Negative electrode for lithium secondary battery and method for producing same
By designing specific negative electrode active layer structure and processing technology on the negative electrode of lithium secondary battery, the problem of N/P ratio inversion and fast charging characteristics is solved, and high negative electrode active material load and excellent fast charging performance are achieved.
Patent Information
- Application Number
- CN202380029061.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-02-09
- Filing Date
- 2023-11-27
- Publication Date
- 2024-11-05
AI Technical Summary
During the manufacturing process of lithium secondary battery, during the positive electrode and negative electrode stacking, the N/P ratio inversion phenomenon causes lithium ions to be unable to embed negative electrode active material, forming dendrites, impairing battery safety, and increasing the load of negative electrode active material reduces fast charging characteristic.
Design a lithium secondary battery negative electrode, which includes a negative current collector and an negative electrode active layer. The negative electrode active layer is divided into a central area, an edge area and a landslide area. Through magnetic field processing and rolling technology, a specific arrangement value ratio and thickness are met. Gradient conditions to increase the load and orientation of the negative electrode active material and prevent lithium precipitation.
It achieves a high load of negative electrode active material at the end of the negative electrode active layer, inhibits lithium precipitation, and maintains or improves fast charging performance, enhancing the safety and energy density of the battery.
Smart Images

Figure CN118901151A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a negative electrode for a lithium secondary battery and a method for producing the same.
[0002] This application claims priority to Korean Patent Application No. 10-2022-0183016 filed on December 23, 2022 and Korean Patent Application No. 10-2023-0017427 filed on February 9, 2023, the disclosures of which are incorporated herein by reference in their entirety. Background Art
[0003] In recent years, secondary batteries have been widely used in small devices such as portable electronic devices and medium and large devices such as battery packs or power storage in hybrid electric vehicles or electric vehicles.
[0004] These secondary batteries are rechargeable / dischargeable power generation devices composed of a stacked structure of positive electrode / separator / negative electrode, wherein the positive electrode generally contains lithium metal oxide as the positive electrode active material, and the negative electrode contains a carbon-based active material such as graphite, so that lithium ions emitted from the positive electrode during charging are adsorbed into the carbon-based active material of the negative electrode, and lithium ions contained in the carbon-based active material during discharging are adsorbed into the lithium metal oxide of the positive electrode, and charging and discharging are repeated.
[0005] Meanwhile, one of the factors that determine the performance of a secondary battery is the capacity ratio of the active materials contained in the positive electrode and the negative electrode, respectively. The capacity ratio can be expressed as an N / P ratio, which is the total capacity of the negative electrode obtained by considering the capacity per unit area and / or weight of the negative electrode divided by the total capacity of the positive electrode obtained by considering the capacity per unit area and / or weight of the positive electrode, and is generally controlled to have a value of 1 or more because it has a significant impact on the safety and capacity of the battery.
[0006] However, in the manufacturing process of lithium secondary batteries, a reversal phenomenon in which the N / P ratio becomes less than 1 occurs when the positive electrode active layer leaves the negative electrode active layer during the lamination of the positive and negative electrodes. In this case, when the N / P ratio becomes less than 1, lithium ions cannot be embedded in the negative electrode active material during battery charging and precipitate on the negative electrode surface to form dendrites. Such dendrites are particularly likely to occur when lithium secondary batteries are used for a long time under high rate conditions. These dendrites may cause a short circuit inside the battery, thereby compromising the safety of the battery.
[0007] To address this problem, conventional attempts have been made to increase the negative electrode active material loading at the end of the negative electrode active layer. However, this has the following limitations: as the loading of the negative electrode active material increases, the distance lithium ions travel in the negative electrode increases, which may lead to a decrease in fast charging characteristics, etc., thereby reducing the commercial viability of the battery.
[0008] Therefore, there is a great need for a technology that can maintain or improve the rapid charge characteristics above a certain level even when the negative electrode active material loading at the end of the negative electrode active layer is increased to suppress lithium precipitation at the end of the negative electrode active layer. Summary of the invention
[0009] [Technical issues]
[0010] The present invention aims to provide a negative electrode for a lithium secondary battery and a method for manufacturing the same, wherein the negative electrode for a lithium secondary battery has a high negative electrode active material loading at the end of the negative electrode active layer and has excellent rapid charging performance, thereby suppressing lithium precipitation at the end of the negative electrode active layer.
[0011] [Technical solution]
[0012] In order to solve the above problems, in an exemplary embodiment, the present invention provides a negative electrode for a lithium secondary battery, comprising:
[0013] A negative electrode current collector; and
[0014] a negative electrode active layer, which is disposed on at least one side of the negative electrode current collector and comprises a carbon-based negative electrode active material,
[0015] wherein the negative electrode active layer is divided into: a central region including the central portion of the negative electrode active layer in the width direction; a landslide region located at the edge of the negative electrode active layer and having a thickness gradient; and an edge region located between the central region and the landslide region; and
[0016] The negative electrode active layer satisfies the following equations 1 and 2:
[0017] [Equation 1]
[0018] 2.7≤[OI 边缘 ] / [OI 中心 ]≤4.8
[0019] [Equation 2]
[0020] 1.5≤[OI 滑坡 ] / [OI 中心 ]≤2.6
[0021] In Equation 1 and Equation 2,
[0022] OI 边缘 Indicates the arrangement value (OI) of the edge area,
[0023] OI 中心 Indicates the arrangement value (OI) of the center area,
[0024] OI 滑坡represents the ranking index (OI) of the landslide area, and
[0025] The arrangement value (OI) represents the peak area (I) representing the [0,0,4] crystal plane in the XRD measurement result of the negative electrode active layer. 004 ) and the peak area representing the [1,1,0] crystal plane (I 110 ) ratio (I 004 / I 110 ).
[0026] Here, the alignment value (OI) of the central region of the negative electrode active layer 中心 ) can be from 0.7 to 1.5.
[0027] Furthermore, the ratio of the central region of the negative electrode active layer in the total length in the width direction of the negative electrode active layer may be at least 90%, and the ratio of the landslide region of the negative electrode active layer in the total length in the width direction of the negative electrode active layer may be 3% or less.
[0028] Meanwhile, the average thickness of the central region of the negative electrode active layer is 100 μm to 300 μm, and the exposed surface of the landslide region of the negative electrode active layer may have an inclination angle of 70° or more relative to the negative electrode current collector.
[0029] Meanwhile, the carbon-based active material may include at least one of natural graphite and artificial graphite.
[0030] In addition, in an exemplary embodiment, the present invention provides a method for manufacturing a negative electrode for a lithium secondary battery, comprising:
[0031] applying a negative electrode slurry including a carbon-based active material onto a negative electrode current collector;
[0032] applying a magnetic field to the applied negative electrode slurry; and
[0033] The negative electrode slurry to which the magnetic field is applied is dried to form a negative electrode active layer.
[0034] wherein the negative electrode active layer is divided into: a central region including the central portion of the negative electrode active layer in the width direction; a landslide region located at the edge of the negative electrode active layer and having a thickness gradient; and an edge region located between the central region and the landslide region; and
[0035] The negative electrode active layer satisfies the following equations 1 and 2:
[0036] [Equation 1]
[0037] 2.7≤[OI 边缘 ] / [OI 中心 ]≤4.8
[0038] [Equation 2]
[0039] 1.5≤[OI 滑坡 ] / [OI 中心 ]≤2.6
[0040] In Equation 1 and Equation 2,
[0041] OI 边缘 Indicates the arrangement value (OI) of the edge area,
[0042] OI 中心 Indicates the arrangement value (OI) of the center area,
[0043] OI 滑坡 represents the ranking index (OI) of the landslide area, and
[0044] The arrangement value (OI) represents the peak area (I) representing the [0,0,4] crystal plane in the XRD measurement result of the negative electrode active layer. 004 ) and the peak area representing the [1,1,0] crystal plane (I 110 ) ratio (I 004 / I 110 ).
