Hard alloy, and coated tool and cutting tool using same
By forming a rich deβ layer of iron metal on the surface of the crossing area of the cemented carbide, the problem of insufficient defect resistance of the cutting edge part of the cemented carbide is solved, and higher defect resistance and longer service life are achieved .
Patent Information
- Application Number
- CN202380028719.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-28
- Filing Date
- 2023-03-01
- Publication Date
- 2024-11-05
AI Technical Summary
The existing cemented carbide lacks defect resistance in the edges of the cutting edges, which is prone to cracks and collapses during the cutting process, resulting in a shortening of the tool service life.
The deβ layer consisting of only WC and iron metal is formed on the surface of the crossing area of the front blade surface and the back blade surface of the cemented carbide. The average thickness relationship of the deβ layer (b < a) is adjusted to improve defect resistance, and Combined with the honing process and the firing process, an intersection area of convex curved surface or planar shape is formed.
It significantly improves the defect resistance of cemented carbide, reduces the risk of defects on the cutting edge, extends the service life of the cutting edge, and maintains the sharpness of the cutting edge.
Smart Images

Figure CN118900926A_ABST
Abstract
Description
[0001] Cross-reference to related applications
[0002] This application claims the benefit of priority from Japanese Patent Application No. 2022-051034 filed on March 28, 2022, and the entire disclosure of the prior application is incorporated herein by reference. Technical Field
[0003] The present invention relates to cemented carbide and a coated tool and a cutting tool using the same. Background Art
[0004] Cemented carbide containing WC (tungsten carbide) as a hard phase is used for substrates in coated tools and for cutting tools such as end mills. Such cemented carbide is required to have defect resistance and the like.
[0005] As a cemented carbide with excellent defect resistance, for example, Japanese Patent No. 3235259 (Patent Document 1) records that a β-layer is present at the cutting edge of the cemented carbide, and also records the thickness of the β-layer. In addition, Japanese Patent No. 3656838 (Patent Document 2) does not record that a β-layer is present at the cutting edge of the cemented carbide, but records the thickness of the β-layer of the rake face and the flank face being adjusted. Summary of the invention
[0006] The cemented carbide of one unrestricted mode disclosed in the present invention has: a hard phase containing W and C; a solid solution phase containing W, C and Ti; and a binder phase containing an iron group metal. The surface of the intersection area between the front cutting edge and the back cutting edge in the cemented carbide has a de-β layer composed only of WC and iron group metal. The average thickness of the de-β layer of the front cutting edge in the intersection area is set to a, and the average thickness of the de-β layer of the back cutting edge in the intersection area is set to b. The relationship between a and b satisfies b <a。
[0007] A coated tool according to one non-limited aspect of the present disclosure includes: the above-mentioned cemented carbide; and a coating located on a surface of the cemented carbide.
[0008] A cutting tool according to one non-limited aspect of the present disclosure includes: a shank extending from a first end toward a second end and having a groove on the first end side; and the above-mentioned coated tool located in the groove. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 This is a perspective view of a cemented carbide showing one embodiment of the present disclosure which is not limited thereto.
[0010] Figure 2 yes Figure 1The cross-sectional view of the II section in the cemented carbide shown is a cross-sectional view orthogonal to the intersection region when viewed from the rake face (top view).
[0011] Figure 3 This is a cross-sectional view showing the vicinity of the surface of a coated tool according to one embodiment of the present disclosure which is not limited thereto.
[0012] Figure 4 This is a cross-sectional view showing the vicinity of the surface of a coated tool according to one embodiment of the present disclosure which is not limited thereto.
[0013] Figure 5 This is a perspective view showing a cutting tool according to one embodiment of the present disclosure which is not limited thereto. DETAILED DESCRIPTION
[0014] <Hard alloy>
[0015] Hereinafter, the unrestricted cemented carbide 1 of the present disclosure will be described in detail using the accompanying drawings. However, in the following referenced figures, for the convenience of description, only the main components required in the description of the embodiment are simplified. Therefore, the cemented carbide 1 may have any constituent components not shown in the referenced figures. In addition, the dimensions of the components in the figures do not faithfully show the dimensions of the actual constituent components and the dimensional ratios of the components. These aspects are also the same in the coated tool and cutting tool described later.
[0016] The cemented carbide 1 may have a hard phase, a solid solution phase, and a binder phase.
