Identifying media and article

Through the combination of cholesteric regular material sheets and pattern-like phase difference layer design, the problems of high manufacturing cost and insufficient design of existing identification media are solved, and the identification media with high recognition functions and diversified appearance changes are realized, reducing the Manufacturing complexity.

CN118901029APending Publication Date: 2024-11-05ZEON CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028686.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-20
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing identification media requires wide band processing during the manufacturing process, which leads to high costs and difficulty in obtaining a silver appearance, and has limited design changes, which cannot meet various appearance changes and aesthetic requirements.

Method used

A combination of cholesteric regular material sheets with specific optical characteristics is used as the light reflective layer, and a pattern-like phase difference layer is formed through a specific structural design, so that silver appearance and various design changes can be obtained without wide banding processing.

Benefits of technology

The identification medium with high recognition function and design variation is realized, which reduces manufacturing costs and can display diverse appearance changes under different observation conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118901029A_ABST
    Figure CN118901029A_ABST
Patent Text Reader

Abstract

Provided is an identification medium having a light reflecting layer that reflects incident light into circularly polarized light, and a patterned phase difference layer that includes a region having a phase difference, the light reflecting layer is provided on the layer of the identification medium so that the region having the phase difference occupies a partial region of the display surface of the identification medium, the light reflecting layer includes a sheet (i) and a sheet (ii) as sheets of a material having cholesteric regularity, and the sheet (i) and the sheet (ii) have different colors. The rotation direction of the reflected light of the sheet (i) and the rotation direction of the reflected light of the sheet (ii) are different from each other. The invention also provides an article with the identification medium.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an identification medium for identifying the authenticity of an article, and an article having the identification medium. Background Art

[0002] In order to easily determine whether an item is genuine, an identification medium is usually provided on the item. The identification medium is required to have anti-counterfeiting properties and an identification function. The anti-counterfeiting properties of the identification medium mentioned here refer to the properties that the identification medium cannot be easily copied by conventional techniques such as printing using conventional materials. The identification function of the identification medium refers to the function of being able to distinguish a genuine identification medium from a counterfeit identification medium forged by conventional techniques with a high degree of reliability by some means.

[0003] In some known identification media, materials with cholesteric regularity are used as light reflecting layers (e.g., Patent Documents 1 and 2). When light is incident on a material with cholesteric regularity, only one component of its circular polarization component in a rotational direction can be reflected. Since such a property cannot be obtained by copying using conventional materials such as printing, such a property can be used to obtain an identification medium with high anti-counterfeiting performance and identification function.

[0004] There are many materials with cholesteric regularity, and their optical properties can be expressed by selecting the reflection center wavelength λc, the half-peak width Δλ of the reflection band, and their ratio Δλ / λc as indicators. Materials with relatively large Δλ / λc values ​​can be regarded as relatively wide-band materials, and materials with relatively narrow Δλ / λc values ​​can be regarded as relatively narrow-band materials.

[0005] As a main material having cholesteric regularity, a cholesteric resin layer can be cited. The cholesteric resin layer mentioned here is a layer of a material having a structure obtained by polymerizing and curing a polymerizable liquid crystal material capable of exhibiting a cholesteric liquid crystal phase in a state exhibiting a cholesteric liquid crystal phase.

[0006] In most cases, the object whose authenticity needs to be determined is of high value, so it is required to have excellent aesthetics. Therefore, the identification medium given to the object is also required to have excellent aesthetics. Specifically, the appearance during observation for showing the identification function (observation through a device such as a viewer, observation under polarized light, etc.), the appearance during ordinary observation other than this (observation with the naked eye under natural light without a device such as a viewer, etc.), or the appearance during these two observations is required to have excellent aesthetics. In the identification medium described in patent document 1, as part of its structural elements, a cholesteric resin layer after so-called broadband treatment is used. The cholesteric resin layer after broadband treatment can widen its reflection band to such an extent that it covers the entire visible light region. In this case, the layer can present a mirror-like silver appearance, and as a result, it can exert high design properties.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent document 1: International Publication No. 2021 / 153761 (corresponding publication: European Patent Application Publication No. 4099067);

[0010] Patent document 2: Japanese Patent Application Publication No. 2005-055556. Summary of the invention

[0011] Problem that the invention aims to solve

[0012] Based on the above situation, the identification medium for authenticity identification is required to have a better aesthetics than the existing known identification medium. In addition, in addition to the silver appearance, various appearances are also required, and the variation of the appearance change mode in the observation for showing the identification function is also required.

[0013] In addition, the broadband treatment of the cholesteric resin layer for obtaining the above-mentioned silver appearance is a known technology, but it requires precise and multi-stage processes such as irradiation with weak ultraviolet rays and heating. As a result, the cost of the material using the manufacturing method involving the broadband treatment becomes high. Therefore, there is a need for an identification medium that can be obtained even without broadband treatment and can obtain an appearance with excellent aesthetics such as a silver appearance.

[0014] Therefore, an object of the present invention is to provide an identification medium and an article which have a high identification function and can be easily manufactured, and which have many variations in the design properties in observations for expressing the identification function and can exhibit high design properties.

[0015] Solutions for solving problems

[0016] In order to solve the above problems, the present inventors studied the use of a cholesteric resin layer that can be obtained even without broadband treatment as a light reflecting layer as a main structural element, thereby obtaining an identification medium showing the same silver appearance as the cholesteric resin layer after broadband treatment. As a result, the present inventors found that the above problems can be solved by combining sheets of a material having cholesteric regularity and having specific optical characteristics in a specific manner as a light reflecting layer, thereby completing the present invention.

[0017] That is, the present invention includes the following contents.

[0018] [1] An identification medium comprising a light reflecting layer and a patterned phase difference layer,

[0019] The light reflecting layer is a layer that reflects incident light into circularly polarized light.

[0020] The patterned phase difference layer is a layer including a region having a phase difference, and is provided on the identification medium in such a manner that the region having a phase difference occupies a part of the display surface of the identification medium.

[0021] The light reflecting layer comprises sheets (i) and sheets (ii) as sheets of materials having cholesteric regularity,

[0022] The colors of the sheet (i) and the sheet (ii) are different from each other, and

[0023] The rotation direction of the light reflected by the sheet (i) and the rotation direction of the light reflected by the sheet (ii) are different from each other.

[0024] [2] The identification medium according to [1], wherein the light reflecting layer further includes a sheet (iii) as a sheet of the material having cholesteric regularity, and the sheet (iii) has a color different from that of either the sheet (i) or the sheet (ii).

[0025] [3] The identification medium according to [1] or [2], wherein the light reflecting layer satisfies the following formulas (b-1) to (b-2):

[0026] 0.90≤B(430-490)Ave / G(500-600)Ave≤1.05 Formula (b-1)

[0027] 0.90≤R(600-660)Ave / G(500-600)Ave≤1.05 Formula (b-2)

[0028] In the formula,

[0029] B(430-490)Ave is the average value of the integrated reflectivity of the light reflecting layer at wavelengths of 430nm to 490nm.

[0030] G(500-600)Ave is the average value of the integrated reflectivity of the light reflecting layer at a wavelength of 500nm to 600nm.

[0031] R(600-660)Ave is an average value of the integrated reflectance of the light reflecting layer at a wavelength of 600 nm to 660 nm.

[0032] [4] The identification medium according to [3], wherein the light reflecting layer satisfies the following formulas (b-1') to (b-2'):

[0033] 0.92≤B(430-490)Ave / G(500-600)Ave≤1.04 Formula (b-1')

[0034] 0.92≤R(600-660)Ave / G(500-600)Ave≤1.04 Formula (b-2').

[0035] [5] The identification medium according to any one of [1] to [4], wherein the light reflecting layer exhibits a color ranging from light coloring to silver.

[0036] [6] The identification medium according to any one of [1] to [5], wherein any one of the sheets of the material having cholesteric regularity in the light reflecting layer satisfies formula (c),

[0037] 0.10≤Δλ / λc≤0.25 Formula (c)

[0038] Wherein, Δλ is the half-peak width of the reflection band of the above-mentioned sheet, and λc is the selective reflection center wavelength of the above-mentioned sheet.

[0039] [7] The identification medium according to [6], wherein the pieces of the material having cholesteric regularity in the light reflecting layer all satisfy the above formula (c).

[0040] [8] The identification medium according to any one of [1] to [7], wherein the patterned phase difference layer is a λ / 4 wave plate or a λ / 2 wave plate.

[0041] [9] The identification medium according to any one of [1] to [8], wherein the thickness of the sheet is 3 μm or more and 7 μm or less.

[0042]

[10] The identification medium according to any one of [1] to [9], wherein the average particle size of each of the sheets is 100 μm or less.

[0043]

[11] The identification medium according to any one of [1] to

[10] , wherein the patterned phase difference layer is located closer to the viewing side than the light reflecting layer.

[0044]

[12] The identification medium according to any one of [1] to

[11] , wherein the light reflecting layer further includes a sheet having a reflection band including a region with a wavelength greater than 660 nm.

[0045]

[13] The identification medium according to any one of [1] to

[12] , wherein the average value of the integrated reflectance of the light reflecting layer at 430 to 660 nm is 20% or more.

[0046]

[14] The identification medium according to any one of [1] to

[13] , further comprising a light absorbing layer at a position on the opposite side of the light reflecting layer to the viewing side.

[0047]

[15] The identification medium according to any one of [1] to

[14] , wherein the identification medium has a covering layer at a position closer to the viewing side than the patterned phase difference layer.

[0048]

[16] The identification medium according to any one of [1] to

[15] , further comprising a mounting member for mounting the identification medium on an article.

[0049]

[17] An article having the identification medium according to any one of [1] to

[16] .

[0050] Effects of the Invention

[0051] According to the present invention, it is possible to provide an identification medium and an article which have a high identification function and can be easily manufactured, and which have many variations in the expression of design in observation for expressing the identification function and can exhibit high design. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 This is a perspective view schematically showing an example of the identification medium of the present invention.

[0053] Figure 2 To show that Figure 1 The illustrated identification medium is a longitudinal cross-sectional view of a state in which the identification medium is cut along line 1a. DETAILED DESCRIPTION

[0054] The present invention will be described in detail below by showing examples and embodiments. However, the present invention is not limited to the examples and embodiments shown below, and can be arbitrarily modified within the scope of the claims of the present invention and the scope equivalent thereto.

[0055] In the following description, unless otherwise specified, "(meth)acryloyl" refers to a term including "acryloyl", "methacryloyl" and a combination thereof. Similarly, "(thio)epoxy" refers to a term including "epoxy", "thioepoxy" and a combination thereof.

[0056] In the following description, unless otherwise specified, the in-plane retardation Re of a certain layer is a value represented by Re=(nx-ny)×d. Here, nx represents the refractive index in the direction perpendicular to the thickness direction of the layer (in-plane direction) providing the maximum refractive index. Ny represents the refractive index in the direction orthogonal to the nx direction in the above-mentioned in-plane direction of the layer. d represents the thickness of the layer. Unless otherwise specified, the measurement wavelength of the delay is 590nm. The in-plane retardation Re can be measured using a phase difference meter ("AxoScan" manufactured by AxoMetrix).

[0057] In the following description, unless otherwise specified, the direction of the slow axis of a certain layer means the direction of the slow axis in the in-plane direction.