[0045] Here, in the step of applying the negative electrode slurry, the applied negative electrode slurry may satisfy the following equation 3:
[0046] [Equation 3]
[0047] R 滑坡 <R 中心 <R 边缘
[0048] In equation 3,
[0049] R 滑坡 represents the average thickness of the landslide area,
[0050] R 边缘 represents the average thickness of the edge region,
[0051] R 中心 represents the average thickness of the central region.
[0052] In addition, the step of applying a magnetic field applies a magnetic field of 2,000 G to 6,000 G, and the application time may be 5 seconds to 60 seconds.
[0053] Furthermore, the step of applying the magnetic field is performed by introducing magnetic members at the upper and lower parts of the applied negative electrode slurry, the length of the magnetic members being 105% to 200% of the length of the negative electrode slurry in the width direction.
[0054] In addition, the step of forming the negative electrode active layer includes: drying the negative electrode slurry; and rolling the dried negative electrode slurry.
[0055] Here, the thickness ratio of the edge region of the negative electrode active layer may be 105% to 130% based on the average thickness of the central region of the negative electrode active layer before rolling.
[0056] [Beneficial Effects]
[0057] The negative electrode of the present invention includes a negative electrode active layer on a negative electrode current collector, and the negative electrode active layer is divided into a central region, an edge region, and a landslide region, whereby lithium precipitation at the end of the negative electrode active layer can be suppressed by making the arrangement value (OI) of each carbon-based negative electrode active material contained in the central region, the edge region, and the landslide region satisfy equations 1 and 2. In addition, the secondary battery including the negative electrode has an advantage of excellent fast charging performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 and Figure 2 It is a diagram showing the cross-sectional structure of the negative electrode of the present invention.
[0059] Figure 3 This is a diagram showing the cross-sectional structure of a negative electrode active layer before roll pressing after the negative electrode slurry is dried in the production of the negative electrode of the present invention. DETAILED DESCRIPTION
[0060] The invention is susceptible to various modifications and may have numerous embodiments, some of which are described in detail below.
[0061] However, this is not intended to limit the present invention to any specific embodiment, and should be construed to include all modifications, equivalents, or replacements falling within the scope of the idea and technology of the present invention.
[0062] The terms "comprising" or "having" are used herein to indicate the presence of features, numbers, steps, actions, components or members, or a combination thereof, described in the specification, and it should be understood that the possibility of the presence or addition of one or more other features, numbers, steps, actions, components, members, or a combination thereof is not excluded in advance.
[0063] Furthermore, when a portion of a layer, film, region, or plate is disposed “on” another portion, this includes not only a case where the portion is disposed “directly” “on” another portion, but also a case where a third portion is interposed therebetween. Conversely, when a portion of a layer, film, region, or plate is disposed “under” another portion, this includes not only a case where the portion is disposed “directly” “under” another portion, but also a case where a third portion is interposed therebetween. Furthermore, in the present application, “on” may include not only a case where it is disposed on an upper portion, but also a case where it is disposed on a lower portion.
[0064] In addition, in the present invention, "comprising ... as a main component" may refer to containing 50% by weight or more (or 50% by volume or more), 60% by weight or more (or 60% by volume or more), 70% by weight or more (or 70% by volume or more), 80% by weight or more (or 80% by volume or more), 90% by weight or more (or 90% by volume or more), or 95% by weight or more (or 95% by volume or more) of a defined component relative to the total weight (or total volume). For example, "comprising graphite as a main component of the negative electrode active material" may refer to containing at least 50% by weight, at least 60% by weight, at least 70% by weight, at least 80% by weight, at least 90% by weight, or at least 95% by weight of graphite based on the total weight of the negative electrode active material, and in some cases may refer to the entire negative electrode active material being composed of graphite and containing 100% of graphite.
[0065] In addition, as used herein, "carbon-based negative electrode active materials are oriented" or "carbon-based negative electrode active materials are arranged" may refer to that the crystal planes of the carbon-based negative electrode active materials constituting the negative electrode active material particles are distributed in a predetermined orientation relative to the surface of the negative electrode current collector, which may be different from the carbon-based negative electrode active material particles themselves being arranged to have a specific orientation within the negative electrode active layer.
[0066] In addition, "highly oriented carbon-based negative electrode active material" may refer to that the carbon-based negative electrode active material contained in the negative electrode active layer is arranged at a high frequency relative to the surface of the negative electrode collector, and in some cases, the carbon-based negative electrode active material contained in the negative electrode active layer is arranged at a high angle relative to the surface of the negative electrode collector.
[0067] In addition, "a high alignment value of a carbon-based negative electrode active material" may refer to a larger value of the "alignment value (OI)" mentioned herein, which means that the carbon-based negative electrode active material contained in the negative electrode active layer is arranged at a low angle relative to the surface of the negative electrode current collector. Conversely, "a low alignment value of a carbon-based negative electrode active material" means that the "alignment value (OI)" has a smaller value, which may indicate that the carbon-based negative electrode active material contained in the negative electrode active layer is arranged at a high angle relative to the surface of the negative electrode current collector.
[0068] The present invention will now be described in more detail.
[0069] Negative electrode for lithium secondary battery
[0070] In an exemplary embodiment, the present invention provides a negative electrode for a lithium secondary battery, comprising:
[0071] A negative electrode current collector; and
[0072] a negative electrode active layer, which is disposed on at least one side of the negative electrode current collector and comprises a carbon-based negative electrode active material,
[0073] wherein the negative electrode active layer is divided into: a central region including the central portion of the negative electrode active layer in the width direction; a landslide region located at the edge of the negative electrode active layer and having a thickness gradient; and an edge region located between the central region and the landslide region; and
[0074] The negative electrode active layer satisfies the following equations 1 and 2:
[0075] [Equation 1]
[0076] 2.7≤[OI 边缘 ] / [OI 中心 ]≤4.8
[0077] [Equation 2]
[0078] 1.5≤[OI 滑坡 ] / [OI 中心 ]≤2.6
[0079] In Equation 1 and Equation 2,
[0080] OI 边缘 Indicates the arrangement value (OI) of the edge area,
[0081] OI 中心 Indicates the arrangement value (OI) of the center area,
[0082] OI 滑坡 represents the ranking index (OI) of the landslide area, and
[0083] The arrangement value (OI) represents the peak area (I 004 ) and the peak area representing the [1,1,0] crystal plane (I 110 ) ratio (I 004 / I 110 ).
[0084] Figure 1 and Figure 2 2 is a cross-sectional view showing the structure of negative electrodes 100 and 200 of the present invention, in which a negative electrode active layer is provided on one surface of a negative electrode current collector.
[0085] The negative electrode 100 and 200 for lithium secondary battery of the present invention includes a negative electrode active layer 120 and 220 containing a carbon-based negative electrode active material located on at least one side of the negative electrode current collector 110 and 210. The negative electrode active layer 120 and 220 is a layer that realizes the electrical activity of the negative electrode. The negative electrode active layer 120 and 220 is prepared by applying a negative electrode slurry containing a negative electrode active material to at least one side of the negative electrode current collector 110 and 210, and then drying and rolling. The negative electrode active material performs an electrochemical redox reaction during battery charge and discharge.
[0086] In this case, the negative electrode active layers 120 and 220 are divided into a central region, an edge region, and a landslide region in the width direction of the negative electrodes 100 and 200. Specifically, the negative electrode active layers 120 and 220 include a central region in the width direction, and include central regions 121 and 221, the ratio of which in the total length in the width direction is at least 90%. The central regions 121 and 221 constitute most of the negative electrode active layers 120 and 220, and the ratio in the total length in the width direction of the negative electrode active layers 120 and 220 may be at least 93%, at least 95%, at least 97%, or at least 96% to 99%. As used herein, "the width direction of the negative electrode active layers 120 and 220" may mean a direction perpendicular to the direction in which the negative electrode current collector travels during the manufacture of the negative electrode. In some cases, the "width direction of the negative electrode active layers 120 and 220" may be the same as the direction from the side where the negative electrode tab is formed to the opposite side thereof when the negative electrode is manufactured. By adjusting the length ratio of the central regions 121 and 221 of the negative electrode active layers 120 and 220 to the above range, the present invention can further improve the energy density of the negative electrode.