[0017] The hard phase may contain W (tungsten) and C (carbon). In other words, the hard phase may contain WC. The hard phase may contain WC as a main component. The "main component" may refer to a component having the largest mass % value compared to other components. Specifically, the upper two mass % values of the components contained in the hard phase may be W and C.
[0018] The solid solution phase may contain W, C and Ti (titanium). The solid solution phase may contain W, C and Ti as main components. That is, in the solid solution phase, the total value of the mass % of W, C and Ti may be the largest. In addition, the top three values of the mass % of the components contained in the solid solution layer may be W, C and Ti.
[0019] The bonding phase may contain an iron group metal. Examples of the iron group metal include Co (cobalt) and Ni (nickel). The bonding phase may contain at least one of Co and Ni. The bonding phase may contain an iron group metal as a main component. The bonding phase can function as a phase that bonds adjacent hard phases. For an iron group metal including Co and Ni as an example, the mass % value of the component contained in the bonding phase can be the maximum.
[0020] The composition of each of the hard phase, the solid solution phase, and the binder phase can be measured, for example, by energy dispersive X-ray spectroscopy (EDS). The measurement can also be performed using EDS attached to an electron microscope. Examples of electron microscopes include scanning electron microscopes (SEM) and transmission electron microscopes (TEM).
[0021] like Figure 1 and Figure 2 As shown in the non-limiting example, the cemented carbide 1 may have a rake face 3 and a flank face 5. That is, the cemented carbide 1 may be in the shape of a cutting tool. In addition, the cemented carbide 1 may be in the shape of a plate. For example, the cemented carbide 1 may be as Figure 1 The shape of the cemented carbide 1 is not limited to a four-sided plate shape. In this case, the upper surface can be the rake face 3, and the side surface can be the back face 5. It should be noted that the shape of the cemented carbide 1 is not limited to the four-sided plate shape. For example, the rake face 3 can also be a triangle, a pentagon, a hexagon or a circle.
[0022] The cemented carbide 1 is not limited to a specific size. For example, the width D1 of the rake face 3 can be set to 3 to 20 mm. In addition, the width D2 of the flank face 5 can be set to 5 to 20 mm. The width D1 and the width D2 can be dimensions in a direction orthogonal to the intersecting ridgeline of the rake face 3 and the flank face 5.
[0023] The cemented carbide 1 may have an intersection region 7 between the front cutting edge 3 and the back cutting edge 5. The intersection region 7 is also the cutting edge ridge portion, and the cutting edge may be subjected to honing as the cutting edge treatment, and the portion subjected to the cutting edge treatment is used as the cutting edge ridge portion. The so-called honing treatment may be a processing method in which a grinding wheel (welding head) is pushed to rotate while being reciprocated for grinding. In other words, the intersection region 7 may also be an area in the intersection ridge portion between the front cutting edge 3 and the back cutting edge 5 that has been subjected to honing. Specifically, the area from the boundary portion L1 on the front cutting edge 3 side of the cutting edge ridge portion when viewed from the front cutting edge 3 (viewed from above) to the range S1 of the back cutting edge 5 and the area from the boundary portion L2 on the back cutting edge 5 side of the cutting edge ridge portion when viewed from the back cutting edge 5 (viewed from above) to the range S2 of the front cutting edge 3 may also be the intersection region 7 (refer to Figure 2 ).
[0024] It should be noted that, when it is difficult to identify the boundary L1, the position 80 μm from the flank face 5 when viewed from the rake face 3 may be regarded as the boundary L1. In addition, when it is difficult to identify the boundary L2, the position 60 μm from the rake face 3 when viewed from the flank face 5 may be regarded as the boundary L2.
[0025] The intersection region 7 may be a convex surface shape. It should be noted that the shape of the intersection region 7 is not limited to a convex surface shape. The intersection region 7 may, for example, be a plane shape that has been chamfered. It should be noted that the intersection region 7 as a plane shape is inclined relative to the front cutting edge 3 and the back cutting edge 5, so the end of the front cutting edge 3 side of the intersection region 7 and the end of the back cutting edge 5 side of the intersection region 7 can be easily determined, respectively. In addition, in the case where the intersection region 7 is a convex surface shape, the end of the front cutting edge 3 side of the intersection region 7 and the end of the back cutting edge 5 side of the intersection region 7 can be easily determined, respectively, based on the difference between the front cutting edge 3 and the back cutting edge 5 of the plane shape and the intersection region 7 as a convex surface shape.