[0058] In the following description, unless otherwise specified, the directions of the components being "parallel" and "perpendicular" may include errors within the range of, for example, ±4°, preferably ±3°, and more preferably ±1°, within the range that does not impair the effects of the present invention.

[0059] In the following description, for the sake of convenience, "right-handed circularly polarized light" and "left-handed circularly polarized light" are defined based on the following rotation direction: the rotation direction of circularly polarized light when the light emission target is observed from the light emission source. That is, when the light emission target is observed from the light emission source, polarized light whose polarization direction rotates clockwise as the light travels is defined as right-handed circularly polarized light, and polarized light whose polarization direction rotates in the opposite direction is defined as left-handed circularly polarized light.

[0060] In the following description, unless otherwise specified, the identification medium is described as being placed horizontally with the display surface facing upward. Therefore, the side from which the identification medium is viewed is sometimes referred to as the "upper" side, and the opposite side is referred to as the "lower" side. For example, the surface of one side surface and the other side surface of a layer that is closer to the display surface of the identification medium is sometimes referred to as the "upper" surface. In addition, the direction perpendicular to the "upper" and "lower" directions is sometimes referred to as the "horizontal" direction.

[0061] Observation of identification media includes observation for the purpose of developing identification functions under specific conditions (observation through a device such as an observer, observation under polarized light, etc.) and normal observation (observation under natural light with the naked eye without observation through a device such as an observer, etc.). In the following description, unless otherwise specified, observations other than those clearly specified as being for the purpose of developing identification functions and those that are clear from the context as being for the purpose of developing identification functions are considered normal observations.

[0062] [Overview of Identification Media]

[0063] The identification medium of the present invention comprises a light reflecting layer and a patterned phase difference layer.

[0064] Figure 1 This is a perspective view schematically showing an example of the identification medium of the present invention. Figure 2 To show that Figure 1 The longitudinal cross-sectional view of the identification medium after being cut along line 1a is shown. Figure 1 and Figure 2 As shown, the identification medium 100 sequentially comprises a light absorbing layer 110, a light reflecting layer 120, a patterned phase difference layer 140, and a coating layer 150, and further comprises a structure having adhesive layers 131 and 132 between the layers. Since the patterned phase difference layer 140 only covers a part of the display surface 160, the display surface 160 is provided with an area 160A covered by the patterned phase difference layer 140 and an area 160B not covered by the patterned phase difference layer 140.

[0065] The patterned phase difference layer is usually disposed at a position closer to the viewing side than the light reflecting layer. Therefore, the display surface of the identification medium is usually the surface on the patterned phase difference layer side of the identification medium.

[0066] In this example, an example is shown in which a flat glass plate without flexibility is used as the coating layer 150 and is pressed onto the light reflecting layer and the patterned phase difference layer 140 to form the identification medium 100. Therefore, the patterned phase difference layer 140 is embedded in the light reflecting layer 120. However, due to Figure 1 and Figure 2 For schematic illustration, the thickness of the layer is shown relatively large, so in an actual identification medium, the embedding may be so small that it cannot be seen. Figure 1 and Figure 2 The example shown has a different structure, which can suppress the embedding. For example, the material constituting the coating layer is not limited to a non-flexible material such as a glass plate, but can also be a flexible material such as a resin film. In addition, an optically isotropic transparent layer can also be arranged on the same plane as the patterned phase difference layer 140.

[0067] [Patterned phase difference layer]

[0068] The patterned phase difference layer is a layer including an area with a phase difference, and is provided on the identification medium in such a manner that the area with a phase difference occupies a part of the display surface of the identification medium. In the following description, the part of the patterned phase difference layer involving the area with a phase difference is sometimes referred to as a "phase difference layer".

[0069] In the display surface, the area other than the area occupied by a phase difference layer may be an area occupied by other phase difference layers having different phase differences, an area occupied by an isotropic layer having no phase difference, or an area where none of these exist. Figure 1 and Figure 2 In the example of FIG. 1 , the patterned phase difference layer 140 is a layer occupying only a partial area 160A of the display surface.

[0070] As examples of regions with phase difference, regions that function as λ / 4 wave plates and regions that function as λ / 2 wave plates can be cited. A region that functions as a λ / 4 wave plate refers to a region where the in-plane delay Re is λ / 4 or a value close to λ / 4 at at least one wavelength λ within the wavelength band in which the light reflecting layer functions. For example, a region where Re is ((λ / 4)×0.6)nm to ((λ / 4)×1.4)nm, and preferably a region where Re is ((λ / 4)×0.8)nm to ((λ / 4)×1.2)nm can be used as a region with phase difference. Similarly, a region that functions as a λ / 2 wave plate refers to a region where the in-plane delay Re is λ / 2 or a value close to λ / 2, such as a region where Re is ((λ / 2)×0.6)nm to ((λ / 2)×1.4)nm, and preferably a region where Re is ((λ / 2)×0.8)nm to ((λ / 2)×1.2)nm. The wavelength λ can be set to 590 nm, which is a wavelength near the center of visible light.

[0071] exist Figure 1 and Figure 2 In the example of FIG. 1 , the patterned phase difference layer 140 occupies only a partial region 160A of the display surface and functions as a λ / 4 wave plate as a whole.

[0072] Examples of patterned phase difference layers and more specific descriptions of the materials constituting the patterned phase difference layers will be described later.

[0073] [Light reflecting layer]

[0074] The light reflecting layer in the present invention is a layer that reflects the incident light into circularly polarized light. Specifically, the light reflecting layer is a layer that reflects a certain polarization component into circularly polarized light when non-polarized light containing various polarization components is incident. The light reflecting layer can be a right-handed reflective circular polarizer (i.e., a reflective circular polarizer that selectively reflects the right-handed circular polarization component in the incident light) or a left-handed reflective circular polarizer (i.e., a reflective circular polarizer that selectively reflects the left-handed circular polarization component in the incident light). However, this selective reflection only occurs in the reflection band in the entire wavelength band, and the reflected proportion depends on the reflectivity of each wavelength of the incident light. Most of the components in the incident light that are not reflected are transmitted through the light reflecting layer, and a part is absorbed by the light reflecting layer.

[0075] The light reflecting layer in the identification medium of the present invention includes a sheet (i) and a sheet (ii) of a material having cholesteric regularity. However, the sheets included in the light reflecting layer are not limited to these, and in addition to sheets (i) and (ii), sheets having cholesteric regularity other than these can also be included. The sheet has a granular structure obtained by crushing a layered structure, and the sheet of material having cholesteric regularity can be obtained by crushing a layered structure composed of a material having cholesteric regularity. As the layered structure, a cholesteric resin layer can be used. Such a sheet can preferably be made into particles with a flat structure by selecting and using those graded into appropriate particle sizes. In the case of the particles with a flat structure as structural elements of a layered structure, the surface that serves as the main surface before crushing can be easily arranged in the same direction as before crushing. Therefore, each sheet in the layered structure containing it can show the same optical properties as the cholesteric resin layer before crushing. Specific examples of cholesteric resin layers will be described separately later.

[0076] The average particle size of each sheet is preferably 100 μm or less, more preferably 75 μm or less. By having such a small particle size, they are not viewed as components with different colors on the display surface, but the optical properties of three or more sheets work together to present an appearance such as a silver pearlescent feeling, and high design properties, which is one of the effects of the present invention, can be obtained. The silver pearlescent appearance mentioned here refers to an appearance formed by uniformly distributing tiny particles having a color tone other than silver, such as red, green, and blue, and presents a design that can be reminiscent of pearl luster, unlike a uniform achromatic silver appearance.

[0077] On the other hand, the lower limit of the average particle size is preferably 10 μm or more, more preferably 25 μm or more. By having an average particle size greater than the above lower limit, the aspect ratio of the sheet can be made high, resulting in that the optical properties of the cholesteric resin layer before pulverization can be well manifested even in the sheet. In addition, the appearance of silver pearlescent feeling different from uniform achromatic silver can be well manifested.

[0078] The desired average particle size can be obtained by pulverizing the cholesteric resin layer and then classifying the pulverized product by an appropriate method.

[0079] The average particle size of the sheet can be obtained by measuring the particle size distribution of the sheet using a laser scattering method and obtaining the average particle size based on the particle size distribution. As a measuring instrument for the laser scattering method, a laser diffraction / scattering particle size distribution measuring device (e.g., LA-960 manufactured by Horiba Seisakusho) can be used. In the present invention, unless otherwise specified, the average value of the average particle size of the sheet can be a volume average.

[0080] The thickness of the sheet is preferably 3 μm or more, on the other hand, preferably 7 μm or less. By making the thickness above the lower limit, the desired optical effect such as high reflectivity can be well manifested. On the other hand, by making the thickness below the upper limit, the occurrence of poor orientation can be effectively suppressed. In addition, a sheet with a desired high aspect ratio can be easily obtained. The thickness of the sheet usually depends on the thickness of the cholesteric resin layer before pulverization. In the case where the thickness of the cholesteric resin layer before pulverization is uniform, the thickness of the obtained sheet can also be the same uniform value. However, in the case of deviation in thickness, the volume average value can be used as the thickness of the sheet.

[0081] For the aspect ratio of the sheet, the ratio obtained by dividing the average particle size of the sheet by the thickness of the sheet can be used as an index. The ratio is preferably 3 or more, more preferably 5 or more, particularly preferably 8 or more, preferably 40 or less, more preferably 30 or less, and particularly preferably 20 or less.

[0082] The sheets with cholesteric regularity contained in the light reflecting layer each have a specific reflection band. Therefore, each can have a half-peak width Δλ and a selective reflection center wavelength λc of a specific reflection band. The half-peak width Δλ refers to the difference between the maximum wavelength and the minimum wavelength in the wavelength region showing a reflectivity of 50% or more of the peak reflectivity in the reflection band. For example, in the case where the peak reflectivity is 40%, the half-peak width Δλ is the difference between the maximum wavelength and the minimum wavelength in the wavelength region showing a reflectivity of 20% or more. The selective reflection center wavelength λc is the average value of the maximum wavelength and the minimum wavelength (that is, the value of their total divided by 2). The units of Δλ and λc can usually be expressed in nm. The values ​​of Δλ and λc of the sheet are usually consistent with the values ​​of Δλ and λc of the cholesteric resin layer before crushing, so the values ​​of Δλ and λc of the cholesteric resin layer can be directly adopted as the Δλ and λc of the sheet.

[0083] In the present invention, the values ​​of Δλ and λc of a specific slice among the slices may be indicated by adding the symbol of the slice. For example, Δλ(i) and λc(i) respectively indicate the values ​​of Δλ and λc of slice (i).

[0084] As the reflectivity of the light reflecting layer and the sheet at each wavelength, the integral reflectivity measured using non-polarized light as the incident light can be used. The integral reflectivity can be measured using an ultraviolet visible spectrophotometer with an integrating sphere (e.g., "UV-Vis 770" manufactured by JASCO Corporation). Generally speaking, since the proportion of light diffusely reflected by the sheet is relatively large without specular reflection, the measured value of the integral reflectivity can be used as a good indicator.