[0087] In addition, the edge regions 122 and 222 are located outside the central regions 121 and 221 , and the landslide regions 123 and 223 are located outside the edge regions 122 and 222 .
[0088] In this case, the edge area and the landslide area can be sequentially and continuously arranged on both sides of the central area 121, such as Figure 1 In some cases, due to the punching (or notching) of the electrode sheet during the manufacture of the negative electrode, the edge region and the landslide region may be sequentially and continuously disposed on only one side of the central region 221, as shown in FIG. Figure 2 shown.
[0089] The landslide regions 123 and 223 are regions with a thickness gradient located at the edges of the negative electrode active layers 120 and 220. The ratio of the landslide regions 123 and 223 in the total length in the width direction of the negative electrode active layers 120 and 220 may be 3% or less. Specifically, considering the energy density of the negative electrode, the landslide regions 123 and 223 may have a shape in which the thickness decreases outward in the region adjacent to the edge regions 122 and 222, and the ratio in the total length in the width direction of the negative electrode active layers 120 and 220 may be 2% or less, 1% or less, 0.5% or less, 0.01% to 1%, or 0.01% to 0.5%. In this case, the length ratio is based on the ratio of the total length in the width direction of the negative electrode active layers 120 and 220, and when as Figure 1 When the landslide areas 123 and 223 are arranged on both sides of the central area 121, the length ratio of each landslide area can be halved to 1 / 2 of the length ratio.
[0090] In addition, the landslide regions 123 and 223 may have a thickness gradient with a thickness gradually decreasing outwardly, so that the exposed surface may have a predetermined inclination angle relative to the negative electrode current collectors 110 and 210. For example, the exposed surface of the landslide regions 123 and 223 may have an inclination angle of more than 70° relative to the negative electrode current collectors 110 and 210, so that it has a thickness gradient that gradually decreases outwardly. Specifically, the inclination angle of the exposed surface of the landslide regions 123 and 223 may be more than 75°, more than 80°, more than 85°, 70 to 85°, 75 to 80°, 70 to 75° relative to the negative electrode current collectors 110 and 210. By adjusting the inclination angle of the exposed surface of the landslide regions 123 and 223 relative to the negative electrode current collectors 110 and 210 to the above range, the present invention can prevent the N / P ratio from being reversed at the end of the electrode assembly assembled with the positive electrode, and can further improve the adhesion of the negative electrode end to the separator.
[0091] In addition, by having a higher negative electrode active material loading than the central regions 121 and 221, when the stacking position of the negative electrode active layer is outside the negative electrode active layer in the secondary battery, the edge regions 122 and 222 can prevent lithium from being precipitated from the ends of the negative electrode active layers 120 and 220 by suppressing the N / P ratio from becoming less than 1.
[0092] In this case, the edge regions 122 and 222 may occupy the remaining length except for the length ratio of the above-mentioned central regions 121 and 221 and the landslide regions 123 and 223. For example, the ratio of the edge regions 122 and 222 in the total length in the width direction of the negative electrode active layers 120 and 220 may be less than 7%, less than 5%, less than 4%, less than 2.5%, 0.09% to 3%, or 0.5% to 1%. The edge regions 122 and 222 may be arranged on both sides of the central region 121, and the landslide regions 123 and 223 may also be so, so that the length ratio of each edge region may be halved to 1 / 2 of the length ratio.
[0093] In addition, the negative electrodes 100 and 200 of the present invention have excellent fast charging performance. As described above, by controlling the unit area loading of the carbon-based negative electrode active material in the edge regions 122 and 222 to be higher than the unit area loading of the carbon-based negative electrode active material in the central regions 121 and 221, the negative electrodes 100 and 200 can prevent lithium from being precipitated from the ends of the negative electrode active layers 120 and 220 due to the reversal of the N / P ratio between the negative electrode and the positive electrode. However, in this case, the edge regions 122 and 222 having a higher carbon-based negative electrode active material loading than the remaining regions may increase the structural tortuosity of the negative electrode active layer, thereby increasing the travel distance of lithium ions and reducing the diffusion rate, which may cause lithium to precipitate from the negative electrode surface during fast charging. Therefore, the negative electrode 100 and 200 of the present invention solves this problem by orienting the carbon-based negative electrode active material contained in the negative electrode active layer 120 and 220 so that the crystal plane angle of the negative electrode active layer 120 and 220 relative to the surface of the negative electrode current collector 110 and 210 is reduced, but the oriented carbon-based negative electrode active material has a predetermined tendency in each region of the negative electrode active layer 120 and 220. Here, the orientation and / or arrangement value of the carbon-based negative electrode active material (e.g., graphite) can be determined by crystal plane analysis of the carbon-based negative electrode active material (CA) contained in the negative electrode active layer.
[0094] In one example, the negative active layers 120 and 220 may satisfy the following equations 1 and 2:
[0095] [Equation 1]
[0096] 2.7≤[OI 边缘 ] / [OI 中心 ]≤4.8
[0097] [Equation 2]
[0098] 1.5≤[OI 滑坡 ] / [OI 中心 ]≤2.6
[0099] In Equation 1 and Equation 2,
[0100] OI 边缘 Indicates the arrangement value (OI) of the edge area,
[0101] OI 中心 Indicates the arrangement value (OI) of the center area,
[0102] OI 滑坡 represents the ranking index (OI) of the landslide area, and
[0103] The arrangement value (OI) represents the peak area (I 004 ) and the peak area representing the [1,1,0] crystal plane (I 110 ) ratio (I 004 / I 110 ).
[0104] The arrangement value (OI) of the carbon-based negative electrode active material (CA) can be an indicator of the degree to which the crystal structure of the spherical carbon-based negative electrode active material is oriented in a specific direction, especially relative to the orientation of the surface of the negative electrode current collector, which is measured by X-ray diffraction (XRD). More specifically, the negative electrode active layer can be characterized by X-ray diffraction measurement, which shows the peaks of carbon-based negative electrode active material graphite at 2θ=26.5±0.2°, 42.4±0.2°, 43.4±0.2°, 44.6±0.2°, 54.7±0.2° and 77.5±0.2°, which represent [0,0,2] plane, [1,0,0] plane, [1,0,1]R plane, [1,0,1]H plane, [0,0,4] plane and [1,1,0] plane, respectively. The peak at 2θ=43.4±0.2° can also be regarded as the overlap of peaks corresponding to the [1,0,1]R plane of the carbon-based negative active material (CA) and the [1,1,1] plane of the current collector (eg, copper (Cu)).
[0105] Among them, the arrangement value (OI) of the carbon-based negative electrode active material (CA) can be measured by using the ratio of the peak area at 2θ=54.7±0.2° representing the [0,0,4] plane to the peak area at 2θ=77.5±0.2° representing the [1,1,0] plane, and more specifically, the ratio of the areas obtained by integrating the intensities of the above peaks.
[0106] Here, the peak at 2θ=54.7±0.2° is a peak of the [0,0,4] plane of the graphite crystal plane having a slope with the negative electrode current collector. Therefore, the arrangement value (OI) may mean that when the value is close to 0, the slope relative to the surface of the negative electrode current collector is close to 90°, and when the value is large, the slope relative to the surface of the negative electrode current collector is close to 0° or 180°. In other words, compared with the case where the carbon-based negative electrode active material (CA) is arranged at a low angle, the negative electrode active layer of the present invention may have a lower carbon-based negative electrode active material (CA) arrangement value (OI), so that the carbon-based negative electrode active material (CA) has a high angle relative to the negative electrode current collector (e.g., an angle of 60° or more, 70° or more, 70° to 90°, 80° to 90°, 65° to 85°, or 70° to 85°).
