 L; changing the percentage of the volume of the carbonization chamber occupied by RCA between 1% and 50%; changing the temperature of the carbonization chamber between 0°C and 80°C; changing the relative humidity of the carbonization chamber between 10% and 75%; changing the gauge pressure of the carbon dioxide gas in the carbonization chamber between 1 psig and 100 psig (6.9 kPa and 690 kPa); changing the initial carbon dioxide pressurization or the continuous carbon dioxide pressurization; changing the flushing of the carbonization chamber by applying a vacuum or by at least one cycle of pressurization with carbon dioxide gas followed by depressurization; changing the distribution of the RCA in the carbonization chamber to include simple loose loading and in multiple baskets; changing the duration of carbonization between 1 hour and 72 hours; monitoring multiple parameters that vary over time during each experiment of treating RCA, the parameters including at least one member of the group consisting of the temperature of the carbonization chamber, the relative humidity of the carbonization chamber, the gauge pressure of the carbon dioxide gas in the carbonization chamber; the ratio of the mass of carbon dioxide to the mass of RCA; and the mass consumption of carbon dioxide.
[0195] The method may further include performing a plurality of experiments and measurements after the carbonization treatment (on the RCA). These experiments and measurements may include: specific gravity; absorption capacity; aggregate crushing value; Los Angeles abrasion; freeze-thaw resistance; phenolphthalein test; and laboratory batch percolation test. The laboratory batch percolation test may include measurements of pH and heavy metal concentrations, the heavy metals including at least one member of the group consisting of Pb-208, Se-78; Cd-112; Cr-52; and As-75.
[0196] The method may further include measuring properties of various concretes including various carbonized RCA mixtures. The properties may include compressive strength, modulus of rupture, modulus of elasticity, surface resistivity, and volume resistivity.
[0197] The method may further include acquiring data before, during and / or after each carbonization treatment; analyzing the acquired data using at least one member of the group consisting of univariate regression, multivariate regression, principal component analysis and singular value decomposition; and determining the optimal range and / or optimal values of multiple input parameters for the carbonization RCA for at least one property of the RCA after carbonization.
[0198] All references, including publications, patent applications, and patents, cited herein are hereby incorporated by reference to the same extent as if each reference was individually and specifically indicated to be incorporated by reference and was set forth in its entirety herein.
[0199] Unless otherwise indicated herein or clearly contradicted by the context, the use of the terms "one" and "an" and "the" and "at least one" and similar references in the context of describing the present invention (especially in the context of the following claims) should be interpreted as covering both the singular and the plural. Unless otherwise indicated herein or clearly contradicted by the context, the use of the term "at least one" followed by a list of one or more items (e.g., "at least one of A and B") should be interpreted as one item selected from the listed items (A or B) or any combination of two or more of the listed items (A and B). Unless otherwise specified, the terms "including", "having", "including" and "containing" should be interpreted as open terms (i.e., meaning "including but not limited to"). Unless otherwise indicated herein, the description of the range of values herein is intended only to be used as a shorthand method of individually referring to each individual value falling within the range, and each individual value is incorporated into the specification as if it were individually described herein. All methods described herein can be performed in any suitable order, unless otherwise indicated herein or otherwise clearly contradicted by the context. The use of any and all examples or exemplary language (e.g., "such as") provided herein is intended only to better illustrate the invention and does not limit the scope of the invention unless otherwise required. No language in the specification should be construed as indicating any non-claimed element is essential to the practice of the invention.
[0200] Preferred embodiments of the present invention are described herein, including the best mode known to the inventor for practicing the present invention. By reading the above description, changes in these preferred embodiments may become apparent to those of ordinary skill in the art. The inventor expects that the technician will adopt such changes where appropriate, and the inventor intends to practice the present invention in a manner different from that specifically described herein. Therefore, the present invention includes all modifications and equivalents to the subject matter described in the appended claims as permitted by applicable law. In addition, unless otherwise indicated herein or otherwise clearly contradictory to the context, any combination of the above elements in all possible variations thereof is encompassed by the present invention.
Claims
1. A method for processing recycled concrete aggregate (RCA), the method comprising: constructing a chamber configured to form a hermetic seal; loading the RCA into the chamber; hermetically sealing the chamber; pressurizing the interior of the chamber with carbon dioxide gas; monitoring the pressure and relative humidity of the interior of the chamber; and The pressure and the relative humidity are controlled until predetermined conditions are met. 2 . The method of claim 1 , wherein controlling the pressure and the relative humidity comprises setting at least one of the pressure and the relative humidity to a fixed value or an initial value range, and controlling the other until the predetermined condition is met.