[0085] The colors of the sheet (i) and the sheet (ii) are different from each other. Specifically, it is preferred that the difference between the selected center wavelength λc(i) of the sheet (i) and the selected center wavelength λc(ii) of the sheet (ii) is 70 nm or more. In addition, it is preferred that the selected center wavelength λc(i) of the sheet (i) and the selected center wavelength λc(ii) of the sheet (ii) belong to different regions among the three regions of 430 nm to 490 nm, 500 nm to 600 nm, and greater than 600 nm to 660 nm.

[0086] The rotation direction of the light reflected by the sheet (i) and the rotation direction of the light reflected by the sheet (ii) are different from each other. That is, when one of them is a sheet that reflects right-handed circularly polarized light, the other is a sheet that reflects left-handed circularly polarized light.

[0087] The light reflecting layer includes sheets satisfying the above conditions as sheets (i) and sheets (ii), so that the design of the light reflecting layer having a large change in observation for developing the identification function can be easily expressed. Specifically, in observation for developing the identification function, the change in the color of the latent image can be observed, and as a result, the identification function with high design can be expressed.

[0088] The light reflecting layer preferably satisfies the following formulae (b-1) and (b-2).

[0089] 0.90≤B(430-490)Ave / G(500-600)Ave≤1.05 Formula (b-1)

[0090] 0.90≤R(600-660)Ave / G(500-600)Ave≤1.05 Formula (b-2)

[0091] In the formula, B(430-490)Ave is the average value of the integrated reflectivity of the light reflecting layer at wavelengths of 430nm to 490nm, G(500-600)Ave is the average value of the integrated reflectivity of the light reflecting layer at wavelengths of 500nm to 600nm, and R(600-660)Ave is the average value of the integrated reflectivity of the light reflecting layer at wavelengths of 600nm to 660nm. The light reflecting layer satisfying formulas (b-1) and (b-2) can be obtained by adjusting the type and mixing ratio of the sheets constituting the light reflecting layer.

[0092] When the light reflecting layer satisfies the formulas (b-1) and (b-2), the light reflecting layer exhibits uniform reflection in a wide wavelength range within the visible light band, and as a result, can exhibit the same silver appearance as the cholesteric resin layer after the wide-band treatment. As a result, it can be obtained by an easy manufacturing method such as mixing sheets that can be manufactured relatively easily, and can exhibit high design properties.

[0093] From the viewpoint of more effectively obtaining the above-mentioned advantages, the light reflecting layer more preferably satisfies the following formulae (b-1′) to (b-2′).

[0094] 0.92≤B(430-490)Ave / G(500-600)Ave≤1.04 Formula (b-1')

[0095] 0.92≤R(600-660)Ave / G(500-600)Ave≤1.04 Formula (b-2')

[0096] The light reflecting layer preferably further includes a sheet (iii). Here, sheet (iii) is a sheet having a color different from that of any one of sheets (i) and (ii). Specifically, it is preferred that the difference between the selected center wavelength λc(i) of sheet (i) and the selected center wavelength λc(iii) of sheet (ii), and the difference between the selected center wavelength λc(ii) of sheet (ii) and the selected center wavelength λc(iii) of sheet (ii) are both 70nm or more. In addition, it is preferred that the selected center wavelength λc(i) of sheet (i), the selected center wavelength λc(ii) of sheet (ii), and the selected center wavelength λc(iii) of sheet (iii) all belong to different regions among the three regions of 430nm or more and 490nm or less, 500nm or more and 600nm or less, and greater than 600 and 660nm or less.

[0097] Since the rotation direction of the light reflected from the sheet (i) is different from the rotation direction of the light reflected from the sheet (ii), the rotation direction of the light reflected from the sheet (iii) must be different from one of them and the same as the other.

[0098] By including sheet (iii) in addition to sheets (i) and (ii) in the light reflecting layer, further changes can be obtained in the display of design in the observation for displaying the identification function. In addition, these sheets can work together to easily achieve selective reflection in a wide wavelength range. As a result, a light reflecting layer that satisfies formulas (b-1) and (b-2), or formulas (b-1') and (b-2') can be easily constructed, and a light reflecting layer that exhibits the same silver appearance as the cholesteric resin layer after broadband processing can be obtained, resulting in the ability to take into account both ease of manufacture and high design performance.

[0099] The light reflecting layer preferably has an appearance that presents a color ranging from light coloring to silver. Specifically, it is preferred that the a* value and b* value of the light reflecting layer are within ±5, respectively, and √(|a*|^2+|b*|^2)≤5. If the focus is on presenting a silver color, it is preferred that the a* value and b* value are within ±3, respectively, and √(|a*|^2+|b*|^2)≤3. In the prior art, a light reflecting layer presenting such an appearance is mainly realized by a cholesteric resin layer after a wide-band treatment, but the light reflecting layer in the identification medium of the present invention can present the same silver appearance even without relying on the cholesteric resin layer after a wide-band treatment. As a result, it can be obtained by an easy manufacturing method such as mixing sheets that can be manufactured more easily, and high design properties can be exerted.

[0100] It is preferred that any one of the sheets of the material having cholesteric regularity in the light reflecting layer satisfies the formula (c), and it is more preferred that all of them satisfy the formula (c).

[0101] 0.10≤Δλ / λc≤0.25 Formula (c)

[0102] The upper limit of the value of Δλ / λc is preferably 0.25 or less, and more preferably 0.15 or less. On the other hand, the lower limit thereof is preferably 0.10 or more, and more preferably 0.12 or more.

[0103] A sheet having a Δλ / λc value below the above upper limit can be easily obtained even without performing a broadband treatment on the cholesteric resin layer, and can be manufactured using a conventionally known polymerizable liquid crystal compound. By using a sheet having such a reflection band and satisfying the other conditions of the present invention, the obtained light reflection layer can satisfy formulas (b-1) and (b-2) (or formulas (b-1') and (b-2')) and exhibit the same silver appearance as the cholesteric resin layer after the broadband treatment. Therefore, in its manufacturing process, the burden of obtaining special materials and the burden of processes such as precise and multi-stage irradiation and heating of weak ultraviolet rays can be reduced, and it can be manufactured at low cost.

[0104] On the other hand, by setting the lower limit of the value of Δλ / λc to be equal to or greater than the above lower limit, selective reflection can be more effectively expressed.

[0105] Generally, in the case of a cholesteric resin layer manufactured by performing a broadband treatment, the pitch of the helical structure is not constant within the layer but has a gradient, and the helical structure having the pitch gradient shows a large Δλ / λc value or a wide Δλ to the extent that the value of Δλ / λc cannot be calculated. In contrast, in the case of a cholesteric resin layer manufactured without performing a broadband treatment, the pitch is constant within the layer in many cases, so the Δλ / λc value is a small value of 0.25 or less. In the case of such a small Δλ / λc value, the reflection band becomes narrow, so the color presented by the cholesteric resin layer is a single color.

[0106] The light reflecting layer can include a sheet having the following reflection band as a sheet other than the above three types, and the above reflection band includes a region with a wavelength greater than 660nm. Specifically, in addition to the sheets (i), (ii) and (iii), a sheet (IR) having a selective reflection center wavelength λc(IR) greater than 660nm can be included. By including such a sheet (IR), the blue shift when observed at an angle can be reduced. In addition, the recognition function using incident light in the infrared region can also be demonstrated.

[0107] Regarding the light reflecting layer, the average value of the integrated reflectivity at 430 to 660 nm is preferably 20% or more, more preferably 30% or more. On the other hand, the theoretical upper limit of the reflectivity is 50%. By having such a high reflectivity, the color brought about by the reflection appears clearly, and an appearance with high recognition function and excellent aesthetics can be obtained. In the present invention, by using the combination of the above-mentioned sheets as the material constituting the light reflecting layer, such a high reflectivity can be obtained even without performing a complex treatment such as a wide-band treatment. Figure 1 and Figure 2 In the case where a patterned phase difference layer 140 and a coating layer 150 are provided on the upper side of the light reflecting layer 120 as in the example shown, the light loss caused by passing through these layers is usually sufficiently small. In this case, the reflectivity of the light reflecting layer can be measured by measuring the reflectivity of the display surface in the identification medium. Alternatively, if the reflectivity of the display surface in the identification medium is 20% or more, it can be said that the reflectivity of the light reflecting layer is also 20% or more.

[0108] In addition to the sheet, the light reflecting layer may also include a material used to form an integral material and include the sheet. Specifically, it may include a medium used to manufacture a common ink. Furthermore, it may also include a diluent used to dilute the medium.

[0109] The method for forming the light reflecting layer is not particularly limited, and a known method can be used. For example, a sheet mixed ink containing the sheet and the medium and any other components is prepared, applied to a suitable substrate, and cured by drying, etc., thereby forming the light reflecting layer.

[0110] [Other structural elements]

[0111] The identification medium of the present invention may have any structural elements in addition to the above-mentioned light reflection layer and patterned phase difference layer. Figure 1 and Figure 2 As exemplified in the identification medium 100 shown in FIG. 1 , the identification medium can include a light absorbing layer, a coating layer, and an adhesive layer.

[0112] The light absorbing layer is a layer that absorbs incident light. The light absorbing layer can be a black layer. The material of the light absorbing layer can be any material, and can be, for example, a film colored in black. The light absorbing layer can be arranged on the back side of the light reflecting layer, that is, the position of the light reflecting layer on the opposite side to the viewing side. In the case where the light reflecting layer is a reflective circular polarizer, most of the incident light that is not reflected will be transmitted. When the light absorbing layer is arranged on the back side of the light reflecting layer, the transmitted light will be absorbed, as a result, the effect brought by the reflected light can be viewed more clearly. On the other hand, in the case where the light absorbing layer is not arranged on the back side of the light reflecting layer, the back side of the light reflecting layer can be viewed, so the effect brought by the reflected light will become unclear, but a design effect that allows the identification medium to be a transparent object can be obtained.

[0113] The coating layer can be arranged at a position closer to the viewing side than the patterned phase difference layer. The coating layer can be a transparent material such as a glass plate or a resin film. By providing the coating layer, the light reflecting layer and the patterned phase difference layer can be protected during use.

[0114] The adhesive layer is a layer for bonding the above-mentioned various layers together. As a material constituting the adhesive layer, a known adhesive having a transparency high enough not to significantly inhibit the transmission of light in the identification medium can be appropriately selected and used.

[0115] The identification medium may also have a mounting member. The mounting member refers to a member that performs a function when the identification medium is mounted on an article. A part or all of the mounting member may also serve as a decorative member. Examples of mounting members include members such as rings, buckles, hooks, threads, chains, belts, etc. extending from the periphery of the identification medium, and shells such as trays that also serve as decorative members. The mounting member may be directly attached to the light reflecting layer and / or the patterned phase difference layer, which are necessary structural elements of the identification medium, or may be combined via any member other than these. The combination with the mounting member may be any of adhesion by an adhesive, adhesion by welding, mechanical bonding such as screwing or ligation, etc. In addition, the mounting member may be the same layer as the above-mentioned adhesive layer, in which case the identification medium and the member of the installation object can be bonded via this layer.

[0116] [Example of the role of identification medium]

[0117] When the identification medium of the present invention is used, incident light is made incident on the display surface of the identification medium, reflected by the light reflecting layer to become reflected light, and the reflected light is observed.