[0107] Taking this into account, Equation 1 shows the alignment value (OI 中心 ) than the alignment value (OI) of the carbon-based negative electrode active material in the edge region 边缘 ) is smaller. This means that the carbon-based negative electrode active material in the central region is arranged at a higher angle relative to the surface of the negative electrode current collector than the carbon-based negative electrode active material in the edge region. By arranging the carbon-based negative electrode active material in the central region at a higher angle relative to the negative electrode current collector than the carbon-based negative electrode active material in the edge region, the negative electrode active layers 120 and 220 of the present invention can satisfy Equation 1, where the ratio is 2.7 to 4.8 (i.e., 2.7≤[OI 边缘 ] / [OI 中心 ]≤4.8), more specifically 2.7 to 4.8 (i.e. 2.7≤[OI 边缘 ] / [OI 中心 ]≤4.8); 2.9 to 4.5 (i.e. 2.9≤[OI 边缘 ] / [OI 中心 ]≤4.5); 3.0 to 4.5 (i.e. 3.0≤[OI 边缘 ] / [OI 中心 ]≤4.5); 2.9 to 3.8 (i.e. 2.9≤[OI 边缘 ] / [OI 中心 ]≤3.8); 3.8 to 4.6 (i.e. 3.8≤[OI 边缘 ] / [OI 中心 ]≤4.6); or 3.1 to 4.2 (i.e. 3.1≤[OI 边缘 ] / [OI 中心 ]4.2).
[0108] In addition, Equation 2 shows the arrangement value of the carbon-based negative electrode active material in the central region (OI 中心) than the arrangement value (OI) of the carbon-based negative electrode active material in the landslide area. 滑坡 ) is smaller. This means that the carbon-based negative electrode active material in the central region is arranged at a higher angle relative to the surface of the negative electrode current collector than the carbon-based negative electrode active material in the landslide region. By arranging the carbon-based negative electrode active material in the central region at a higher angle relative to the negative electrode current collector than the carbon-based negative electrode active material in the landslide region, the negative electrode active layers 120 and 220 of the present invention can satisfy Equation 2, wherein the ratio is 1.5 to 2.6 (1.5≤[OI 滑坡 ] / [OI 中心 ]≤2.6), more specifically 1.8 to 2.6 (1.8≤[OI 滑坡 ] / [OI 中心 ]≤2.6); 1.7 to 2.3 (1.7≤[OI 滑坡 ] / [OI 中心 ]≤2.3); 2.2 to 2.5 (2.2≤[OI 滑坡 ] / [OI 中心 ]≤2.5); 1.9 to 2.2 (1.9≤[OI 滑坡 ] / [OI 中心 ]≤2.2); or 2.0 to 2.5 (2.0≤[OI 滑坡 ] / [OI 中心 ]≤2.5).
[0109] The arrangement value (OI) of the carbon-based negative electrode active material (CA) of each region of the negative electrode active layers 120 and 220 may satisfy a predetermined range so as to satisfy the conditions of equations 1 and 2. This keeps the average arrangement value of the carbon-based negative electrode active material CA contained in the negative electrode active layers 120 and 220 low as a whole. Specifically, the arrangement value (OI) of the carbon-based negative electrode active material (CA) contained in the central regions 121 and 221 of the negative electrode active layers 120 and 220 is 中心 ) may be 0.7 to 1.5, more specifically 0.7 to 1.3, 0.7 to 1.0, 0.9 to 1.2, or 0.8 to 1.1. In this case, the arrangement value (OI) of the central regions 121 and 221 is 中心 ) may have a deviation of 5% or less from the average arrangement value of the negative electrode active layers 120 and 220.
[0110] In addition, the arrangement value (OI) of the carbon-based negative electrode active material contained in the edge regions 122 and 222 边缘 ) may be greater than the arrangement value (OI) of the carbon-based negative electrode active material contained in the central regions 121 and 221. 中心This is because the edge regions 122 and 222 have a relatively high carbon-based negative electrode active material loading compared to the central regions 121 and 221, which may lead to the alignment value (OI 边缘 ) is slightly higher than the arrangement value (OI) of the carbon-based negative electrode active material contained in the central region. 中心 ), this is because of overcrowding of the carbon-based negative electrode active materials contained in the edge regions 122 and 222 during rolling after the carbon-based negative electrode active materials are oriented.
[0111] By adjusting the arrangement value (OI) of the carbon-based negative electrode active material (CA) contained in the central regions 121 and 221, the edge regions 122 and 222, and the landslide regions 123 and 223 of the negative electrode active layers 120 and 220, respectively, as described above, the present invention can obtain an ion migration channel that enables lithium ions to travel a shorter distance in each region. Therefore, the negative electrode of the present invention can prevent the increase in resistance caused by the long-distance travel of lithium ions during rapid charging, thereby preventing the charging performance from being reduced, and can prevent lithium from being precipitated from the negative electrode surface.
[0112] Meanwhile, the average thickness of the negative electrode active layers 120 and 220 may be 100 μm to 300 μm, more specifically 100 μm to 250 μm or 130 μm to 190 μm, and the average thickness may be the same as the average thickness of the central regions 121 and 221. By adjusting the average thickness of the negative electrode active layers 120 and 220 to the above range, the present invention can advantageously control the orientation of the carbon-based negative electrode active material (CA) contained in each region, which can improve the fast charging characteristics of the battery including the negative electrodes 100 and 200.
[0113] In addition, the negative electrode active layers 120 and 220 may have a structure in which two separate layers are stacked, depending on the battery mode or product application in which the negative electrode of the present invention is used, but not limited thereto. In this case, the negative electrode of the present invention may have a structure in which a first negative electrode active layer (not shown) is disposed on the negative electrode current collectors 110 and 210, and a second negative electrode active layer (not shown) is disposed on the first negative electrode active layer. In this case, the first negative electrode active layer and the second negative electrode active layer contain a carbon-based negative electrode active material (CA), but the carbon-based negative electrode active material (CA) contained in each layer may be the same or different.
[0114] In addition, the negative electrode active layers 120 and 220 include a carbon-based negative electrode active material (CA) as a negative electrode active material to achieve electrical activity through a reversible oxidation-reduction reaction during battery charge and discharge.
[0115] Carbon-based negative electrode active material (CA) refers to a material with carbon atoms as its main component, and such carbon-based negative electrode active material (CA) may include graphite. Graphite may include one or more of natural graphite and artificial graphite. Preferably, it may include natural graphite or a mixture of natural graphite and artificial graphite.
[0116] Preferably, the carbon-based negative electrode active material (CA) is a spherical graphite assembly formed by agglomeration of multiple flake graphites. Flake graphite includes natural graphite, artificial graphite, calcined carbon (bulk mesophase) based on tar and pitch, graphitized coke (raw coke, green coke, pitch coke, needle coke, petroleum coke, etc.), and preferably a variety of highly crystalline natural graphite assemblies are used. In addition, a graphite assembly can be formed by assembling 2 to 100 pieces, preferably 3 to 20 pieces of flake graphite.
[0117] In addition, the average particle size (D 50 ) can be 0.5μm to 20μm, and more specifically can be 0.5μm to 15μm, 0.5μm to 10μm, 5μm to 20μm, 10μm to 20μm, 12μm to 18μm, 2μm to 7μm, 0.5μm to 5μm or 1μm to 3μm.
[0118] The average particle size of natural graphite can be advantageously made smaller to maximize the disorder of each particle in the expansion direction, thereby preventing particle expansion due to the charging of lithium ions. However, when the particle size of natural graphite is less than 0.5 μm, a large amount of binder may be required due to the increase in the number of particles per unit volume. On the other hand, if the average particle size exceeds 20 μm, the expansion becomes severe, resulting in deterioration of the cohesion between particles and between particles and current collectors with repeated charge and discharge, which may significantly reduce the cycle characteristics.
[0119] Furthermore, in addition to the main component of the carbon-based negative electrode active material (CA), the negative electrode active layer of the present invention may optionally include a conductive material, a binder, other additives, etc. as required.
