Core-shell particle with piezoelectric effect, preparation method of core-shell particle and composite resin taking core-shell particle as antibacterial filler

By using core-shell structural particles formed by barium glass powder and barium titanate in dental composite resins, the problems of bacterial growth and insufficient antibacterial performance caused by the voids during use of composite resins are solved, and long-term antibacterial and mechanical properties are achieved. Improve, extend the restoration life and ensure biocompatibility.

CN118903198APending Publication Date: 2024-11-08BEIJING UNIV OF CHEM TECH +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410921768.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing dental composite resins have polymerization and shrinkage in use, which promote bacterial growth and secondary caries, and lack antibacterial properties. Release antibacterial agents can easily lead to bacterial resistance and biocompatibility problems, affecting mechanical properties.

Method used

Barium glass powder is used as the mechanical core, and barium titanate with piezoelectric properties is coated with piezoelectric properties to form core-shell structural particles. It is prepared by the sol-gel method to enhance the piezoelectric and mechanical properties of the composite resin.

Benefits of technology

The long-term antibacterial effect of composite resin is achieved, reducing the probability of secondary caries, extending the restoration life, while maintaining good biocompatibility and mechanical properties, avoiding the drug resistance of antibacterial agents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention relates to the technical field of dental repair materials, and particularly discloses a core-shell particle with a piezoelectric effect, a preparation method of the core-shell particle and composite resin with the core-shell particle as antibacterial filler. The core-shell particle is of a core-shell structure which takes barium glass powder as a core and coats barium titanate on the outer layer; the preparation method of the core-shell particle comprises the following steps: respectively preparing a solution I, a solution II and a solution III; dissolving barium acetate in hot acetic acid to obtain a solution I; adding tetrabutyl titanate into acetic acid, and then adding acetylacetone to obtain a solution II; dispersing barium glass powder in an acetic acid solution to obtain a solution III; adding the cooled solution I and solution III into the solution II, and stirring to obtain barium titanate precursor sol; and carrying out rotary evaporation and sintering on the barium titanate precursor sol, and naturally cooling to room temperature to obtain the core-shell particles. The core-shell particle and the composite resin provided by the invention have good antibacterial property and mechanical property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of dental restorative materials, and more specifically, to a core-shell particle with piezoelectric effect and a preparation method thereof, and a composite resin using the core-shell particle as an antibacterial filler. Background Art

[0002] Due to the problems of modern people's eating habits and living habits, the incidence of dental caries continues to increase, causing irreversible damage to teeth. Since there are abundant blood vessels and nerves inside the teeth, dental caries will cause severe pain in the later stage, so the treatment of dental caries is urgent. At present, the composite resin used in clinical treatment has the defect of polymerization shrinkage, which leads to gaps between it and the repair interface. The gaps are easy to breed bacteria. The acid produced by bacterial reproduction to form biofilm will cause secondary dental caries, which will lead to repair failure. In addition, the composite resins currently used on the market lack antibacterial properties, and the antibacterial agents used in the research are mostly release-type antibacterial agents. On the one hand, the release-type antibacterial agent has the problem of burst release, so it is easy for bacteria to develop drug resistance and also easy to cause biocompatibility problems; on the other hand, with the release of the release-type antibacterial agent, the mechanical properties of the composite resin will also be affected. Intrinsic antibacterial agents use their own antibacterial ability, such as the positive and negative charges they carry and the reactive oxygen species (ROS) they produce to damage the cell membrane to carry out antibacterial. This antibacterial method does not release particles or ions into the oral environment, so it has no significant adverse effect on the mechanical properties of the composite resin and usually has long-lasting antibacterial ability. Compared with release-type antibacterials, they do not develop antibiotic resistance. Among intrinsic antibacterials, polymers containing positively charged groups, such as quaternary ammonium compounds (QACs), have been widely explored. The antibacterial mechanism of QAC is mainly divided into two types: the first is through the positive charge it carries, the positively charged (N+) site of the QAC-based resin interacts with the microbial cell wall, destroying the integrity of the cell wall; the second is through its chemical structure, the long lipophilic alkyl chain in QAC can penetrate the bacterial cell membrane, causing cytoplasmic material leakage and autolysis, thereby causing bacterial cell death, but in the process of adding it to the resin, it will increase the hydrophilicity of the resin, facilitate bacterial adhesion and bring about cytotoxicity and other disadvantages, while piezoelectric materials achieve antibacterial effects by generating ROS (reactive oxygen species) and positive and negative charges on the surface. Compared with the existing antibacterial agents used in composite resins, piezoelectric materials can achieve a long-lasting antibacterial effect without causing bacteria to develop drug resistance. The biological environment in the oral cavity, such as the stress generated by chewing, can well meet the conditions for polarization and catalysis of piezoelectric materials. Therefore, the composite resin can be made piezoelectric by compounding piezoelectric materials, thereby achieving an antibacterial effect. In addition, the surface of the composite resin with piezoelectric materials added will have negative charges, which can absorb calcium ions in the environment, thereby promoting tooth remineralization.