[0026] The intersection region 7 may be located at a part of the intersection ridgeline portion between the rake face 3 and the flank face 5 or may be located at the entire intersection ridgeline portion. The intersection region 7 can be used for cutting a workpiece.
[0027] Cemented carbide 1 can be Figure 2 As shown in the non-limited example, the surface of the intersection region 7 has a de-β layer 9 composed only of WC and iron group metals. The de-β layer 9 is a layer rich in iron group metals such as Co and has high toughness, and can act as a layer that absorbs the impact generated between the workpiece and the workpiece during cutting and suppresses defects. Therefore, when the cemented carbide 1 has a de-β layer 9 on the surface of the intersection region 7, the intersection region 7 is not easy to be defective.
[0028] It should be noted that the de-β layer 9 composed only of WC and iron group metals means that the components constituting the de-β layer 9 are almost entirely WC and iron group metals. The de-β layer 9 may also contain impurities at a level that is unavoidable in the manufacturing process. The total content of impurities may be 3% by mass or less, in other words, the total value of WC and iron group metals may be 97% by mass or more.
[0029] The cemented carbide 1 may have a de-β layer 9 on the entire surface of the intersection region 7. In other words, the entire surface of the intersection region 7 of the cemented carbide 1 may be a de-β layer 9. In addition, the cemented carbide 1 may also have a de-β layer 9 on the surface other than the intersection region 7. The composition of the iron group metal in the de-β layer 9 may be the same as that of the iron group metal in the binder phase. Confirmation of the de-β layer 9 is performed, for example, by EDS.
[0030] Here, the average thickness of the β-depleted layer 9 of the rake face 3 in the intersection region 7 can be set as a, and the average thickness of the β-depleted layer 9 of the flank face 5 in the intersection region 7 can be set as b. Moreover, the relationship between a and b can satisfy b < a. In this case, it is difficult to generate cracks, chipping, etc. in the intersection region 7, and it is even more difficult for the intersection region 7 to be defective. Therefore, the carbide 1 has high resistance to defect.
[0031] The relationship between a and b can also satisfy 1 < a / b ≤ 2.5. In this case, it is easy to improve the resistance to defect of the carbide 1.
[0032] The relationship between a and b can also satisfy 1.5 ≤ a / b ≤ 2.5. In this case, it is easy to further improve the resistance to defect of the carbide 1.
[0033] The average thickness of the β-depleted layer 9 of the rake face 3 in the intersection region 7 can also be the average thickness of the β-depleted layer 9 at the end portion on the rake face 3 side of the intersection region 7 observed from the rake face 3. Therefore, the average thickness of the β-depleted layer 9 of the rake face 3 in the intersection region 7 can also be renamed as the average thickness of the β-depleted layer 9 in the region S1a at the end portion on the rake face 3 side of the intersection region 7. The region S1a can be, for example, a region at a distance of 10 μm from the boundary portion L1.
[0034] In addition, the average thickness of the β-depleted layer 9 of the flank face 5 in the intersection region 7 can refer to the average thickness of the β-depleted layer 9 at the end portion on the flank face 5 side of the intersection region 7 observed from the flank face 5. Therefore, the average thickness of the β-depleted layer 9 of the flank face 5 in the intersection region 7 can also be renamed as the average thickness of the β-depleted layer 9 in the region S2a at the end portion on the flank face 5 side of the intersection region 7. The region S2a can be, for example, a region at a distance of 5 μm from the boundary portion L2.
[0035] The measurement of the thickness of the β-depleted layer 9 can be carried out by cross-sectional observation using an electron microscope. The observed cross-section can be, for example, Figure 2 the cross-section shown. That is, the observed cross-section can also be a cross-section orthogonal to the intersection region 7 when viewed from above the rake face 3 (top view). Moreover, in this cross-section, the thickness of the β-depleted layer 9 can be measured at five or more measurement points at intervals of 1 μm within a width range of 5 μm or more at any position in the region S1a or the region S2a, and its average value can be calculated.
[0036] a and b are not limited to specific thicknesses. For example, a can be set to 7.3 - 14.3 μm. In addition, b can be set to 2.9 - 13 μm.