[0118] Examples of light incident on the identification medium include non-polarized light, linearly polarized light, circularly polarized light, and elliptically polarized light. When the incident light is non-polarized light, the identification medium can be used by selectively observing the linear polarization component or circular polarization component of the reflected light in the observation of the reflected light. As the incident non-polarized light, ordinary ambient light such as sunlight and indoor lighting can be used.

[0119] Selectively observing the linear polarization component of the reflected light can be performed by visually observing the reflected light across the observation linear polarizer. Selectively observing the circular polarization component of the reflected light can be performed by visually observing the reflected light across the observation circular polarizer. In order to avoid obstruction of the incidence of ambient light, the observation linear polarizer and the observation circular polarizer can usually be used in a state separated from the identification medium. The lower limit of the separation distance can be appropriately adjusted according to the size of the identification medium and the observation linear polarizer, and can usually be more than 100mm. On the other hand, the upper limit of the separation distance can be appropriately adjusted within the range where the reflected light of the identification medium can be observed, and is usually less than 30m.

[0120] Like this, the linear polarizer for observation used at a position separated from the identification medium may be a special product for the method of use of the present invention, or may be a conventional linear polarizer for other purposes. For example, since most commercially available polarized sunglasses can function as linear polarizers, such commercially available polarized sunglasses may also be used as linear polarizers for observation. As examples of circular polarizers for observation, circular polarizers consisting of a combination of a linear polarizer and a phase difference film, and circular polarizers containing a layer of cholesteric material (such as those described in International Publication No. 2020 / 121791) can be cited.

[0121] refer to Figure 1 and Figure 2 In the following description, the following example is described: the light reflection layer 120 only includes sheets (i) and (ii) as sheets, sheet (i) is a left-handed reflective circular polarizer that reflects red light with a λc of 650nm as reflected light (i.e., a reflective circular polarizer that selectively reflects the left-handed circular polarization component in the incident light), sheet (ii) is a right-handed reflective circular polarizer that reflects blue light with a λc of 450nm as reflected light (i.e., a reflective circular polarizer that selectively reflects the right-handed circular polarization component in the incident light), the patterned phase difference layer 140 is a layer that functions as a λ / 4 wave plate as a whole, the incident light is non-polarized light, and the outgoing light is observed through the linear polarizer. This example is equivalent to Example 14 in the embodiments described later.

[0122] When the non-polarized light incident on the area 160B of the display surface 160 of the identification medium 100 passes through the transparent coating layer 150 and the adhesive layer 132 downward and reaches the light reflecting layer 120, the left-handed circularly polarized component in the reflection band of the sheet (i) and the right-handed circularly polarized component in the reflection band of the sheet (ii) are reflected and travel upward, and the other components pass through the reflection layer 120 downward and are absorbed by the light absorbing layer. The reflected light is emitted from the area 160B of the display surface 160 as a mixture of a red left-handed circularly polarized component and a blue right-handed circularly polarized component. When observed through a linear polarizer, the linear polarization component of a certain direction in each circularly polarized light is separated and observed. As a result, in this observation, an intermediate color, namely magenta, which is presented by the mixture of red and blue can be observed. Even if the azimuth angle of the identification medium 100 (the rotation angle when the identification medium is rotated with the direction perpendicular to the display surface as the axis) is changed, the amount of the linear polarization component will not change.

[0123] On the other hand, the non-polarized light incident on the area 160A of the display surface 160 of the identification medium 100 travels downward through the transparent coating layer 150 and the adhesive layer 132, and then reaches the patterned phase difference layer 140. When the light travels downward through the patterned phase difference layer 140, its linear polarization component is converted into a circular polarization component, and the circular polarization component is converted into a linear polarization component, but since the original incident light is non-polarized light, the result is that no change in the polarization state occurs. When the light further reaches the light reflection layer 120, the left-handed circular polarization component in the reflection band of the sheet (i) and the right-handed circular polarization component in the reflection band of the sheet (ii) are reflected and travel upward, and the other components travel downward through the reflection layer 120 and are absorbed by the light absorption layer. The reflected light travels upward through the patterned phase difference layer 140, where it is converted into linear polarization light, and is emitted from the area 160A of the display surface 160 as light having a hue corresponding to the reflection band and a mixture of linear polarization components with different polarization directions. That is, when circularly polarized light passes through the λ / 4 wave plate, it is converted into linearly polarized light, and its polarization direction is a direction that forms an angle of 45° relative to the slow axis of the λ / 4 wave plate. Since the angular direction of this angle is opposite when the transmitted light is left-handed circularly polarized light and when it is right-handed circularly polarized light, the polarization directions of these polarized lights are orthogonal. Therefore, the polarization direction of the red linear polarized light reflected from the plate (i) and the polarization direction of the blue linear polarized light reflected from the plate (ii) are mutually orthogonal. When observed across the linear polarizer, by making the azimuth angle of the identification medium 100 and the transmission axis direction of the linear polarizer change relatively, its hue changes between blue and red. That is, when the transmission axis direction of the linear polarizer is consistent with the polarization direction of the red linear polarized light, the red color becomes the strongest, and when the transmission axis direction of the linear polarizer is consistent with the polarization direction of the blue linear polarized light, the blue color becomes the strongest, and in the middle position, the intermediate color corresponding to the azimuth angle can be observed.

[0124] Therefore, by changing the relative angle between the identification medium 100 and the observation linear polarizer, it is possible to observe that the brightness and hue of the region 160B remain unchanged, while only the hue of the region 160A changes. In addition, when the amount of reflected light from the sheet (i) is greatly different from the amount of reflected light from the sheet (ii), the brightness of the region 160A can also be greatly changed by changing the angle relationship.

[0125] On the other hand, in the case of the identification medium 100 that is not observed through a linear polarizer in the state after the non-polarized light is incident, the observer observes a mixture of blue right-handed circularly polarized components and red left-handed circularly polarized components emitted from region 160B, and a mixture of blue linear polarized components and red linear polarized components with mutually orthogonal polarization directions emitted from region 160A. Since the loss of light when the light passes through the patterned phase difference layer 140 can be very small, the brightness of the light emitted from region 160A and the light emitted from region 160B are substantially the same. Since the difference in the polarization state of these lights cannot be recognized by human vision, the observer cannot recognize the difference between them. In addition, even if the relative angle relationship between the identification medium 100 and the observer changes, the observer cannot recognize the change based on the change in the polarization state.

[0126] In the method of use of this example, the identification medium of the present invention can bring about a special effect that the relative changes in color tone and brightness can be observed only when the linear polarizer is separated. Such a special effect cannot be obtained by a copy easily obtained by conventional printing and other technologies. Therefore, the identification medium of the present invention exerts a high recognition function and anti-counterfeiting function in such use.

[0127] By changing the relative brightness, characters, graphics, etc. can be displayed on the display surface. Such an image that cannot be observed in normal observation but can be observed only in a specific observation of the identification medium is called a "latent image" of the identification medium.

[0128] The above example is an example of a case where the patterned phase difference layer 140 is a λ / 4 wave plate. When the patterned phase difference layer 140 is a λ / 2 wave plate, the rotation direction of the circularly polarized light emitted from the region 160A is opposite to the rotation direction of the circularly polarized light emitted from the region 160B. Therefore, by using a right-handed circular polarizer and a left-handed circular polarizer in combination as observation polarizers, observation can be performed through them respectively and the observation results can be compared, thereby making it possible to utilize the identification function of the identification medium.

[0129] [Specific examples of cholesteric resin layer]

[0130] Hereinafter, a material having cholesteric regularity, which is a material of a sheet serving as a constituent element of the light reflecting layer, and a cholesteric resin layer as an example thereof will be described.

[0131] Cholesteric regularity refers to the following structure: on a certain plane inside the material, the molecular axes are arranged in a certain direction, the direction of the molecular axes in the next plane overlapping with it is slightly deflected at an angle, and the angle is further deflected in the next plane, and as the planes arranged in this way are successively passed through, the angle of the molecular axes in the plane gradually deflects (twists). That is, when the molecules inside a layer of a certain material have cholesteric regularity, the molecules are arranged in a certain direction of the molecular axes on a first plane inside the layer. In the next second plane inside the layer overlapping with the first plane, the direction of the molecular axes is slightly deflected at an angle compared to the direction of the molecular axes in the first plane. In the next third plane further overlapping with the second plane, the direction of the molecular axes is further deflected at an angle compared to the direction of the molecular axes in the second plane. In this way, in the planes arranged in an overlapping manner, the angles of the molecular axes in the plane are successively deflected (twisted). A structure in which the direction of the molecular axes is gradually twisted like this is usually a helical structure, which is optically a chiral structure.

[0132] The cholesteric resin layer refers to a layer obtained by curing a curable liquid crystal compound exhibiting a cholesteric liquid crystal phase. The cholesteric resin layer can be obtained, for example, by polymerizing a polymerizable liquid crystal compound in a state exhibiting a cholesteric liquid crystal phase. More specifically, the cholesteric resin layer can be obtained by applying a liquid crystal composition containing a polymerizable liquid crystal compound to an appropriate substrate, etc., making a layer, oriented in a cholesteric liquid crystal phase and curing.

[0133] As a polymerizable liquid crystal compound, a photopolymerizable liquid crystal compound is preferred. As a photopolymerizable liquid crystal compound, a photopolymerizable liquid crystal compound that can be polymerized by irradiating active energy rays can be used. As active energy rays, energy rays that can cause the polymerization reaction of the photopolymerizable liquid crystal compound can be used from a wide range of energy rays such as visible light, ultraviolet rays and infrared rays, and ionizing radiation such as ultraviolet rays is particularly preferred. As a photopolymerizable liquid crystal compound preferably used in a cholesteric liquid crystal composition, a rod-shaped liquid crystal compound having two or more reactive groups in one molecule is particularly preferred, and a compound represented by formula (1) is particularly preferred.

[0134] R 3 -C 3 -D 3 -C 5 -MC 6 -D 4 -C 4 -R 4 Formula (1)

[0135] In formula (1), R 3 and R 4are reactive groups, each independently selected from (meth)acryloyl, (thio)epoxy, oxetanyl, thietanyl, aziridine, pyrrolyl, vinyl, allyl, fumarate, cinnamoyl, The group selected from the group consisting of oxazoline group, mercapto group, iso(thio)cyanate group, amino group, hydroxyl group, carboxyl group and alkoxysilyl group. By having these reactive groups, a liquid crystal composition cured layer having high mechanical strength can be obtained when the liquid crystal composition is cured.

[0136] In formula (1), D 3 and D 4 Each independently represents a group selected from the group consisting of a single bond, a linear or branched alkyl group having 1 to 20 carbon atoms, and a linear or branched alkylene oxide group having 1 to 20 carbon atoms.

[0137] In formula (1), C 3 ~C 6 Each independently represents a group selected from a single bond, -O-, -S-, -SS-, -CO-, -CS-, -OCO-, -CH2-, -OCH2-, -CH=NN=CH-, -NHCO-, -O-(C=O)-O-, -CH2-(C=O)-O-, and -CH2O-(C=O)-.