[0003] However, piezoelectric nanoparticles, as individual entities, will be shielded by the reinforcing fillers after being added to the composite resin. A large volume fraction of fillers needs to be added to make them interconnected in order to exert the original antibacterial effect of the piezoelectric material. This not only makes the antibacterial effect less effective, but also affects the amount of reinforcing fillers added, thereby affecting other performance properties of the composite resin.

[0004] Therefore, it is necessary to provide a new piezoelectric material to overcome the above defects as much as possible. Summary of the invention

[0005] The present application provides a core-shell particle with piezoelectric effect and a preparation method thereof, and a composite resin using the core-shell particle as an antibacterial filler.

[0006] This application proposes a new type of reinforcing filler design - core-shell structure particles, which use conventional barium glass powder as the mechanical core and are coated with piezoelectric barium titanate to form a piezoelectric shell. When added to the composite resin, it simultaneously satisfies the addition amount of piezoelectric filler and reinforcing filler in the composite resin, forming a continuous piezoelectric phase and ensuring the good mechanical properties of the material. The sol-gel method is used to achieve uniform coating of barium titanate on the surface of barium glass powder, and particles with a core-shell structure are obtained. This structure not only allows the particles to be regarded as piezoelectric nanoparticles in the composite resin to achieve the purpose of antibacterial, but also satisfies the mechanical properties of the material due to its internal barium glass powder.

[0007] In the first aspect, the present application provides a core-shell particle, which adopts the following technical solution: A core-shell particle, which has a core-shell structure with barium glass powder as the core and barium titanate as the outer layer.

[0008] Optionally, the barium glass powder has a particle size of 500-1000 nm.

[0009] In the present application, the particle size of the barium glass powder cannot be greater than 1000 nm. When the particle size of the barium glass powder is greater than 1000 nm, it will affect the subsequent coating effect, resulting in uneven coating of barium titanate on the surface of the barium glass powder.

[0010] Optionally, the shell structure formed by the barium titanate has a thickness of 150-200 nm.

[0011] In a second aspect, the present application provides a method for preparing core-shell particles, using the following technical solution: A method for preparing core-shell particles, the preparation method specifically comprising the following steps: (1) preparing solution I, solution II and solution III respectively; dissolving barium acetate in acetic acid at 50-60° C. to prepare solution I; adding tetrabutyl titanate to acetic acid and then adding acetylacetone to prepare solution II; dispersing barium glass powder in acetic acid solution to prepare solution III; (2) adding the cooled solution I and solution III to solution II and stirring to obtain a barium titanate precursor sol; (3) The barium titanate precursor sol is rotary evaporated, sintered, and naturally cooled to room temperature to obtain core-shell particles.

[0012] In the present application, the acetic acid in solution I serves as a solvent for barium acetate, and the acetic acid in solution II serves to prevent premature hydrolysis of tetrabutyl titanate. The reason for selecting acetic acid as a solvent is that it will not undergo a hydrolysis reaction with tetrabutyl titanate.

[0013] Optionally, the molar ratio of the barium acetate to the tetrabutyl titanate is 1:1.

[0014] In the present application, the molar ratio of barium acetate to tetrabutyl titanate can only be 1:1. If it is any other ratio, the remaining raw materials cannot be removed in the subsequent process, which will result in poor product purity.

[0015] Optionally, the weight ratio of the barium glass powder added into the reaction system to the barium titanate generated in the reaction system is 1:3.

[0016] In the present application, the weight ratio of the barium glass powder to the prepared barium titanate is 1:3. If it is other ratios, the coating effect of the barium titanate will be affected, resulting in too little barium titanate coating or uneven coating.

[0017] Optionally, the temperature cannot be decreased during the dissolution of the barium acetate.

[0018] If the temperature drops during the dissolution of barium acetate, the barium acetate will precipitate and cause recrystallization, thus affecting the preparation effect.

[0019] Optionally, the preparation method is carried out under normal pressure.

[0020] Optionally, the stirring time is 18-21 hours.

[0021] Optionally, the sintering temperature is 1050-1100°C.

[0022] Optionally, the sintering time is 3-5h.