[0037] The average thickness of the β-removed layer 9 in the intersection region 7 may also decrease monotonically from the rake face 3 side toward the flank face 5 side. When the average thickness of the β-removed layer 9 is the above structure, cracks and breakage are less likely to occur in the intersection region 7, and the intersection region 7 is less likely to be defective.
[0038] In addition, the intersection region 7 may also have a region between the end on the front cutting face 3 side and the end on the back cutting face 5 side and the average thickness of the β-debonded layer 9 is c. In other words, the intersection region 7 also has another region between the region S1a and the region S2a, and the average thickness of the β-debonded layer 9 in this region may be c. In this case, c may be smaller than a and b. When the average thickness of the β-debonded layer 9 is the above-mentioned structure, the β-debonded layer 9 at the tip of the blade can be made thinner, so the sharpness of the tip of the blade can be ensured.
[0039] like Figure 2 As shown in the non-limited example, when the cross-section region 7 is a convex curved surface, the region where the average thickness of the β-free layer 9 is c can be located at the position with the smallest curvature radius in the cross-section region 7. Specifically, the curvature radius of the cross-section region 7 in the region where the average thickness of the β-free layer 9 is c can be smaller than the curvature radius of the cross-section region 7 in the region S1a and the region S2a. When the cross-section region 7 is the above-mentioned structure, the blade tip can be sharpened and the sharpness of the blade tip can be ensured.
[0040] The region where the average thickness of the β-depleted layer 9 is c may also be located at a position closer to the back face 5 than the front face 3. In other words, the region where the average thickness of the β-depleted layer 9 is c may also be located at a position closer to the back face 5 than the front face 3. In this case, the advantage of increasing the thickness of the β-depleted layer 9 on the front face 3 and improving the defect resistance can be obtained.
[0041] The width of the intersection region 7 when viewed from the rake face 3 may be larger than the width of the intersection region 7 when viewed from the flank face 5. In this case, by increasing the curvature radius of the honing of the rake face 3, an advantage of improved fracture resistance can be obtained.
[0042] <Method for manufacturing cemented carbide>
[0043] Next, a method for producing a cemented carbide according to one embodiment of the present disclosure, which is not limited thereto, will be described by taking a case where the cemented carbide 1 is produced as an example.
[0044] First, as raw material powders, WC powder, Co powder, TiC powder, etc. can be prepared. The ratio of Co powder can be 4 to 12% by mass. In addition, the ratio of TiC powder can be 0.5 to 15% by mass. The balance can also be WC powder.
[0045] The average particle size of the raw material powder can be appropriately selected within the range of 0.1 to 10 μm. The average particle size of the raw material powder can be a value measured by the Microtrac method.
[0046] The prepared raw material powders can be mixed and formed in such a way as to have a rake face 3 and a flank face 5 to obtain a formed body. At this time, the intersection ridge line portion of the rake face 3 and the flank face 5 can also be pre-formed into a chamfered shape by die pressing. In this case, it is easy to form a β-phase depleted layer 9 on the surface of the intersection region 7. As the chamfer, it can include forming the intersection ridge line portion into a convex curved surface shape, a planar shape.
[0047] The obtained formed body can be subjected to a debinding treatment and then sintered to obtain a cemented carbide 1. The sintering can be carried out in a non-oxidizing atmosphere such as a vacuum, an argon atmosphere, and a nitrogen atmosphere. The sintering temperature can be 1450 to 1600 °C. The sintering time can be 0.5 to 3 hours. When sintering is carried out at such a sintering temperature and sintering time, it is easy to form a β-phase depleted layer 9 on the surface of the cemented carbide 1.
[0048] The obtained cemented carbide 1 can also be subjected to a honing treatment to form the intersection region 7 of the rake face 3 and the flank face 5. Then, the intersection region 7 can be ground in such a way that the relationship between a and b satisfies b < a to adjust the thickness of the β-phase depleted layer 9. The grinding can be carried out, for example, by brushing, sandblasting, and barrel polishing.
[0049] It should be noted that the above manufacturing method is an example of the method for manufacturing the cemented carbide 1. Therefore, of course, the cemented carbide 1 is not limited to the cemented carbide manufactured by the above manufacturing method.
[0050] <Coated cutting tool>
[0051] Next, taking the case of having the above-mentioned cemented carbide 1 as an example, use Figure 3 and Figure 4 to illustrate a coated cutting tool 101 of an unrestricted embodiment of the present disclosure.