[0138] In formula (1), M represents a mesogenic group. Specifically, M represents an unsubstituted or substituted azomethine, azoxy, phenyl, biphenyl, terphenyl, naphthalene, anthracene, benzoate, cyclohexanecarboxylic acid phenyl ester, cyanophenylcyclohexane, cyano substituted phenyl pyrimidine, alkoxy substituted phenyl pyrimidine, phenyl diphenyl ester ... A group in which two to four identical or different skeletons in alkanes, diphenylacetylenes, and alkenylcyclohexylbenzonitriles are bonded by bonding groups such as -O-, -S-, -SS-, -CO-, -CS-, -OCO-, -CH2-, -OCH2-, -CH=NN=CH-, -NHCO-, -O-(C=O)-O-, -CH2-(C=O)-O-, and -CH2O-(C=O)-.

[0139] Examples of the substituent that the mesogenic group M may have include a halogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, a cyano group, a nitro group, an -OR 5 、-OC(=O)-R 5 、-C(=O)-OR 5 、-OC(=O)-OR 5 、-NR 5 -C(=O)-R 5、-C(=O)-NR 5 R 7 , or -OC(=O)-NR 5 R 7 Here, R 5 and R 7 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms. 5 and R 7 In the case of an alkyl group, -O-, -S-, -OC(=O)-, -C(=O)-O-, -OC(=O)-O-, -NR 6 -C(=O)-, -C(=O)-NR 6 -、-NR 6 -, or -C(=O)- (excluding the case where two or more -O- are inserted adjacently and two or more -S- are inserted adjacently). 6 It represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

[0140] Examples of the substituent in the above-mentioned “alkyl group having 1 to 10 carbon atoms which may have a substituent” include a halogen atom, a hydroxyl group, a carboxyl group, a cyano group, an amino group, an alkoxy group having 1 to 6 carbon atoms, an alkoxyalkoxy group having 2 to 8 carbon atoms, an alkoxyalkoxyalkoxy group having 3 to 15 carbon atoms, an alkoxycarbonyl group having 2 to 7 carbon atoms, an alkylcarbonyloxy group having 2 to 7 carbon atoms, and an alkoxycarbonyloxy group having 2 to 7 carbon atoms.

[0141] In addition, the above-mentioned rod-shaped liquid crystal compound is preferably an asymmetric structure. Here, the asymmetric structure means that in formula (1), the mesogenic group M is the center, and R 3 -C 3 -D 3 -C 5 -M- vs. -MC 6 -D 4 -C 4 -R 4 Different structures: By using a rod-like liquid crystal compound having an asymmetric structure as the rod-like liquid crystal compound, the alignment uniformity can be further improved.

[0142] Preferred specific examples of the rod-like liquid crystal compound include the following compounds (B1) to (B14). However, the rod-like liquid crystal compound is not limited to the following compounds.

[0143] [Chemical formula 1]

[0144]

[0145] [Chemical formula 2]

[0146]

[0147] [Chemical formula 3]

[0148]

[0149] When the liquid crystal composition contains the rod-like liquid crystal compound, the liquid crystal composition preferably contains a compound represented by formula (2) as an alignment aid in combination with the rod-like liquid crystal compound.

[0150] R 1 -A 1 -BA 2 -R 2 (2)

[0151] In formula (2), R 1 and R 2 Each is independently a group selected from a linear or branched alkyl group having 1 to 20 carbon atoms, a linear or branched alkylene oxide group having 1 to 20 carbon atoms, a hydrogen atom, a halogen atom, a hydroxyl group, a carboxyl group, a (meth)acryloyl group into which any bonding group may be inserted, an epoxy group, a mercapto group, an isocyanate group, an amino group, and a cyano group.

[0152] The above-mentioned alkyl and epoxyalkyl groups may be unsubstituted or may be substituted with one or more halogen atoms. Furthermore, the above-mentioned halogen atoms, hydroxyl groups, carboxyl groups, (meth)acryloyl groups, epoxy groups, mercapto groups, isocyanate groups, amino groups and cyano groups may be bonded to alkyl and epoxyalkyl groups having 1 to 2 carbon atoms.

[0153] As R 1 and R 2 Preferred examples include a halogen atom, a hydroxyl group, a carboxyl group, a (meth)acryloyl group, an epoxy group, a mercapto group, an isocyanate group, an amino group, and a cyano group.

[0154] In addition, R 1 and R 2 At least one of them is a reactive group. 1 and R 2 At least one of the above-mentioned compounds represented by formula (2) is fixed in the liquid crystal composition cured layer during curing, and a more solid layer can be formed. Here, the reactive group can include, for example, a carboxyl group, a (meth)acryloyl group, an epoxy group, a mercapto group, an isocyanate group, and an amino group.

[0155] In formula (2), A 1 and A 2Each independently represents a group selected from 1,4-phenylene, 1,4-cyclohexylene, cyclohexene-1,4-ene, 4,4'-biphenylene, 4,4'-bicyclohexylene, and 2,6-naphthylene. The above-mentioned 1,4-phenylene, 1,4-cyclohexylene, cyclohexene-1,4-ene, 4,4'-biphenylene, 4,4'-bicyclohexylene, and 2,6-naphthylene may be unsubstituted, or may be substituted with one or more halogen atoms, hydroxyl groups, carboxyl groups, cyano groups, amino groups, alkyl groups having 1 to 10 carbon atoms, halogenated alkyl groups, etc. In A 1 and A 2 When there are two or more substituents in each of the groups, they may be the same or different.

[0156] As A 1 and A 2 Particularly preferred groups include groups selected from 1,4-phenylene, 4,4'-biphenylene, and 2,6-naphthylene. These aromatic ring skeletons are relatively rigid compared to alicyclic skeletons, have a high affinity with the mesogen of the rod-like liquid crystal compound, and further improve the alignment uniformity.

[0157] In formula (2), B is selected from a single bond, -O-, -S-, -SS-, -CO-, -CS-, -OCO-, -CH2-, -OCH2-, -CH=NN=CH-, -NHCO-, -O-(C=O)-O-, -CH2-(C=O)-O-, and -CH2O-(C=O)-.

[0158] Particularly preferred groups for B include a single bond, -O-(C=O)-, and -CH=NN=CH-.

[0159] Particularly preferred specific examples of the compound represented by formula (2) include the following compounds (A1) to (A10). These may be used alone or in combination of two or more at any ratio.

[0160] [Chemical formula 4]

[0161]

[0162] In the above compound (A3), "*" represents a chiral center.

[0163] The weight ratio represented by (total weight of the compounds represented by formula (2)) / (total weight of rod-like liquid crystal compounds) is preferably 0.001 or more, more preferably 0.01 or more, further preferably 0.05 or more, preferably 1 or less, and more preferably 0.65 or less. By making the above-mentioned weight ratio above the above-mentioned lower limit, the orientation uniformity can be improved in the layer of the liquid crystal composition. In addition, by making the above-mentioned weight ratio below the upper limit, the orientation uniformity can be improved. In addition, the stability of the liquid crystal phase of the liquid crystal composition can be improved. Furthermore, since the refractive index anisotropy Δn of the liquid crystal composition can be improved, a liquid crystal composition cured layer having desired optical properties such as selective reflection performance of circularly polarized light can be stably obtained. Here, with respect to the total weight of the compounds represented by formula (2), when only one compound represented by formula (2) is used, the weight of the compound is represented, and when two or more are used, the total weight is represented. Similarly, with respect to the total weight of the rod-like liquid crystal compounds, when only one rod-like liquid crystal compound is used, the weight of the compound is represented, and when two or more are used, the total weight is represented.

[0164] Furthermore, when the compound represented by formula (2) and a rod-shaped liquid crystal compound are used in combination, the molecular weight of the compound represented by formula (2) is preferably less than 600, and the molecular weight of the rod-shaped liquid crystal compound is preferably greater than 600. Thus, since the compound represented by formula (2) can enter the gap between the rod-shaped liquid crystal compound having a larger molecular weight than the compound represented by formula (2), the alignment uniformity can be improved.

[0165] The liquid crystal composition for forming a cholesteric resin layer can also include any component constituting the cholesteric resin layer and a solvent for facilitating the processing of the liquid crystal composition. As examples of any component, a chiral agent, a polymerization initiator, and a surfactant can be cited. As specific examples of any component and solvent, and a liquid crystal composition, those described in Japanese Patent Publication No. 2019-188740 can be cited.

[0166] In the present invention, it is preferred that all sheets constituting the light reflecting layer are solidified products of liquid crystal compositions, and the liquid crystal compositions contain common polymerizable liquid crystal compounds. Specifically, for all cholesteric resin layers used to obtain various sheets, the liquid crystal composition preferably used to manufacture the cholesteric resin layer contains any one of the above-mentioned rod-shaped liquid crystal compounds as a polymerizable liquid crystal compound. In addition, it is more preferred that the liquid crystal compositions of all sheets have the same composition except for the proportion of the chiral agent, and the reflection band is adjusted according to the proportion of the chiral agent. By using a sheet with a common composition like this, a good color can be obtained. In addition, since the deterioration over time during the use of the identification medium can be made more uniform, the reduction in aesthetics and the reduction in identification function that are accompanied by degradation over time can be suppressed.

[0167] The method for forming a cholesteric resin layer using a liquid crystal composition is not particularly limited and can be performed by a known method. Specifically, the cholesteric resin layer can be formed by coating the liquid crystal composition on the surface of a support film having an orientation-limiting force, performing an orientation treatment as required, and then curing the polymerizable material constituting the liquid crystal composition by an appropriate method such as ultraviolet irradiation.

[0168] [Specific example of patterned phase difference layer]

[0169] The patterned phase difference layer is a layer including a region having a phase difference. The region having a phase difference occupies a part of the display surface of the identification medium.

[0170] Examples of the retardation layer (the portion of the patterned retardation layer having a retardation region) include the region functioning as a λ / 4 wave plate and the region functioning as a λ / 2 wave plate exemplified above.

[0171] As the material constituting the phase difference layer, various solid materials with optical anisotropy can be cited. As an example thereof, a stretched film obtained by stretching a transparent material can be cited. More specifically, a film in which an optically isotropic film is stretched and given an in-plane delay Re that can function as a λ / 4 wave plate or a λ / 2 wave plate can be cited. From the viewpoint of being able to obtain relatively cheaply and easily giving a desired value of Re and being easily formed into a desired arbitrary shape, a stretched film is preferred.

[0172] As another example of a material constituting a phase difference layer, a solidified material of a liquid crystal compound can be cited. Specifically, it is a layer obtained by curing a solidified liquid crystal compound oriented in the following liquid crystal state, and the above-mentioned liquid crystal state is a liquid crystal state that exhibits a phase difference that can function as a λ / 4 wave plate or a λ / 2 wave plate. As examples of such layers and methods for manufacturing them, those described in International Publication No. 2019 / 116995 can be cited. Since the solidified material of the liquid crystal compound can easily form a film having a different phase difference between a certain part and another certain part, it is particularly preferred when it is required to form a film as a patterned phase difference layer.

[0173] [thing]

[0174] The article of the present invention has the above-mentioned identification medium of the present invention.

[0175] Examples of articles include clothing, shoes, hats, clothing items, jewelry, daily necessities, and other articles. The article of the present invention can have an identification function by having an identification medium. By having this identification function, it is possible to identify that the identification medium and the article are not counterfeits but genuine products. In addition, the identification medium can give a design effect to the article. The identification medium can be set on the article as a decoration, component, or accessory of an article such as a label, a small pendant, a badge, a sticker, etc.