[0023] In a third aspect, the present application provides an application of core-shell particles as composite resin fillers for dental restorations.

[0024] In a fourth aspect, the present application provides a composite resin comprising the core-shell particles.

[0025] The composite resin disclosed in the present application is a long-lasting antibacterial dental repair composite resin, which includes a methacrylate monomer resin, a diluent, a photoinitiator, a co-initiator and an inorganic filler. The core-shell particles provided in the present application are used as the inorganic filler.

[0026] This application can at least achieve the following beneficial effects: (1) The core-shell particles provided in the present application are composed of a barium titanate shell layer with a piezoelectric effect and a barium glass powder core with a reinforcing effect. The barium titanate shell layer can utilize the stress generated by chewing teeth and the mechanical stimulation of an ultrasonic toothbrush to produce ROS to achieve an antibacterial effect, and the barium glass powder core can also provide mechanical support for the composite resin, ensuring the durability and stability of the composite resin for dental restoration.

[0027] (2) The composite resin provided in this application has both good antibacterial and mechanical properties, and can achieve long-term antibacterial effects in the oral cavity, greatly reducing the incidence of secondary caries and extending the life of composite resin restorations.

[0028] (3) In addition, the composite resin provided in this application has other advantages, such as good biocompatibility, suitable processing performance and clinical operability, etc. These characteristics will contribute to the wide application of the material in the field of oral medicine and provide patients with safer and more effective treatment options.

[0029] (4) This application implements technical transformation of conventional mechanical filler barium glass powder and successfully obtains a multifunctional core-shell filler, which, when added to composite resin, can not only give the composite resin an antibacterial effect, but also does not affect the basic properties of the composite resin. Compared with other antibacterial fillers currently used in dental restoration resins, especially release-type antibacterial fillers, it has a long-lasting antibacterial effect and will not cause bacteria in the oral cavity to develop drug resistance. The operation method is simple and only requires chewing or brushing with an ultrasonic toothbrush to trigger. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 Characterization results of the basic properties of BT@BAG core-shell particles ((a) BT@BAG TEM image; (b) BT@BAG XRD image; (c) BT@BAG DLS image; (d) BT@BAG EDS image).

[0031] Figure 2 Characterization results of the piezoelectric catalytic performance of different piezoelectric fillers ((a) BT NPs hydroxyl radical test graph; (b) BT NPs superoxyl radical test graph; (c) BT@BAG hydroxyl radical test graph; (d) BT@BAG superoxyl radical test graph).

[0032] Figure 3 The test results of Rhodamine B dye degradation by different piezoelectric fillers under ultrasonic conditions ((a) BT@BAG; (b) BT NPs; (c) percentage of remaining dye).

[0033] Figure 4The test results of different materials on bacterial growth (US- indicates no ultrasonic treatment; US+ indicates ultrasonic treatment).

[0034] Figure 5 is the antibacterial rate of different materials.

[0035] Figure 6 The test results of bacterial growth of composite resins with different materials added.

[0036] Figure 7 The antibacterial rate of composite resins with different materials added.

[0037] Figure 8 These are the SEM images corresponding to the antibacterial test of composite resins with different materials added.

[0038] Fig. 9 Characterization results of the piezoelectric catalytic performance of composite resins with different materials added ((a) 60 BT hydroxyl radical test graph; (b) 60 BT superoxyl radical test graph; (c) 60 BT@BAG hydroxyl radical test graph; (d) 60 BT@BAG superoxyl radical test graph).

[0039] Fig.10 These are the test results of the flexural strength and flexural modulus of composite resins with different materials added.

[0040] Fig.11 SEM images of the cross-section of the three-point bending test of the composite resin with different materials added ((a)(d) 60 BAG; (b)(e) 60 BT; (c)(f) 60 BT@BAG; the magnifications of (a)(b)(c) and (d)(e)(f) are different).

[0041] Fig.12 This is a biocompatibility test diagram of the composite resin with different materials added (wherein TCPS represents the control group without material, BAG represents the composite resin with 60wt% BAG added; BT NPs represents the composite resin with 60wt% BT NPs added; BT@BAG represents the composite resin with 60wt% BT@BAG added).

[0042] Fig.13 These are the fluorescence staining images of L929 cells cultured with composite resins containing different materials for 5 days (TCPS represents the control group without any material, BAG represents the composite resin with 60wt% BAG added; BT represents the composite resin with 60wt% BT NPs added; BT@BAG represents the composite resin with 60wt% BT@BAG added).