[0052] The coated cutting tool 101, as an unrestricted example shown in Figure 3 and Figure 4 can have only the cemented carbide 1 and a coating 103 located on the surface of the cemented carbide 1. The coated cutting tool 101 can have the cemented carbide 1 as a substrate. When the coated cutting tool 101 has the cemented carbide 1, the cemented carbide 1 has high resistance to chipping, so cutting performance such as interrupted cutting performance is easily improved. Therefore, the coated cutting tool 101 has high durability.
[0053] The coating 103 can be located on the entire surface of the cemented carbide 1, and in addition, it can also be located only on a part. That is, the coating 103 can also be located on at least a part of the surface of the cemented carbide 1.
[0054] The coating 103 can be formed by chemical vapor deposition (CVD). In other words, the coating 103 can also be a CVD film. It should be noted that the coating 103 can also be a PVD film formed by physical vapor deposition (PVD).
[0055] The coating layer 103 may be a single-layer structure or a structure in which a plurality of layers are stacked. Examples of the composition of the coating layer 103 include TiCN (titanium carbonitride), Al2O3 (aluminum oxide), and TiN (titanium nitride).
[0056] The coating 103 may also be Figure 3 As shown in the non-limiting example, the TiCN layer 105 and the Al2O3 layer 107 are provided in this order from the cemented carbide 1. The TiCN layer 105 may be in contact with the cemented carbide 1. The Al2O3 layer 107 may be in contact with the TiCN layer 105.
[0057] The coating 103 may also be Figure 4 As shown in the non-limiting example, the TiN layer 109, the TiCN layer 105 and the Al2O3 layer 107 are provided in order from the cemented carbide 1. The TiN layer 109 may be in contact with the cemented carbide 1. The TiCN layer 105 may be in contact with the TiN layer 109. The Al2O3 layer 107 may be in contact with the TiCN layer 105.
[0058] The coating 103 is not limited to a specific thickness. For example, the thickness of the TiCN layer 105 can be set to about 1.0 to 15 μm. The thickness of the Al2O3 layer 107 can be set to about 1 to 15 μm. The thickness of the TiN layer 109 can be set to about 0.1 to 5 μm. The thickness of the coating 103 can be measured by cross-sectional observation using an electron microscope. In addition, the thickness of the coating 103 can be an average value. For example, the thickness can be measured at any position of each layer at a width range of more than 10 μm at intervals of 1 μm at more than 10 measurement points, and the average value can be calculated.
[0059] The coated tool 101 may have a through hole 111. Figure 1 The through hole 111 is shown in FIG. The through hole 111 can be used to install a fixing screw or a clamping member when the coated tool 101 is held in the tool holder. The through hole 111 can be formed from the upper surface (front blade surface 3) to the lower surface located on the opposite side of the upper surface, and can also be opened on these surfaces. It should be noted that there is no problem even if the through hole 111 is opened in the mutually opposing areas of the side surface (flank blade surface 5).
[0060] <Method for manufacturing coated tool>
[0061] Next, a method for manufacturing a coated tool according to one embodiment of the present disclosure, which is not limited thereto, will be described by taking a case where the coated tool 101 is manufactured as an example.
[0062] The coated tool 101 can be obtained by forming a coating 103 on the surface of the cemented carbide 1 by a CVD method.
[0063] The TiCN layer 105 can be formed as follows. First, as a reaction gas composition, a mixed gas consisting of 0.1 to 10 volume % titanium tetrachloride (TiCl4) gas, 10 to 60 volume % nitrogen (N2) gas, 0.1 to 15 volume % methane (CH4) gas, and the remainder hydrogen (H2) gas can be adjusted. Then, the mixed gas is introduced into the chamber, the temperature is set to 800 to 1100°C, and the pressure is set to 5 to 30 kPa, and the TiCN layer 105 can also be formed.
[0064] The Al2O3 layer 107 can be formed as follows. First, as a reaction gas composition, a mixed gas consisting of 0.5 to 5 volume % aluminum chloride (AlCl3), 0.5 to 3.5 volume % hydrogen chloride (HCl) gas, 0.5 to 5 volume % carbon dioxide (CO2) gas, 0.5 volume % or less hydrogen sulfide (H2S) gas, and the rest hydrogen (H2) gas can be adjusted. Then, the mixed gas can be introduced into the chamber, the temperature can be set to 930 to 1010°C, and the pressure can be set to 5 to 10 kPa to form the Al2O3 layer 107.