[0120] The conductive material may include one or more of carbon black, acetylene black, Ketjen black, carbon nanotubes, carbon fibers, etc., but is not limited thereto.
[0121] In one example, the negative electrode active layer may include carbon black, carbon nanotubes, carbon fibers, etc., alone or in combination, as the conductive material.
[0122] In this case, the content of the conductive material may be 0.1 to 10 parts by weight based on a total of 100 parts by weight of the negative electrode active layer. Specifically, the content of the conductive material may be 0.1 to 8 parts by weight, 0.1 to 5 parts by weight, 0.1 to 3 parts by weight, 2 to 6 parts by weight, or 0.5 to 2 parts by weight. By controlling the content of the conductive material within the range described above, the present invention can prevent the resistance of the negative electrode from increasing due to the low content of the conductive material and reducing the charge capacity. In addition, the present invention can prevent the content of the negative electrode active material from decreasing due to an excess of conductive material to cause a decrease in charge capacity or prevent the rapid charge characteristics from decreasing due to an increase in the load of the negative electrode active layer.
[0123] In addition, the binder can be suitably applied as a component that helps the bonding of the negative electrode active material to the conductive material and to the current collector, and the degree does not reduce the electrical properties of the electrode. Specifically, the binder may include one or more selected from the group consisting of vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVdF), polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber (SBR) and fluorinated rubber.
[0124] Based on a total of 100 parts by weight of the negative electrode active layer, the content of the binder may be 0.1 to 10 parts by weight, more specifically 0.1 to 8 parts by weight, 0.1 to 5 parts by weight, 0.1 to 3 parts by weight, or 2 to 6 parts by weight. By controlling the content of the binder contained in the negative electrode active layer within the above range, the present invention can prevent the adhesion degradation of the active layer caused by the low content of the binder, or prevent the degradation of the electrical properties of the electrode caused by the excessive amount of the binder.
[0125] In addition, the negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, nickel, titanium, calcined carbon, etc. can be used, and in the case of copper or stainless steel, those surface-treated with carbon, nickel, titanium, silver, etc. can also be used. In addition, considering the conductivity and total thickness of the manufactured negative electrode, the average thickness of the negative electrode current collector can be appropriately adopted to be 1 to 500 μm.
[0126] Lithium secondary battery
[0127] Furthermore, in one embodiment, the present invention provides a lithium secondary battery including an electrode assembly including a positive electrode, the negative electrode of the present invention as described above, and a separator disposed between the positive electrode and the negative electrode.
[0128] The lithium secondary battery of the present invention includes: an electrode assembly having a plurality of positive electrodes, a separator and a negative electrode arranged in sequence; and an electrolyte composition having a lithium salt and an electrolyte additive dissolved in a non-aqueous organic solvent. Here, the lithium secondary battery includes a negative electrode having a structure in which a negative electrode active layer is stacked on a negative electrode current collector, and the negative electrode active layer is divided into a central region, an edge region and a landslide region, wherein the arrangement value (OI) of each carbon-based negative electrode active material contained in the central region, the edge region and the landslide region satisfies equations 1 and 2. Therefore, the lithium secondary battery has the advantage of having excellent fast charging characteristics, while lithium precipitation does not occur at the end of the negative electrode active layer during charging and discharging.
[0129] In this case, the negative electrode has the same configuration as described above, and thus a detailed description is omitted.
[0130] In addition, the positive electrode may be provided with a positive electrode active layer, which is prepared by coating, drying and pressing a slurry containing a positive electrode active material on a positive electrode current collector. Here, in addition to the positive electrode active material, the positive electrode active layer may optionally include a conductive material, a binder, other additives, etc. as needed.
[0131] The positive electrode active material may include one or more of lithium metal oxides represented by the following Chemical Formula 1 and Chemical Formula 2, which can undergo an electrochemical reaction on the positive electrode current collector to reversibly intercalate and deintercalate lithium ions:
[0132] [Chemical formula 1]
[0133] Li x [Ni y Co z Mn w M 1 v ]O2
[0134] [Chemical formula 2]
[0135] LiM 2 p Mn q P r O4
[0136] In Chemical Formula 1 and Chemical Formula 2,
[0137] M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B and Mo,
[0138] x, y, z, w, and v are respectively 1.0 ≤ x ≤ 1.30, 0.5 ≤ y < 1, 0 < z ≤ 0.3, 0 < w ≤ 0.3, and 0 ≤ v ≤ 0.1, where y + z + w + v = 1,
[0139] M 2 is Ni, Co, or Fe,
[0140] p is 0.05 ≤ p ≤ 1.0,
[0141] q is 1 - p or 2 - p, and
[0142] r is 0 or 1.
[0143] The lithium metal oxides represented by Chemical Formula 1 and Chemical Formula 2 are materials containing high contents of nickel (Ni) and manganese (Mn) respectively, and when used as the positive electrode active material, compared with the conventionally used positive electrode active materials such as lithium iron phosphate (LiFeO4), they have the advantages of being able to stably supply high-capacity and / or high-voltage power.
[0144] In this case, the lithium metal oxide represented by Chemical Formula 1 may include LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.9 Co 0.05 Mn 0.05 O2, LiNi 0.6 Co 0.2 Mn 0.1 Al 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.15 Al 0.05 O2, LiNi 0.7 Co 0.1 Mn 0.1 Al 0.1 O2, etc., and the lithium metal oxide represented by Chemical Formula 2 may include LiNi 0.7 Mn 1.3 O4, LiNi 0.5 Mn 1.5 O4, LiNi 0.3 Mn 1.7 O4, LiFePO4, LiFe 0.7 Mn 0.3 PO4, etc., which can be used alone or in combination.
[0145] In addition, based on a total of 100 parts by weight of the positive electrode active layer, the content of the positive electrode active material can be at least 85 parts by weight, and based on a total of 100 parts by weight of the positive electrode active layer, the content of the positive electrode active material can more specifically be at least 90 parts by weight, at least 93 parts by weight, or at least 95 parts by weight.
[0146] Furthermore, the positive electrode active layer may further include a conductive material, a binder, other additives, and the like in addition to the positive electrode active material.
[0147] In this case, the conductive material used to improve the electrical properties of the positive electrode can be any material conventionally used in the art, but more specifically can include at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, denka black, ketjen black, Super-P, channel black, furnace black, lamp black, summer black, graphene and carbon nanotubes.
[0148] In addition, based on a total of 100 parts by weight of each positive electrode active layer, the content of the conductive material can be 0.1-5 parts by weight, more specifically, based on a total of 100 parts by weight of the positive electrode active layer, the content of the conductive material can be 0.1 to 4 parts by weight; 2 to 4 parts by weight; 1.5 to 5 parts by weight; 1 to 3 parts by weight; 0.1 to 2 parts by weight; or 0.1 to 1 part by weight.
[0149] In addition, the binder is used to bind the positive active material, the positive electrode additive and the conductive material to each other, and can be used without restriction as long as it has this function. Specifically, the binder may include one or more resins selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVdF-co-HFP), polyvinylidene fluoride (PVdF), polyacrylonitrile, polymethyl methacrylate and copolymers thereof. In one example, the binder may include polyvinylidene fluoride.
[0150] In addition, the content of the binder may be 1 to 10 parts by weight, more specifically 2 to 8 parts by weight or 1 to 5 parts by weight, based on a total of 100 parts by weight of each positive electrode active layer.
[0151] The total thickness of the positive electrode active layer is not particularly limited, but may be 50 to 300 μm, more specifically 100 to 200 μm; 80 to 150 μm; 120 to 170 μm; 150 to 300 μm; 200 to 300 μm; or 150 to 190 μm.
[0152] In addition, as the positive electrode current collector, the positive electrode can use a positive electrode current collector having high conductivity and not causing chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, etc. can be used, and in the case of aluminum or stainless steel, those surface-treated with carbon, nickel, titanium, silver, etc. can also be used. In addition, considering the conductivity and total thickness of the positive electrode to be manufactured, the average thickness of the current collector can be appropriately 3 μm to 500 μm.