[0176] In addition to the identification medium of the present invention, the article of the present invention can also have a polarizer observer. As the polarizer observer, there can be cited a device having an observation polarizer such as the above-mentioned observation linear polarizer or observation circular polarizer and being equipped on the article in a manner that the identification medium can be observed across the observation polarizer. The polarizer observer can be made into a shape such as a label and be equipped on the article body through a belt or the like. In this way, by having a polarizer observer in addition to the identification medium, a common article user can easily identify the identification medium.

[0177] Example

[0178] The present invention will be described in detail below with reference to the following examples. However, the present invention is not limited to the following examples, and can be arbitrarily modified and implemented without departing from the scope of the claims of the present invention and the scope of its equivalents.

[0179] In the following description, "%" and "parts" indicating amounts are based on weight unless otherwise specified. In addition, the following operations are performed in an atmosphere of normal temperature and pressure unless otherwise specified.

[0180] In the following description, as a commercially available adhesive, unless otherwise specified, a transparent tape "LUCIACS CS9621T" manufactured by Nitto Denko Corporation (thickness 25 μm, visible light transmittance 90% or more, in-plane retardation 3 nm or less) was used.

[0181] In the following description, the term "CLC" may be used as an abbreviation to indicate a cholesteric resin layer or a sheet obtained by pulverizing the cholesteric resin layer.

[0182] [Method for measuring reflectivity of CLC layer]

[0183] The support film was peeled off from the multilayer member to obtain a CLC layer. The reflectance of the CLC layer when non-polarized light (wavelength 300 nm to 950 nm) was measured using an ultraviolet visible spectrophotometer with an integrating sphere ("UV-Vis 770" manufactured by JASCO Corporation).

[0184] [Method for measuring the rotation direction of circularly polarized light reflected by the CLC layer]

[0185] The CLC layer is irradiated with non-polarized light, and the reflected light is observed through a right-handed circular polarizing plate and a left-handed circular polarizing plate to determine whether the rotation direction of the circularly polarized light as the reflected light is right-handed or left-handed.

[0186] [Measurement method of in-plane retardation and slow axis direction]

[0187] The in-plane retardation and the slow axis direction were measured at a measurement wavelength of 550 nm using a phase difference meter (“Axoscan” manufactured by Axometrics).

[0188] [Measurement of average particle size of tablets]

[0189] The particle size distribution of the sheet was measured by a laser scattering method, and the average particle size was measured from the particle size distribution. As a measuring instrument, a laser diffraction / scattering type particle size distribution measuring device (manufactured by Horiba, Ltd., LA-960) was used.

[0190] [Manufacturing Example 1. Manufacture of a broadband right-handed circularly polarized red-reflecting CLC layer]

[0191] (P1-1. Liquid crystal composition)

[0192] A liquid crystal composition was prepared by mixing 100 parts of a photopolymerizable liquid crystal compound represented by the following formula (X1), 25 parts of a photopolymerizable non-liquid crystal compound represented by the following formula (X2), 7 parts of a chiral agent (“LC756” manufactured by BASF), 5 parts of a photopolymerization initiator (“Irgacure 907” manufactured by Ciba Japan Co., Ltd.), 0.15 parts of a surfactant (“S-420” manufactured by AGC Seimi Chemical Co., Ltd.) and 320 parts of cyclopentanone as a solvent.

[0193] [Chemical formula 5]

[0194]

[0195] (P1-2. Multilayer structure including CLC layer)

[0196] A long polyethylene terephthalate film ("A4100" manufactured by Toyobo Co., Ltd.; thickness 100 μm) was prepared as a support film. The support film was attached to the delivery section of a film conveying device, and the following operation was performed while conveying the support film in the longitudinal direction.

[0197] The surface of the support film was subjected to a rubbing treatment along the longitudinal direction parallel to the conveying direction. Next, the liquid crystal composition obtained in (P1-1) was coated on the surface of the support film subjected to the rubbing treatment using a die coater to form a layer of the liquid crystal composition. The layer of the liquid crystal composition was subjected to an orientation treatment by heating at 120°C for 5 minutes to orient the liquid crystal composition to exhibit a cholesteric liquid crystal phase. Thereafter, the layer of the liquid crystal composition was irradiated with 830 mJ / cm 2 The layer of the liquid crystal composition was cured by ultraviolet rays. Thus, a multilayer structure (CLC_RaR) having a support film and a red reflective CLC layer (thickness 3 μm) having a circularly polarized light separation function was obtained.

[0198] The reflectivity of the CLC layer of the multilayer component (CLC_RaR) was measured by the above-mentioned measuring method. The results of the measurement showed that the reflectivity of the CLC layer at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.15. In addition, the rotation direction of the circularly polarized light reflected from the CLC layer was measured by the above-mentioned measuring method, and the result was right-handed. The CLC layer was visually observed under natural light and the result was red.

[0199] [Manufacturing Example 2. Manufacture of a Broadband Left-Handed Circularly Polarized Red-Reflecting CLC Layer]

[0200] As a chiral agent, 7.1 parts of the compound represented by the following formula (X3) (D-mannitol, 1,4:3,6-dihydro-, 2,5-bis[4-[[[6-[[[4-[(1-oxo-2-propen-1-yl)oxy]butoxy]carbonyl]oxy]-2-naphthyl]carbonyl]oxy]benzoate]) was used instead of "LC756" manufactured by BASF, and a multilayer component (CLC_RaL) having a support film and a CLC layer (thickness 3 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 1. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. As a result of the measurement, the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.15. In addition, the rotation direction of the circularly polarized light reflected by the CLC layer was measured by the above-mentioned measurement method, and the result was left-handed. The CLC layer was visually observed under natural light and was found to be red.

[0201] [Chemical formula 6]

[0202]

[0203] [Manufacturing Example 3. Manufacture of a broadband right-handed circularly polarized green reflecting CLC layer]

[0204] A multilayer component (CLC_GaR) having a supporting film and a CLC layer (thickness 3 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 1 except that the amount of the chiral agent ("LC756" manufactured by BASF) was changed to 8.1 parts. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement result showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.15. In addition, the rotation direction of the circularly polarized light reflected in the CLC layer was measured by the above-mentioned measurement method, and the result was right-handed. The CLC layer was visually observed under natural light, and the result was green.

[0205] [Manufacturing Example 4. Manufacture of a Broadband Left-Handed Circularly Polarized Green-Reflecting CLC Layer]

[0206] The amount of the chiral agent (X3) was changed to 8.4 parts. In addition, a multilayer component (CLC_GaL) having a supporting film and a CLC layer (thickness 3 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 2. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement result showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.15. In addition, the rotation direction of the circularly polarized light reflected in the CLC layer was measured by the above-mentioned measurement method, and the result was left-handed. The CLC layer was visually observed under natural light, and the result was green.

[0207] [Manufacturing Example 5. Manufacture of a broadband right-handed circularly polarized blue reflecting CLC layer]

[0208] The amount of chiral agent ("LC756" manufactured by BASF) was changed to 9.8 parts. In addition, a multilayer component (CLC_BaR) having a supporting film and a CLC layer (thickness 3 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 1. The coating thickness of the liquid crystal composition was set to a CLC layer thickness of 7 μm, but since poor orientation and turbidity frequently occurred in this case, the example in which the CLC layer thickness was set to 3 μm was adopted as this manufacturing example. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement result showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.15. In addition, the rotation direction of the circularly polarized light reflected in the CLC layer was measured by the above-mentioned measurement method, and the result was right-handed. The CLC layer was visually observed under natural light, and the result was blue.

[0209] [Manufacturing Example 6. Manufacture of a broadband right-handed circularly polarized infrared reflecting CLC layer]

[0210] A multilayer component (CLC_IRaR) having a supporting film and a CLC layer (thickness 3 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 1 except that the amount of the chiral agent ("LC756" manufactured by BASF) was changed to 4 parts. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement results showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.15. The CLC layer was visually observed under natural light and was colorless and transparent.

[0211] [Manufacturing Example 7. Manufacture of Mid-Band Left-Handed Circularly Polarized Light Red Reflecting CLC Layer]

[0212] A multilayer component (CLC_RbL) having a supporting film and a CLC layer (3 μm thick) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 1, except that 100 parts of a photopolymerizable liquid crystal compound represented by the following formula (X4) was used instead of 100 parts of a liquid crystal compound represented by formula (X1), and 6.8 parts of a compound represented by formula (X3) was used instead of "LC756" manufactured by BASF as a chiral agent. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement results showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.12. In addition, the rotation direction of the circularly polarized light reflected in the CLC layer was measured by the above-mentioned measurement method, and the result was left-handed. The CLC layer was visually observed under natural light, and the result was red.

[0213] [Chemical formula 7]

[0214]

[0215] [Manufacturing Example 8. Manufacture of a mid-wavelength right-handed circularly polarized light green reflecting CLC layer]

[0216] 8.2 parts of "LC756" manufactured by BASF was used as a chiral agent instead of the compound represented by formula (X3). In addition, a multilayer component (CLC_GbR) having a supporting film and a CLC layer (thickness 3 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 7. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement result showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.12. In addition, the rotation direction of the circularly polarized light reflected in the CLC layer was measured by the above-mentioned measurement method, and the result was right-handed. The CLC layer was visually observed under natural light, and the result was green.

[0217] [Manufacturing Example 9. Manufacture of a Mid-Band Left-Handed Circularly Polarized Light Green Reflecting CLC Layer]

[0218] The amount of the chiral agent (X3) was changed to 8.5 parts. In addition, a multilayer component (CLC_GbL) having a supporting film and a CLC layer (thickness 3 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 7. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement result showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.12. In addition, the rotation direction of the circularly polarized light reflected in the CLC layer was measured by the above-mentioned measurement method, and the result was left-handed. The CLC layer was visually observed under natural light, and the result was green.

[0219] [Manufacturing Example 10. Manufacture of a mid-wavelength right-handed circularly polarized blue reflecting CLC layer]

[0220] A multilayer component (CLC_BbR) having a supporting film and a CLC layer (thickness 3 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 8 except that the amount of the chiral agent ("LC756" manufactured by BASF) was changed to 10.2 parts. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement result showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.12. In addition, the rotation direction of the circularly polarized light reflected in the CLC layer was measured by the above-mentioned measurement method, and the result was right-handed. The CLC layer was visually observed under natural light, and the result was blue.

[0221] [Manufacturing Example 11. Manufacture of a narrow-band right-handed circularly polarized light red-reflecting CLC layer]

[0222] (P11-1. Liquid crystal composition)

[0223] A liquid crystal composition is prepared by mixing 100 parts of a photopolymerizable liquid crystal compound represented by the following formula (X5), 5.7 parts of a chiral agent ("LC756" manufactured by BASF), 5 parts of a photopolymerization initiator ("Irgacure907" manufactured by Ciba Japan Co., Ltd.), 0.15 parts of a surfactant ("S-420" manufactured by AGC Seimi Chemical Co., Ltd.) and 320 parts of cyclopentanone as a solvent.