[0065] The TiN layer 109 can be formed as follows. First, as a reaction gas composition, a mixed gas consisting of 0.1 to 10 volume % titanium tetrachloride (TiCl4) gas, 10 to 60 volume % nitrogen (N2) gas, and the remainder hydrogen (H2) gas can be adjusted. Then, the mixed gas can be introduced into the chamber, the temperature can be set to 800 to 1010°C, and the pressure can be set to 10 to 85 kPa to form the TiN layer 109.
[0066] It should be noted that the above-mentioned manufacturing method is an example of a method for manufacturing the coated tool 101. Therefore, the coated tool 101 is of course not limited to the coated tool manufactured by the above-mentioned manufacturing method.
[0067] <Cutting tools>
[0068] Next, the case of using the coated tool 101 as an example is given. Figure 5 A cutting tool 201 according to one embodiment of the present disclosure which is not limited thereto will be described.
[0069] The cutting tool 201 may be Figure 5 As shown in the non-limiting example, the cutting tool 201 includes a tool holder 203 extending from a first end 203a toward a second end 203b and having a tool groove 205 on the first end 203a side, and a coated tool 101 located at the tool groove 205. When the cutting tool 201 includes the coated tool 101, the coated tool 101 has high durability, so the cutting tool 201 has high wear resistance and can perform stable cutting.
[0070] The knife groove 205 may be a portion for mounting the coated tool 101. The knife groove 205 may be open on the outer peripheral surface of the tool handle 203 and the end surface on the first end 203a side.
[0071] The coated tool 101 can be mounted on the knife groove 205 in such a manner that the intersection region 7 protrudes outward from the tool handle 203. In addition, the coated tool 101 can be mounted on the knife groove 205 by a fixing screw 207. That is, the coated tool 101 can also be mounted on the knife groove 205 by inserting the fixing screw 207 into the through hole 111 of the coated tool 101, inserting the front end of the fixing screw 207 into the threaded hole formed in the knife groove 205, and screwing the screw parts together. At this time, the lower surface of the coated tool 101 can be in direct contact with the knife groove 205, and a sheet material can be clamped between the coated tool 101 and the knife groove 205.
[0072] Examples of the material of the handle 203 include steel and cast iron. When the material of the handle 203 is steel, the handle 203 has high toughness.
[0073] exist Figure 5 In the example shown, a cutting tool 201 used for so-called turning processing is illustrated. As turning processing, for example, inner diameter processing, outer diameter processing, and grooving processing can be cited. It should be noted that the use of the cutting tool 201 is not limited to turning processing. For example, there is no problem in using the cutting tool 201 for milling processing.
[0074] Hereinafter, the present disclosure will be described in detail with reference to examples, but the present disclosure is not limited to the following examples.
[0075] Example
[0076] [Sample No. 1 to 6]
[0077] <Production of cemented carbide>
[0078] First, WC powder with an average particle size of 9 μm, Co powder with an average particle size of 1.5 μm, and TiC powder with an average particle size of 1.5 μm were prepared as raw material powders. The average particle size of the raw material powders was a value measured by the Microtrac method.
[0079] Next, 7 mass % of Co powder, 2 mass % of TiC powder and the balance of WC powder were mixed and pressed into a cutting tool shape (CNMG120408) with a rake face and a flank face to obtain a molded body. At this time, for Samples No. 1 to 5, the intersection of the rake face and the flank face was chamfered into a convex curved shape by die pressing.
[0080] The obtained compact was subjected to a binder removal treatment and then sintered at 1500° C. for 1 hour to obtain a cemented carbide. The obtained cemented carbide was then subjected to a honing treatment to form an intersection region between the rake face and the flank face.
[0081] The composition of the obtained cemented carbide was measured by EDS. Specifically, the composition was measured by cross-sectional observation using EDS attached to SEM at a magnification of 5000 to 20000 times and the average value of measurements at 5 locations was obtained.
[0082] The results of EDS measurement showed that the obtained cemented carbides all had a hard phase containing W and C as main components, a solid solution phase containing W, C and Ti as main components, and a binder phase containing an iron group metal (Co) as main component. In addition, the cemented carbides of Samples No. 1 to 5 had a de-β layer consisting only of WC and an iron group metal (Co) on the entire surface of the intersection area.