[0153] In addition, the separator placed between the positive electrode and the negative electrode of each unit cell is an insulating film with high ion permeability and mechanical strength, and it is not particularly limited as long as it is those conventionally used in the art, but may include one or more polymers, such as chemically resistant and hydrophobic polypropylene; polyethylene; polyethylene-propylene copolymer. The separator may be in the form of a porous polymer substrate, such as a sheet or non-woven fabric including the above polymers, and in some cases may be in the form of a composite separator in which organic or inorganic particles are coated on a porous polymer substrate by an organic binder. In addition, the separator may have an average pore size of 0.01 to 10 μm and an average thickness of 5 to 300 μm.
[0154] Meanwhile, the lithium secondary battery of the present invention may be shaped into but not specifically limited to include a stacked, zigzag or zigzag-stacked electrode assembly. As an example, the lithium secondary battery of the present invention may be a pouch-type secondary battery or a prismatic secondary battery.
[0155] Negative electrode manufacturing method
[0156] In addition, in an exemplary embodiment, the present invention provides a method for manufacturing a negative electrode for a lithium secondary battery, comprising:
[0157] applying a negative electrode slurry including a carbon-based active material onto a negative electrode current collector;
[0158] applying a magnetic field to the applied negative electrode slurry; and
[0159] The negative electrode slurry to which the magnetic field is applied is dried to form a negative electrode active layer.
[0160] wherein the negative electrode active layer is divided into: a central region including the central portion of the negative electrode active layer in the width direction; a landslide region located at the edge of the negative electrode active layer and having a thickness gradient; and an edge region located between the central region and the landslide region; and
[0161] The negative electrode active layer satisfies the following equations 1 and 2:
[0162] [Equation 1]
[0163] 2.7≤[OI 边缘 ] / [OI中心 ]≤4.8
[0164] [Equation 2]
[0165] 1.5≤[OI 滑坡 ] / [OI 中心 ]≤2.6
[0166] In Equation 1 and Equation 2,
[0167] OI 边缘 Indicates the arrangement value (OI) of the edge area,
[0168] OI 中心 Indicates the arrangement value (OI) of the center area,
[0169] OI 滑坡 represents the ranking index (OI) of the landslide area, and
[0170] The arrangement value (OI) represents the peak area (I 004 ) and the peak area representing the [1,1,0] crystal plane (I 110 ) ratio (I 004 / I 110 ).
[0171] The manufacturing method of the negative electrode of the present invention comprises: applying a negative electrode slurry containing a carbon-based negative electrode active material to a negative electrode current collector; and applying a magnetic field to the surface of the applied negative electrode slurry so that the carbon-based negative electrode active material in the negative electrode slurry is arranged at a predetermined angle relative to the surface of the negative electrode current collector. The negative electrode slurry in which the arrangement value of the carbon-based negative electrode active material has been reduced can then be dried to form a negative electrode active layer, thereby manufacturing the negative electrode.
[0172] Here, the step of applying the negative electrode slurry includes coating the surface of the moving negative electrode current collector by releasing the negative electrode slurry containing the carbon-based negative electrode active material, and can be applied in any manner conventionally applied in the art without limitation. Preferably, the step of applying the negative electrode slurry can utilize a die coating method. The die coating method can be performed by a slit die having a gasket for controlling the release conditions of the negative electrode slurry. In this case, by controlling the shape of the gasket, etc., the load amount, application thickness, etc. of the negative electrode slurry applied to the negative electrode current collector can be easily controlled.
[0173] In addition, the step of applying the negative electrode slurry may apply the negative electrode slurry to satisfy the following equation 3, thereby preventing lithium from being precipitated from the end of the negative electrode active layer during charge and discharge of the secondary battery:
[0174] [Equation 3]
[0175] R 滑坡<R 中心 <R 边缘
[0176] In equation 3,
[0177] R 滑坡 represents the average thickness of the landslide area,
[0178] R 边缘 represents the average thickness of the edge area,
[0179] R 中心 Indicates the average thickness of the central area.
[0180] Equation 3 shows the correlation between the average thickness of the negative electrode slurry applied to each region, so that the average thickness of the negative electrode slurry applied according to the present invention in the edge region 122 can be greater than the average thickness in the central region 121, and the average thickness in the landslide region 123 has a tendency to significantly decrease along the thickness gradient, as shown in Figure 3 As used herein, the “average thickness” may be measured using a confocal microscope, and the method may be different for each region. Specifically, for the center region and the edge region, it may mean measuring the thickness at more than three random points and calculating the average value from the measured values. In the case of a landslide region, it may mean measuring the thickness at a point where the length of the landslide region in the width direction is 1 / 2 of the length of the applied negative electrode slurry.
[0181] For example, the average thickness of the center regions 121 and 221 of the negative electrode slurry may be 180±3 μm, the average thickness of the edge regions 122 and 222 may be 210±3 μm, and the average thickness of the landslide regions 123 and 223 may be 120±3 μm.
[0182] By controlling the average thickness of each region of the negative electrode slurry applied to the negative electrode current collector as described above, even if the average thickness of each region becomes uniform after rolling, the present invention can easily control the loading amount of the carbon-based negative electrode active material in each region. Specifically, even if the average thickness of the central region 121 and 221 and the edge region 122 and 222 of the negative electrode active layer are the same or similar after rolling, the loading amount per unit area of the edge region 122 and 222 can be greater than the loading amount per unit area of the central region 121 and 221.
[0183] At the same time, the step of applying a magnetic field to the negative electrode slurry may be a step of orienting the crystal plane of the carbon-based negative electrode active material contained in the negative electrode slurry to have a predetermined angle relative to the negative electrode current collector. To this end, the step of applying a magnetic field may be performed by a magnetic member disposed on the upper and lower portions of the negative electrode current collector, which moves when the negative electrode slurry is applied to its surface.
[0184] In this case, the arrangement value (OI) of the carbon-based negative electrode active material contained in the negative electrode slurry can be controlled by the applied magnetic field strength or the exposure time to the magnetic field. Therefore, the step of applying the magnetic field can be performed under predetermined magnetic field strength and time conditions.
[0185] Specifically, the step of applying a magnetic field may include applying a magnetic field of 2,000G (Gauss) to 6,000G (Gauss). Specifically, the step of applying a magnetic field may include applying a magnetic field of 2,500G to 5,500G, 3,000G to 5,500G, 3,500G to 5,500G, 4,000G to 5,500G, 3,500G to 4,500G, or 4,500G to 5,000G.
[0186] Furthermore, the step of applying a magnetic field may be performed for 5 seconds to 60 seconds, more specifically 10 seconds to 60 seconds; 10 seconds to 30 seconds; 30 seconds to 60 seconds; 40 seconds to 50 seconds; 15 seconds to 35 seconds; or 10 seconds to 50 seconds.
[0187] In one example, the step of applying a magnetic field may include applying a magnetic field of 4,700±100 G to the negative electrode slurry for 12 seconds to 33 seconds.
[0188] In addition, as described above, the step of applying a magnetic field may be performed by introducing magnetic components at the upper and lower parts of the applied negative electrode slurry, but the size of the magnetic components may be adjusted to be larger than the size of the negative electrode slurry so that the magnetic field applied to the negative electrode slurry may be uniformly applied over the entire surface of the negative electrode slurry. For example, the length ratio of the magnetic component may be 105% to 200% based on the length in the width direction of the negative electrode slurry, and more specifically, the length ratio thereof may be 110% to 180%; 110% to 160%; 110% to 140%; 110% to 130%; 130% to 150%; or 105% to 120% based on the length in the width direction of the negative electrode slurry.
[0189] In the step of applying a magnetic field, the present invention can control the regional orientation of the carbon-based negative electrode active material contained in the negative electrode slurry to satisfy Equations 1 and 2 by controlling the magnetic field strength, application time and / or magnetic component size as described above.