[0224] (P11-2. Multilayer structure including CLC layer)

[0225] As a liquid crystal composition, the liquid crystal composition obtained in (P11-1) was used instead of the liquid crystal composition prepared in (P1-1) of Manufacturing Example 1, and the coating thickness of the liquid crystal composition was changed. In addition, a multilayer component (CLC_RcR) having a support film and a CLC layer (thickness 5μm) having a circularly polarized light separation function was manufactured by the same method as Manufacturing Example 1. A manufacturing method in which the coating thickness of the liquid crystal composition was not changed compared to Manufacturing Example 1 and the thickness of the CLC layer was set to 3μm was also carried out. However, in this case, the reflectivity was as low as 35%, and sufficient optical properties could not be obtained. Therefore, the example in which the thickness of the CLC layer was set to 5μm was adopted as this manufacturing example. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement results showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.09. In addition, the rotation direction of the circularly polarized light reflected on the CLC layer was measured by the above-mentioned measurement method, and the result was right-handed. The CLC layer was visually observed under natural light and was found to be red.

[0226] [Chemical formula 8]

[0227]

[0228] [Manufacturing Example 12. Manufacture of a narrow-band left-handed circularly polarized light red-reflecting CLC layer]

[0229] A multilayer component (CLC_RcL) having a supporting film and a CLC layer (thickness 5 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 11, except that 5.8 parts of the compound represented by formula (X3) were used instead of "LC756" manufactured by BASF as a chiral agent. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement results showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.09. In addition, the rotation direction of the circularly polarized light reflected in the CLC layer was measured by the above-mentioned measurement method, and the result was left-handed. The CLC layer was visually observed under natural light and the result was red.

[0230] [Manufacturing Example 13. Manufacture of a narrow-band right-handed circularly polarized green-reflecting CLC layer]

[0231] A multilayer component (CLC_GcR) having a supporting film and a CLC layer (thickness 5 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 11 except that the amount of the chiral agent ("LC756" manufactured by BASF) was changed to 6.9 parts. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement results showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.09. In addition, the rotation direction of the circularly polarized light reflected in the CLC layer was measured by the above-mentioned measurement method, and the result was right-handed. The CLC layer was visually observed under natural light, and the result was green.

[0232] [Manufacturing Example 14. Manufacture of a narrow-band left-handed circularly polarized green-reflecting CLC layer]

[0233] A multilayer component (CLC_GcL) having a supporting film and a CLC layer (thickness 5 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 12 except that the amount of the chiral agent (X3) was changed to 7.2 parts. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement result showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.09. In addition, the rotation direction of the circularly polarized light reflected in the CLC layer was measured by the above-mentioned measurement method, and the result was left-handed. The CLC layer was visually observed under natural light, and the result was green.

[0234] [Manufacturing Example 15. Manufacture of a narrow-band right-handed circularly polarized blue-green reflecting CLC layer]

[0235] A multilayer component (CLC_XcR) having a supporting film and a CLC layer (thickness 5 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 11 except that the amount of the chiral agent ("LC756" manufactured by BASF) was changed to 7.5 parts. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement result showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.09. In addition, the rotation direction of the circularly polarized light reflected in the CLC layer was measured by the above-mentioned measurement method, and the result was right-handed. The CLC layer was visually observed under natural light, and the result was blue-green.

[0236] [Manufacturing Example 16. Manufacture of a narrow-band right-handed circularly polarized blue-reflecting CLC layer]

[0237] A multilayer component (CLC_BcR) having a supporting film and a CLC layer (thickness 5 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 11 except that the amount of the chiral agent ("LC756" manufactured by BASF) was changed to 8.1 parts. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement result showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.09. In addition, the rotation direction of the circularly polarized light reflected in the CLC layer was measured by the above-mentioned measurement method, and the result was right-handed. The CLC layer was visually observed under natural light, and the result was blue.

[0238] [Manufacturing Example 17. Manufacture of a Broadband Silver Reflective CLC Layer]

[0239] (P17-1. Liquid crystal composition)

[0240] A liquid crystal composition was prepared by the same method as in (P1-1) of Production Example 1, except that the amount of the chiral agent ("LC756" manufactured by BASF) was changed to 8.2 parts.

[0241] (P17-2. Multilayer structure including CLC layer)

[0242] A long polyethylene terephthalate film ("A4100" manufactured by Toyobo Co., Ltd.; thickness 100 μm) was prepared as a support film. The support film was attached to the delivery section of a film conveying device, and the following operation was performed while conveying the support film in the longitudinal direction.

[0243] The surface of the support film is subjected to a friction treatment along the length direction parallel to the conveying direction. Next, the liquid crystal composition obtained in (P17-1) is coated on the surface of the support film subjected to the friction treatment using a die coater to form a layer of the liquid crystal composition. The layer of the liquid crystal composition is subjected to an orientation treatment by heating at 120°C for 5 minutes to orient the liquid crystal composition to exhibit a cholesteric liquid crystal phase. Then, the layer of the liquid crystal composition is subjected to a broadband treatment. In the broadband treatment, 5 mJ / cm 2 ~30mJ / cm 2 The weak ultraviolet irradiation and the heating treatment at 100°C to 120°C were controlled so that the wavelength range capable of exerting the circularly polarized light separation function had a desired wavelength width. Then, the layer of the liquid crystal composition was irradiated with 800 mJ / cm 2 The layer of the liquid crystal composition was cured by ultraviolet light. Thus, a multilayer structure (CLC_S) having a support film and a broadband silver reflective CLC layer (thickness 5 μm) having a circularly polarized light separation function was obtained.

[0244] The reflectivity of the CLC layer of the multilayer component (CLC_S) was measured by the above-mentioned measurement method. The result of the measurement was that the CLC layer showed a roughly uniform reflection in the entire visible light region (450nm to 650nm), so it was impossible to find the half-peak width Δλ of the reflection band and the selective reflection center wavelength λc, and it was impossible to calculate the ratio Δλ / λc. In addition, the rotation direction of the circularly polarized light reflected in the CLC layer was measured by the above-mentioned measurement method, and the result was right-handed. The CLC layer was visually observed under natural light and the result was silver.

[0245] [Manufacturing Example 18. Manufacture of CLC Sheet_RaR]

[0246] The support film was peeled off from the multilayer member (CLC_RaR) obtained in Production Example 1, and the obtained CLC layer was pulverized to obtain a CLC layer flake. The obtained flake was classified with a sieve to obtain a CLC flake_RaR having an average particle size of 25 μm.

[0247] [Manufacturing Examples 19 to 23 and 29 to 39. Manufacture of CLC Sheet]

[0248] Various sheets shown in Table 1 were obtained by the same method as in Production Example 18, except that the members shown in Table 1 were used among the multilayer members obtained in Production Examples 1 to 17.

[0249] [Manufacturing Examples 24 to 28. Manufacture of CLC Sheet]

[0250] Various flakes having an average particle size of 75 μm shown in Table 1 were obtained by the same method as in Production Example 18, except that the multilayered members shown in Table 1 were used in Production Examples 1 to 17 and the sieve used for classification was changed.

[0251] [Table 1]

[0252] Table 1

[0253]

[0254] Reflected light rotation direction: The rotation direction of the reflected light when natural light is incident on the CLC layer. R: right-handed circularly polarized light, L: left-handed circularly polarized light.

[0255] [Production Example 40. λ / 4 stretched resin film]

[0256] A resin film formed of a thermoplastic norbornene resin ("ZEONOR film" manufactured by Zeon Co., Ltd. of Japan; a film manufactured by extrusion molding. Unstretched product) was prepared. The resin film was stretched in one direction at a stretching temperature of 130°C to obtain a phase difference film (R1) having an in-plane retardation capable of functioning as a 1 / 4 wave plate. The phase difference film (R1) had a thickness of 48 μm and an in-plane retardation of 144 nm. The resin film was punched out with a craft punch to obtain a star-shaped λ / 4 stretched resin film used as a phase difference layer.

[0257] [Production Example 41: λ / 2 stretched resin film]

[0258] Two λ / 4 stretched resin films obtained in Manufacturing Example 41 were bonded together via an adhesive ("CS9621T" manufactured by Nitto Denko Corporation). When bonding, the two resin films were aligned so that their slow axes were in the same direction. The multilayer resin film was punched out with a punch to obtain a λ / 2 stretched resin film having a star shape used as a phase difference layer.

[0259] [Example 1]

[0260] (1-1. Tablet mixture)

[0261] The CLC sheet_RaL, CLC sheet_GaL, and CLC sheet_BaR obtained in the above-mentioned manufacturing example were mixed in the weight ratio shown in Table 2 to obtain a CLC sheet mixture.

[0262] (1-2. Production of Light Reflecting Layer)

[0263] 10 parts of the CLC flake mixture obtained in (1-1), 85 parts of screen printing ink ("No. 2500 Medium" manufactured by Jujo Chemical Industry Co., Ltd.), and 5 parts of a special diluent for the screen printing ink (TETRON standard solvent) were mixed to obtain a CLC flake mixed ink. The obtained ink was applied to a light absorbing layer (manufactured by Toyobo Co., Ltd., black PET film, thickness 100 μm) using a notch wheel coater and dried to form a light reflecting layer 1 with a thickness of 40 μm.

[0264] (1-3. Reflection spectrum measurement of light reflecting layer)

[0265] The reflectance spectrum of the light reflecting layer 1 obtained in (1-2) was measured by an ultraviolet visible spectrophotometer ("UV-Vis 770" manufactured by JASCO Corporation) using an integrating sphere. Based on the obtained results, the average values ​​of the integrated reflectances of the blue region (B), green region (G), and red region (R) in the visible light region, namely B (430-490) Ave, G (500-600) Ave, and R (600-660) Ave, were obtained, and their ratios R / G and B / G were calculated. The results are shown in Table 2.

[0266] (1-4. Visual observation of light reflecting layer)

[0267] The light reflecting layer 1 obtained in (1-2) was visually observed to evaluate the color, the degree of glare, and the presence or absence of color change when the observation angle was changed from the front to an oblique angle.

[0268] (1-5. Color measurement of light reflecting layer)

[0269] The light reflecting layer 1 obtained in (1-2) was measured for color indices, namely, a* value and b* value, under D65 light source according to the method of JIS Z 8781-4.

[0270] (1-6. Production of Identification Medium (1))

[0271] The star-shaped λ / 4 stretched resin film obtained in Production Example 40 was bonded via an adhesive to cover a part of the surface of the light reflecting layer 1 obtained in (1-2) as a patterned phase difference layer. Furthermore, a glass plate with a thickness of 0.4 mm was bonded as a coating layer via an adhesive to cover the surface of the light reflecting layer 1 and the surface of the star-shaped λ / 4 stretched resin film. Figure 1 and Figure 2 The schematic structure of the identification medium (1) is shown in FIG. Figure 1 and Figure 2 As shown, the identification medium (1) 100 has a light absorption layer 110, a light reflection layer 120, a patterned phase difference layer 140, and a coating layer 150 in sequence, and also has a structure with adhesive layers 131 and 132 between the layers. The display surface 160 is provided with an area 160A covered by the patterned phase difference layer 140 and an area 160B not covered by the patterned phase difference layer 140.

[0272] (1-7. Observation of identification medium (1))

[0273] The identification medium (1) is kept in a horizontal position, and the azimuth angle of the identification medium (1) is rotated 360 degrees, and the observer observes the identification medium (1) from a vertical direction. The observation is performed with the naked eye and through a linear polarizer of polarized sunglasses. The observation is performed in a bright room with a fluorescent lamp as the light source.