[0083] For Samples No. 1 to 5, the intersection region was polished (brushed or sandblasted) so that a and b had the values shown in Table 1. The values of a and b shown in the column "Average thickness of β-depleted layer in intersection region" in Table 1 were measured by the method exemplified above.
[0084] <Evaluation>
[0085] The obtained cemented carbide was evaluated for cutting. Specifically, a TiN layer with a thickness of 1 μm, a TiCN layer with a thickness of 10 μm, and an Al2O3 layer with a thickness of 6 μm were formed from the cemented carbide (substrate) by CVD method to make a coated tool, and then the cutting evaluation was performed under the following conditions. It should be noted that the thickness of each layer is an average value.
[0086] Processing method: Turning
[0087] Cutting speed: 150m / min
[0088] Feed: 0.4mm / rev
[0089] Cutting depth: 0.5mm
[0090] Cutting material: SCM440 Round rod
[0091] Processing status: WET
[0092] The evaluation results are shown in Table 1. In the evaluation results in Table 1, "the number of impacts until the blade edge is chipped" means the number of impacts until the blade edge is chipped during cutting, and may also be referred to as an intermittent performance evaluation.
[0093] [Table 1]
[0094]
[0095] Samples No. 1 to 4 have significantly improved stability compared to Samples No. 5 to 6. In particular, Sample No. 6 has no debonded β layer on the surface of the intersection area, has the least number of impacts, has low wear resistance at the tip, and is difficult to perform stable cutting as a cutting tool.
[0096] Description of reference numerals:
[0097] 1···Carbide
[0098] 3···Rake face
[0099] 5···Flanking surface
[0100] 7···Intersection area
[0101] 9···De-β layer
[0102] 101···Coated cutting tools
[0103] 103···Coating
[0104] 105···TiCN layer
[0105] 107···Al2O3 layer
[0106] 109···TiN layer
[0107] 111···Through hole
[0108] 201···Cutting tools
[0109] 203···Knife handle
[0110] 203a··First End
[0111] 203b··Second end
[0112] 205···Knife groove
[0113] 207···Fixing screw.
Claims
1. A cemented carbide having: hard phase, which contains W and C; a solid solution phase containing W, C and Ti; as well as A binder phase comprising an iron group metal, wherein The cemented carbide has a de-β layer consisting only of WC and an iron group metal on the surface of the intersection area of the rake face and the flank face in the cemented carbide, The average thickness of the β-depleted layer on the rake face in the intersection region is set to a, The average thickness of the β-depleted layer of the flank surface in the intersection region is set to b, The relationship between a and b satisfies b <a。 2. The cemented carbide according to claim 1, wherein: The relationship between a and b satisfies 1 that the average thickness of the debonded β layer in the intersection region decreases monotonically from the rake face side toward the flank face side.
3. The cemented carbide according to claim 1, wherein: The intersection region has a region between the end portion on the rake face side and the end portion on the flank face side and the average thickness of the de-β layer is c.
4. The cemented carbide according to claim 1, wherein: The c is smaller than the a and the b. The region where the average thickness of the β-free layer is c is located at the position where the radius of curvature is the smallest in the intersection region.
5. The cemented carbide according to claim 4, wherein: The region where the average thickness of the debonded β layer is c is located closer to the flank face side than to the rake face side.
6. The cemented carbide according to claim 4, wherein: The width of the intersection region when viewed from the rake face is larger than the width of the intersection region when viewed from the flank face.
7. The cemented carbide according to claim 1, wherein: The coated tool has:
8. A coated tool, wherein: The cemented carbide according to any one of claims 1 to 7; and The coating is located on the surface of the cemented carbide. The coating comprises, starting from the cemented carbide, a TiCN layer and an Al 2 O 3 layer in sequence.
9. The coated tool according to claim 8, wherein: The coating comprises, starting from the cemented carbide, a TiN layer, a TiCN layer, and an Al 2 O 3 layer in that order.
10. The coated tool according to claim 8, wherein: The cutting tool has:
11. A cutting tool, wherein: a knife handle extending from a first end toward a second end and having a knife groove on a side of the first end; and The coated cutting tool according to any one of claims 8 to 10, which is located in the cutting groove.