[0190] In addition, the step of forming the negative electrode active layer may include: drying the negative electrode slurry; and rolling the dried negative electrode slurry.
[0191] In this case, the step of drying the negative electrode slurry may be performed in such a manner that the orientation of the carbon-based negative electrode active material included in the negative electrode active layer can be maintained, and is not particularly limited.
[0192] For example, the drying may be performed by applying heat energy to the negative electrode slurry using a hot air dryer, a vacuum oven, or the like to dry the negative electrode slurry.
[0193] Furthermore, the step of roll-pressing the dried negative electrode slurry is a step of increasing the density of the negative electrode active layer by applying pressure to the dried negative electrode slurry using a roll press, etc. In this case, the roll pressing may be performed under a temperature condition higher than room temperature.
[0194] More specifically, rolling may be performed at a temperature of 50 to 100° C., more specifically 60 to 100° C., 75 to 100° C., 85 to 100° C., 50 to 90° C., 60 to 80° C., or 65 to 90° C. More specifically, rolling may be performed at a rolling speed of 2 to 7 m / s, and more specifically at a rolling speed of 2 to 6.5 m / s, 2 to 6 m / s, 2 to 5.5 m / s, 2 to 5 m / s, 2 to 4.5 m / s, 2 to 4 m / s, 2.5 to 4 m / s, 2.5 to 3.5 m / s, 3.5 to 5 m / s, 5 to 7 m / s, 5.5 to 6.5 m / s, or 6 to 7 m / s. In addition, the rolling may be performed under a pressure condition of 50 MPa to 200 MPa, more specifically, 50 MPa to 150 MPa, 50 MPa to 100 MPa, 100 MPa to 200 MPa, 150 MPa to 200 MPa, or 80 MPa to 140 MPa.
[0195] By rolling the dried negative electrode slurry under the above temperature, speed and / or pressure conditions, the present invention can increase the energy density of the negative electrode while minimizing the variation in the arrangement value of the carbon-based negative electrode active material contained in the formed negative electrode active layer.
[0196] Hereinafter, the present invention will be described in more detail through Examples and Experimental Examples.
[0197] However, the following embodiments and experimental examples are examples of the present invention, and the present invention is not limited to the following embodiments and experimental examples.
[0198] Examples 1 to 2 and Comparative Examples 1 to 2: Preparation of negative electrode for lithium secondary battery
[0199] A negative electrode for a lithium secondary battery was prepared under the conditions shown in Table 1 below.
[0200] First, natural graphite (average particle size: 10±1 μm) and artificial graphite (average particle size: 8±1 μm) were prepared as carbon-based negative electrode active materials, respectively, and negative electrode slurry was prepared using the prepared carbon-based negative electrode active materials.
[0201] Specifically, mixed graphite as a negative electrode active material is prepared by mixing natural graphite and artificial graphite in a weight ratio of 1-3:7-9, and carbon black is used as a conductive material, carboxymethyl cellulose (CMC) and styrene butadiene rubber (SBR) are used as binders. Then, 95 parts by weight of the mixed graphite, 1 part by weight of carbon black, 1.5 parts by weight of carboxymethyl cellulose (CMC) and 2.5 parts by weight of styrene butadiene rubber (SBR) are mixed with water to obtain a solid content of 50%, thereby preparing a negative electrode slurry.
[0202] Once the negative electrode slurry was prepared, the negative electrode slurry was cast onto a copper sheet (thickness: 10 μm) using a die coater, which was transported in a roll-to-roll motion (transport speed: 5 m / min). The negative electrode slurry was cast so that the average thickness of the negative electrode slurry along the transport direction of the copper sheet was 190 μm, and the average thickness of each region of the negative electrode active layer before rolling was controlled by changing the shape of the gasket set in the die coater, as shown in Table 1.
[0203] At this time, the cross-sectional structure of the applied negative electrode slurry is as follows Figure 1 As shown, each negative electrode slurry is set to set the area at the center with a length ratio of 98.5% relative to the length in the width direction of the negative electrode slurry as the central area. Then, the areas with a total length ratio of 1.0% on both sides of the central area are set as edge areas (the length ratio of each edge area is 0.5%), and the areas with a length ratio of 0.5% outside the edge area are set as landslide areas (the length ratio of each landslide area is 0.25%).
[0204] When measuring the average thickness of each set area, the average thickness of the center area and edge area of the negative electrode slurry is obtained by measuring the confocal thickness of each area three times and calculating the average value. In addition, the average thickness of the landslide area of the negative electrode slurry is defined as the thickness at the point where the length of the landslide area in the width direction is 1 / 2 of the length of the negative electrode slurry.
[0205] After measuring the average thickness of each region of the negative electrode slurry, a permanent magnet with a length ratio of 110 to 120% relative to the length in the width direction of the negative electrode slurry is placed on the upper part of the applied negative electrode slurry and the lower part of the negative electrode current collector, a magnetic field of 4,700±100G is applied for 15 seconds, and the negative electrode slurry to which the magnetic field is applied is hot-air dried to form a negative electrode active layer. The formed negative electrode active layer is rolled at a pressure of 100MPa to 150MPa and a transmission rate of 3m / s at 50±1°C to prepare a negative electrode for a lithium secondary battery.
[0206] In addition, each manufactured negative electrode was subjected to X-ray diffraction spectroscopy analysis (XRD) to measure the spectrum of each region of the negative electrode active layer. The measurement conditions of X-ray diffraction (XRD) are as follows:
[0207] -Target: Cu (Kα-ray) graphite monochromator
[0208] - Slits: Divergence slit = 1 degree, Receiving slit = 0.1 mm, Scattering slit = 1 degree
[0209] - Measurement area: [1,1,0] plane: 76.5°<2θ<78.5° / [0,0,4] plane: 53.5°<2θ<56.0°.
[0210] From the spectrum measured under the above conditions, the corresponding areas of the peaks representing the [0,0,4] and [1,1,0] crystal planes were calculated, and the ratio of these areas (I 004 / I 110 ) to obtain the arrangement value (OI) of the mixed graphite in each region. The calculated values are shown in Table 1 below.
[0211] Table 1
[0212]
[0213] Comparative Examples 3 and 4: Preparation of negative electrodes for lithium secondary batteries
[0214] A negative electrode for a lithium secondary battery was prepared by the same method as Example 1, except that no magnetic field was applied after casting the negative electrode slurry and a permanent magnet having a length ratio of 95% to 100% relative to the width direction length of the negative electrode slurry was used to apply the magnetic field.
[0215] During the negative electrode manufacturing, (1) the average thickness of each region of the applied negative electrode slurry and (2) the arrangement value (OI) of the carbon-based negative electrode active material contained in each region after rolling were measured using the same method as in Example 1, and the measurement results are shown in Table 2 below.
[0216] Table 2
[0217]
[0218] Examples 3 to 4 and Comparative Examples 5 to 8: Preparation of lithium secondary batteries
[0219] Preparation of LiNi with a particle size of 5 μm 0.7 Co 0.1 Mn 0.1 Al 0.1 O2 was used as the positive electrode active material, which was mixed with a carbon-based conductive material and polyvinylidene fluoride as a binder in a weight ratio of 94:3:3 in N-methylpyrrolidone (NMP) to form a slurry, applied to an aluminum sheet, dried in a vacuum oven at 120°C, and roll-pressed to prepare the positive electrode.
[0220] The lithium secondary battery was assembled by disposing a separator including 18 μm polypropylene between the positive electrode obtained above and the negative electrodes prepared in Examples 1 to 2 and Comparative Examples 1 to 4, respectively, inserting it into a case, and then injecting the electrolyte composition.
[0221] Here, the type of negative electrode applied to each lithium secondary battery is shown in Table 3 below.
[0222] Table 3
[0223] Type of negative electrode applied Example 3 The negative electrode prepared in Example 1 Example 4 The negative electrode prepared in Example 2 Comparative Example 5 The negative electrode prepared in Comparative Example 1 Comparative Example 6 The negative electrode prepared in Comparative Example 2 Comparative Example 7 The negative electrode prepared in Comparative Example 3 Comparative Example 8 The negative electrode prepared in Comparative Example 4
[0224] Experimental example
[0225] In order to evaluate the performance of the negative electrode of the present invention, the following experiment was performed.