[0274] In the naked eye observation, a colorless silver pearlescent appearance generated by the reflection of the light reflecting layer 120 is observed in the display surface 160. The patterned phase difference layer 140 is observed as a transparent member, and its star shape is almost invisible. No difference in brightness and color is observed between the area 160A and the area 160B in the display surface 160, and it does not change due to rotation.

[0275] When observing through polarized sunglasses, the star-shaped shape of region 160A is observed. The difference in brightness between region 160A and region 160B changes with rotation. In addition, the color tone of region 160A changes to yellow-blue with rotation.

[0276] (1-8. Measurement of contrast and color change of identification medium (1))

[0277] The identification medium (1) was kept in a horizontal position, and the azimuth angle of the identification medium (1) was rotated 360 degrees under a D65 light source. The display surfaces 160A and 160B were observed from a vertical direction through a linear polarizer based on the method of JIS Z 8781-4. The respective L* values, a* values, and b* values ​​(L*(160A), a*(160A), b*(160A), L*(160B), a*(160B), and b*(160B)) were measured using a spectrophotometer CM-700d manufactured by Konica Minolta under SCE as the measurement condition. These values ​​change with the change of the azimuth angle of the identification medium.

[0278] The difference |L*(160A)-L*(160B)| between L*(160A) and L*(160B) at various azimuth angles θ was measured, and the value of |L*(160A)-L*(160B)| at θ where this value was the largest was defined as ΔL*.

[0279] In addition, √(|a*(160A)-a*(160B)|^2+|b*(160A)-b*(160B)|^2) of various azimuth angles θ is measured, and the value of √(|a*(160A)-a*(160B)|^2+|b*(160A)-b*(160B)|^2) of θ with the largest value is taken as Δa*b*.

[0280] The results are shown in Table 3.

[0281] (1-9. Reflectivity)

[0282] The reflectance when non-polarized light (wavelength 450nm to 650nm) was incident on the area 160B of the display surface 160 of the identification medium (1) was measured using an ultraviolet-visible spectrophotometer with an integrating sphere ("UV-Vis770" manufactured by JASCO Corporation), and the average reflectance at wavelengths of 450nm to 650nm was determined. The results are shown in Table 3.

[0283] [Examples 2 to 9, 13 to 14 and Comparative Example 1]

[0284] The type and ratio of the CLC sheets mixed in (1-1) were changed as shown in Table 2. In addition, light reflecting layers 2 to 9 and 10 to 12 with a thickness of 40 μm were obtained by the same method as in Example 1, and then identification media (2) to (9) and (13) to (15) were obtained and evaluated using them.

[0285] The results are shown in Tables 2 and 3.

[0286] In any of the examples and comparative examples, in the observation of the identification medium (corresponding to (1-7) of Example 1), in the observation with the naked eye, the patterned phase difference layer 140 is observed as a transparent member in the display surface 160, and its star-shaped shape is almost invisible. No difference in brightness and color between the area 160A and the area 160B in the display surface 160 is observed, and it does not change due to rotation. The appearance of the display surface 160 in the observation with the naked eye is shown in Table 3.

[0287] When observed through polarized sunglasses, the star-shaped shape of region 160A is observed. The difference in brightness between region 160A and region 160B changes with rotation. In addition, the color tone of region 160A changes as shown in Table 3 with rotation in the embodiment, but does not change in the comparative example.

[0288] [Examples 10 to 12]

[0289] Identification media (10) to (12) were obtained and evaluated in the same manner as in Examples 1 to 3 except for the following changes.

[0290] As the patterned phase difference layer in (1-6), the star-shaped λ / 2 stretched resin film obtained in Production Example 41 was used instead of the star-shaped λ / 4 stretched resin film obtained in Production Example 40.

[0291] In the observation of the identification medium (1-7) and (1-8), a circular polarizer was used instead of the linear polarizer of the polarized sunglasses. As the circular polarizer, both the observation using a right-handed circular polarizer and the observation using a left-handed circular polarizer were used, and the observation results were compared. When calculating the ΔL* value and Δa*b*, for |L*(160A)-L*(160B)| and √(|a*(160A)-a*(160B)|^2+|b*(160A)-b*(160B)|^2, the larger of the values ​​obtained by the observation using the right-handed circular polarizer and the values ​​obtained by the observation using the left-handed circular polarizer was used as the ΔL* value and Δa*b*.

[0292] In any of the examples and comparative examples, in the observation of the identification medium (corresponding to (1-7) of Example 1), in the observation with the naked eye, the patterned phase difference layer 140 is observed as a transparent member in the display surface 160, and its star-shaped shape is almost invisible. No difference in brightness and color between the area 160A and the area 160B in the display surface 160 is observed, and it does not change due to rotation. The appearance of the display surface 160 in the observation with the naked eye is shown in Table 3.

[0293] In the observation across the circular polarizer, the star-shaped shape of region 160A is observed. The difference in the brightness of region 160A and the brightness of region 160B, when using one of right-handed circular polarizer and left-handed circular polarizer, region 160A is relatively bright, and when using the other, region 160B is relatively bright. In addition, the hue of region 160A changes in the manner shown in Table 3 according to the change of the circular polarizer. The hue of region 160B also changes according to the change of the circular polarizer, but its change mode is opposite to region 160B. That is, the hue viewed when using the right-handed circular polarizer to observe region 160A is viewed when using the left-handed circular polarizer to observe region 160B, and the hue viewed when using the left-handed circular polarizer to observe region 160A is viewed when using the right-handed polarizer to observe region 160B.

[0294] Other evaluation results are shown in Tables 2 and 3.

[0295] [Comparative Example 2]

[0296] A light reflecting layer 13 having a thickness of 40 μm and an identification medium ( 16 ) were obtained and evaluated in the same manner as in Example 1 except that the type of CLC sheet mixed in (1-1) was changed to only CLC sheet_S.

[0297] In the observation of the identification medium (corresponding to (1-7) of Example 1), the following results were obtained. That is, in the observation with the naked eye, a colorless, non-pearlescent silver appearance produced by the reflection of the light reflecting layer 120 was observed in the display surface 160. The patterned phase difference layer 140 was observed as a transparent component, and its star shape was almost invisible. No difference in brightness between the area 160A and the area 160B in the display surface 160 was observed, and it did not change with rotation. In the observation through polarized sunglasses, the star shape of area 160A was observed. The difference in brightness between area 160A and area 160B changes with rotation. The color tone of area 160A does not change with rotation.

[0298] Other evaluation results are shown in Tables 2 and 3.

[0299] [Table 2]

[0300] Table 2

[0301]

[0302] In Table 2, the type of the chip used is indicated by the end of the symbol of each chip. For example, "aL" in the R column indicates that the CLC chip_RaL is used.

[0303] [Table 3]

[0304] Table 3

[0305]

[0306] According to the results shown in Table 3, in the identification medium of the present invention, the appearance of the light reflection layer is a variety of appearances such as silver with a pearly feel, and the design of the beauty that cannot be expected by each sheet monomer is brought into play. In addition, the visibility of the latent image composed of the patterned phase difference layer that cannot be viewed with the naked eye is also large in the light and dark contrast difference (L*) and color change (Δa*b*), and can be clearly viewed. The latent image visibility brought about by the contrast difference and color change has the same usefulness as the case of using the silver CLC layer obtained by the wide-band processing known in the art, or substantially different usefulness, so it can be said that the identification medium of the present invention can show useful latent image visibility even without the complex processing for wide-band processing.

[0307] Description of Reference Numerals

[0308] 100: Identify the medium

[0309] 110: Light absorption layer

[0310] 120: Light reflection layer

[0311] 131: Adhesive layer

[0312] 132: Adhesive layer

[0313] 140: Patterned phase difference layer

[0314] 150: Coating layer

[0315] 160: Display surface

[0316] 160A: Area

[0317] 160B: Area

Claims

1. An identification medium comprising a light reflecting layer and a patterned phase difference layer, The light reflecting layer is a layer that reflects incident light into circularly polarized light. The patterned phase difference layer is a layer including a region having a phase difference, and is provided on the identification medium in such a manner that the region having a phase difference occupies a part of the display surface of the identification medium. The light reflecting layer comprises flakes (i) and flakes (ii) as flakes of a material having cholesteric regularity, The colors of the sheet (i) and the sheet (ii) are different from each other, and The rotation direction of the light reflected by the sheet (i) and the rotation direction of the light reflected by the sheet (ii) are different from each other.

2. The identification medium according to claim 1, wherein: The light-reflecting layer further includes a sheet (iii) as a sheet of the material having cholesteric regularity, and the sheet (iii) has a color different from that of either the sheet (i) or the sheet (ii).

3. The identification medium according to claim 1, wherein: The light reflecting layer satisfies the following formulas (b-1) to (b-2): 0.90≤B(430-490)Ave / G(500-600)Ave≤1.05Formula (b-1) 0.90≤R(600-660)Ave / G(500-600)Ave≤1.05 Formula (b-2) In the formula, B(430-490)Ave is the average value of the integrated reflectivity of the light reflecting layer at wavelengths of 430 nm to 490 nm, G(500-600)Ave is the average value of the integrated reflectivity of the light reflecting layer at a wavelength of 500 nm to 600 nm, R(600-660)Ave is an average value of the integrated reflectivity of the light reflecting layer at a wavelength of 600 nm to 660 nm.

4. The identification medium according to claim 3, wherein the light reflecting layer satisfies the following formulas (b-1') to (b-2'): 0.92≤B(430-490)Ave / G(500-600)Ave≤1.04Formula (b-1') 0.92≤R(600-660)Ave / G(500-600)Ave≤1.04Formula (b-2') 5. The identification medium according to claim 1, wherein The light reflecting layer exhibits a color ranging from light tint to silver.

6. The identification medium according to claim 1, wherein Any one of the sheets of the material having cholesteric regularity in the light reflecting layer satisfies the formula (c), 0.10≤△λλc≤0.25Formula (c) Wherein, Δλ is the half-peak width of the reflection band of the sheet, and λc is the selective reflection center wavelength of the sheet.

7. The identification medium according to claim 6, wherein: All the pieces of the material having cholesteric regularity in the light reflecting layer satisfy the formula (c).

8. The identification medium according to claim 1, wherein The patterned phase difference layer is a λ / 4 wave plate or a λ / 2 wave plate.

9. The identification medium according to claim 1, wherein: The thickness of the sheet is 3 μm or more and 7 μm or less.

10. The identification medium according to claim 1, wherein The average particle size of each of the flakes is 100 μm or less.

11. The identification medium according to claim 1, wherein The patterned phase difference layer is located closer to the viewing side than the light reflecting layer.

12. The identification medium according to claim 1, wherein The light reflecting layer further includes a sheet having a reflection band including a region having a wavelength greater than 660 nm.

13. The identification medium according to claim 1, wherein: The average value of the integrated reflectivity of the light reflecting layer at 430 to 660 nm is greater than 20%.

14. The identification medium according to claim 1, wherein The identification medium further includes a light absorbing layer at a position on the opposite side of the light reflecting layer to the viewing side.

15. The identification medium according to claim 1, wherein The identification medium has a coating layer at a position closer to the viewing side than the patterned phase difference layer.

16. The identification medium according to claim 1, wherein The identification medium further includes a mounting member for mounting the identification medium on an article. 17 . An article comprising the identification medium according to claim 1 .