3. The method of claim 1, wherein pressurizing comprises injecting a volume of carbon dioxide gas sufficient to raise the pressure within the interior of the chamber to a predetermined level. 4 . The method of claim 3 , wherein additional carbon dioxide gas is injected to maintain the pressure in the interior of the chamber at the predetermined level.
5. The method of claim 1, wherein the carbon dioxide has a purity of less than 99%.
6. The method of claim 1, wherein the purity of the carbon dioxide gas is at least 99%. The method according to claim 1 , wherein the predetermined condition is a processing time or a pressure of the interior of the chamber.
8. The method of claim 1, wherein: The pressure inside the chamber is maintained between 20 and 80 psig, and the treatment time is between 1 and 12 hours. Loading the RCA into the chamber includes providing airflow around the RCA, The relative humidity in the chamber is maintained between 40% and 60%, and The temperature within the chamber was maintained between 20°C and 30°C.
9. The method according to claim 1, further comprising: In the chamber, there is provided: at least one pressure sensor; and At least one relative humidity / temperature sensor; at least one dehumidifier; at least one system configured to collect water from at least one dehumidifier; At least one fan; At least one gas injection valve and at least one gas ejection valve are provided operably connected to the chamber.
10. A processed recycled concrete aggregate (RCA), comprising: an RCA loaded into the chamber and hermetically sealed within said chamber; and treating the RCA by exposing the RCA to a carbon dioxide-rich atmosphere at high pressure within the chamber, the temperature and relative humidity of the atmosphere being monitored and controlled until predetermined conditions are met, Wherein treating the RCA changes the proportions of constituent minerals in the RCA, the percentages of calcium carbonate and silicon dioxide increase due to the reaction between calcium hydroxide and calcium silicate hydrate and carbon dioxide.
11. The treated recycled concrete aggregate (RCA) according to claim 10, wherein: The pressure inside the chamber is maintained at between 20 and 80 psig, The processing time is between 1 and 12 hours. Loading the RCA into the chamber includes providing airflow around the RCA, The relative humidity in the chamber is maintained between 40% and 60%, and The temperature within the chamber was maintained between 20°C and 30°C.
12. A method for carbonizing recycled concrete aggregate (RCA), the method comprising: constructing a chamber configured to form a hermetic seal; loading the RCA into the chamber; hermetically sealing the chamber; pressurizing the interior of the chamber with carbon dioxide gas; monitoring the pressure, temperature and relative humidity of the interior of the chamber; and The pressure, the temperature and the relative humidity are controlled until predetermined conditions are met.
13. The method of claim 12, further comprising pre-conditioning the RCA by washing and / or drying the RCA prior to placing the RCA in the chamber.
14. The method of claim 12, further comprising monitoring the pressure in the chamber and maintaining the pressure in the chamber by injecting additional carbon dioxide gas into the chamber.
15. The method of claim 12, further comprising flushing the chamber by applying a vacuum or by at least one cycle of pressurization followed by depressurization with carbon dioxide gas.
16. A method for improving the mechanical and durability properties of Portland cement concrete (PCC), the method comprising treating recycled concrete aggregate (RCA) contained in the PCC according to the method of claim 12.
17. A method for improving the mechanical and durability properties of asphalt cement concrete (ACC), said method comprising treating recycled concrete aggregate (RCA) contained in said ACC according to the method of claim 12.
18. A system for processing recycled concrete aggregate (RCA), the system comprising: A chamber configured to form an airtight seal, the chamber comprising: At least 10L and no more than 3×10 4 the volume of L; and a door configured to form an airtight seal; at least one dehumidifier mounted in the chamber and configured to maintain relative humidity in the chamber; at least one system mounted in the chamber and configured to collect water from the at least one dehumidifier; at least one fan mounted in the chamber and configured to circulate CO2 gas and moisture within the chamber; at least one heating element; at least one pressure sensor mounted and configured to measure pressure within the chamber; at least one relative humidity / temperature sensor mounted and configured to measure relative humidity and temperature within the chamber; a carbon dioxide gas supply operably connected to the chamber via an injection valve; and A blow-off valve is mounted on the chamber and is configured to allow gas to leave the chamber.
Citation Information
Cited By
Recycled aggregate carbonization device and water absorption quantitative regulation and control method
CN118767895A