[0226] a) Evaluate whether lithium precipitation occurs
[0227] The lithium secondary batteries prepared in Examples 3 to 4 and Comparative Examples 5 to 8 were charged to SOC 80% by applying a current at a 1.5C rate, and the voltage change and dV / dQ according to SOC were measured. The presence of a voltage plateau in the measured voltage change or the bimodal shape of the graph of dV / dQ indicates that lithium is precipitated from the negative electrode surface. The results are shown in Table 4 below.
[0228] b) Evaluation of fast charging performance
[0229] For the lithium secondary batteries prepared in Examples 3 to 4 and Comparative Examples 5 to 8, the charge capacity and charge rate were measured after 300 repetitions of the charge-discharge process of 0.5C discharge and 1.7C charge rate charge. The ratio of the measured charge capacity to the initial charge capacity was calculated, and the results are shown in Table 4 below. If the ratio of the calculated charge capacity to the initial charge capacity is greater than 80%, it is marked as "○"; if it is less than or equal to 50%, it is marked as "X"; and if it is greater than 50% but less than 80%, it is marked as "△".
[0230] Table 4
[0231] Is lithium precipitated? Fast charging performance Example 4 X ○ Example 5 X ○ Comparative Example 5 ○ △ Comparative Example 6 X △ Comparative Example 7 X X Comparative Example 8 X X
[0232] As shown in Table 4, it can be seen that the negative electrode for lithium secondary batteries of the present invention not only inhibits lithium precipitation, but also has excellent fast charging performance. Specifically, the negative electrode prepared in the embodiment does not precipitate lithium from the negative electrode surface during charging and discharging, and maintains a charging capacity greater than 80% during fast charging.
[0233] This means that the negative electrode of the embodiment contains a high loading amount of carbon-based negative electrode active material in the edge area of the negative electrode active layer, which has a good effect of inhibiting lithium precipitation during battery charging; the arrangement value (OI) of each carbon-based negative electrode active material contained in the central area, edge area and landslide area of the negative electrode active layer has a configuration that satisfies Formula 1 and Formula 2, which improves the fast charging performance of the battery.
[0234] It can be seen from these results that the negative electrode for lithium secondary batteries of the present invention suppresses lithium precipitation at the end of the negative electrode active layer, and the secondary battery including the negative electrode has excellent rapid charging performance.
[0235] Although the above content has been described with reference to the preferred exemplary embodiments of the present invention, those skilled in the art or those having ordinary knowledge in the art will appreciate that various modifications and changes may be made to the present invention without departing from the concept and technical scope of the present invention described in the following claims.
[0236] Therefore, the technical scope of the present invention is not limited to the contents described in the detailed description of the specification, but should be defined by the patent claims.
[0237] [reference numerals]
[0238] 100 and 200: Negative electrode for lithium secondary battery of the present invention
[0239] 110 and 210: negative electrode current collector
[0240] 120 and 220: Negative active layer
[0241] 121 and 221: The central area of the negative electrode active layer
[0242] 122 and 222: Edge area of the negative electrode active layer
[0243] 123 and 223: Landslide area of the negative electrode active layer
[0244] CA: Carbon-based negative electrode active materials
[0245] ↑: Crystalline arrangement direction of carbon-based negative electrode active materials
Claims
1. A negative electrode for a lithium secondary battery, comprising: Anode current collector; as well as a negative electrode active layer, which is disposed on at least one side of the negative electrode current collector and comprises a carbon-based negative electrode active material, wherein the negative electrode active layer is divided into: a central region including the central portion of the negative electrode active layer in the width direction; a landslide region located at the edge of the negative electrode active layer and having a thickness gradient; and an edge region located between the central region and the landslide region; and The negative electrode active layer satisfies the following equations 1 and 2: [Equation 1] 2.7≤[OI 边缘 ] / [OI 中心 ]≤4.8 [Equation 2] 1.5≤[OI 滑坡 ] / [OI 中心 ]≤2.6 In Equation 1 and Equation 2, OI 边缘 Indicates the arrangement value (OI) of the edge area, OI 中心 Indicates the arrangement value (OI) of the center area, OI 滑坡 represents the ranking index (OI) of the landslide area, and The arrangement value (OI) represents the peak area (I) representing the (0,0,4) crystal plane in the XRD measurement result of the negative electrode active layer. 004 ) and the peak area representing the (1,1,0) crystal plane (I 110 ) ratio (I 004 / I 110 ).
2. The negative electrode for a lithium secondary battery according to claim 1, wherein the arrangement value OI of the central region of the negative electrode active layer is 中心 0.7 to 1.
5.
3. The negative electrode for a lithium secondary battery according to claim 1, wherein the ratio of the central region of the negative electrode active layer to the total length in the width direction of the negative electrode active layer is at least 90%, and The ratio of the landslide region of the negative electrode active layer to the total length in the width direction of the negative electrode active layer is 3% or less. 4 . The negative electrode for a lithium secondary battery according to claim 1 , wherein an average thickness of a central region of the negative electrode active layer is 100 μm to 300 μm. 5 . The negative electrode for a lithium secondary battery as claimed in claim 1 , wherein the carbon-based active material comprises at least one of natural graphite and artificial graphite.
6. A method for manufacturing a negative electrode for a lithium secondary battery, comprising: applying a negative electrode slurry including a carbon-based active material on a negative electrode current collector to form an applied negative electrode slurry; applying a magnetic field to the applied negative electrode slurry; and drying the negative electrode slurry to which the magnetic field is applied to form a negative electrode active layer, wherein the negative electrode active layer is divided into: a central region including the central portion of the negative electrode active layer in the width direction; a landslide region located at the edge of the negative electrode active layer and having a thickness gradient; and an edge region located between the central region and the landslide region; and The negative electrode active layer satisfies the following equations 1 and 2: [Equation 1] 2.7≤[OI 边缘 ] / [OI 中心 ]≤4.8 [Equation 2] 1.5≤[OI 滑坡 ] / [OI 中心 ]≤2.6 In Equation 1 and Equation 2, OI 边缘 Indicates the arrangement value (OI) of the edge area, OI 中心 Indicates the arrangement value (OI) of the center area, OI 滑坡 represents the ranking index (OI) of the landslide area, and The arrangement value (OI) represents the peak area (I) representing the (0,0,4) crystal plane in the XRD measurement result of the negative electrode active layer. 004 ) and the peak area representing the (1,1,0) crystal plane (I 110 ) ratio (I 004 / I 110 ).
7. The method for manufacturing a negative electrode for a lithium secondary battery according to claim 6, wherein in the step of applying the negative electrode slurry, the applied negative electrode slurry satisfies Equation 3: [Equation 3] R 滑坡 <R 中心 <R 边缘 In equation 3, R 滑坡 represents the average thickness of the landslide area, R 边缘 represents the average thickness of the edge region, R 中心 represents the average thickness of the central region. 8 . The method for manufacturing a negative electrode for a lithium secondary battery according to claim 6 , wherein the step of applying a magnetic field applies a magnetic field of 2000 G to 6000 G. 9 . The method for manufacturing a negative electrode for a lithium secondary battery according to claim 6 , wherein the step of applying a magnetic field is performed for 5 seconds to 60 seconds.
10. The method for manufacturing a negative electrode for a lithium secondary battery as claimed in claim 6, wherein the step of applying a magnetic field is performed by introducing magnetic components at the upper and lower parts of the applied negative electrode slurry, and the length of the magnetic components is 105% to 200% of the total length of the negative electrode slurry in the width direction.
11. The method for manufacturing a negative electrode for a lithium secondary battery according to claim 6, wherein the step of forming a negative electrode active layer comprises: Drying the negative electrode slurry; and The dried negative electrode slurry is roll-pressed.