[0043] Fig.14SEM images of the surfaces of composite resins with different materials after mineralization in 1.5 times SBF liquid for three days ((a) 60 BAG; (b) 60 BT; (c) 60 BT@BAG). DETAILED DESCRIPTION

[0044] Before describing the embodiments of the present application in detail, it should be understood that the terms used herein are only used for the purpose of describing specific embodiments. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by ordinary technicians in the field to which the terms belong.

[0045] In the present application, BT@BAG is a core-shell particle of barium titanate encapsulating barium glass powder, BT is barium titanate, BAG is barium glass powder, and BT NPs is barium titanate nanoparticles.

[0046] The present application provides a core-shell particle. The core-shell particle is a core-shell structure of barium titanate coated with barium glass powder. That is, the core structure is barium glass powder, and the particle size can be 500-1000nm; the shell structure is barium titanate particles, and the shell structure thickness is 150-200nm.

[0047] The method for preparing the core-shell particles specifically comprises the following steps: (1) Prepare solution I, solution II and solution III respectively; Barium acetate is dissolved in acetic acid at 50-60°C to form solution I; tetrabutyl titanate is added to acetic acid and acetylacetone in sequence to form solution II; barium glass powder is dispersed in acetic acid solution to form solution III.

[0048] The molar ratio of barium acetate to tetrabutyl titanate is 1:1; and the weight ratio of barium glass powder to the prepared barium titanate is 1:3.

[0049] (2) Add the cooled solution I and solution III to solution II and stir to obtain a barium titanate precursor sol. The stirring time is 18-21 hours.

[0050] (3) The barium titanate precursor sol is rotary evaporated, sintered, and naturally cooled to room temperature to obtain core-shell particles.

[0051] The sintering temperature is 1050-1100°C and the sintering time is 3-5h.

[0052] The above operations were all carried out under normal pressure.

[0053] If the parameters in the above preparation method are changed, it will have an adverse effect on the coating degree of the core-shell particles, and the thickness of the barium titanate and the coating integrity will be affected.

[0054] In the present application, the barium glass powder is not a barium source, but a conventional mechanical filler in dental restoration composite resin. Barium acetate is a barium source, which reacts with tetrabutyl titanate to form barium titanate.

[0055] The present application provides the use of the core-shell particles as composite resin fillers for dental restorations and composite resins comprising the core-shell particles.

[0056] To make the purpose, technical solutions and advantages of this application clearer, the technical solutions in the embodiments of this application are described clearly and completely below. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of this application.

[0057] In the following examples, the barium glass powder was purchased from Schott, and the barium glass powder needed to be pre-treated to remove the silane coupling bonds on the surface. The pre-treatment process was sintering at 400-500° C. for 2-4 hours.

[0058] Barium acetate was purchased from Aladdin. Tetrabutyl titanate was purchased from MacLean. Acetic acid was purchased from Aladdin. Acetylacetone was purchased from MacLean. If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions were used. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0059] The present application is further described in detail below in conjunction with the embodiments and performance test results. Example

[0060] This embodiment provides a core-shell particle.

[0061] The method for preparing the core-shell particles specifically comprises the following steps: (1) Prepare solution I, solution II and solution III respectively; Weigh 1.8675 g (0.007 mol) of barium acetate and dissolve it in 5.6 mL of hot acetic acid as solution I; 2.45 mL (0.007 mol) of tetrabutyl titanate was added to 1.5 mL of acetic acid, and then 1.5 mL of acetylacetone was added and stirred to obtain a yellow clear solution, which was referred to as solution II. 0.5 g of barium glass powder was dispersed in acetic acid as solution III (the pretreatment process of the barium glass powder was sintering at 450° C. for 3 h).

[0062] (2) adding the cooled solution I and solution III to solution II and stirring for 18 hours to obtain a barium titanate precursor sol; (3) The barium titanate precursor sol is subjected to rotary evaporation to remove the solvent to obtain a viscous gel, which is then placed in a muffle furnace and sintered for 3 h at a heating rate of 10°C / min and a sintering temperature of 1050°C. The gel is then naturally cooled to room temperature to obtain core-shell particles.

[0063] The above operations were all carried out under normal pressure.

[0064] Performance test 1 The core-shell particles prepared in the above examples were subjected to the following tests.

[0065] 1. Core-shell particles-physical and chemical properties characterization (1) Characterization results of basic performance The results are as follows Figure 1 shown. Figure 1 In the figure, the characterization method of Figure (a) is transmission electron microscopy (TEM), and the function of transmission electron microscopy is to determine the structure of the particles; the characterization method of Figure (b) is X-ray diffraction (XRD), and the function of X-ray diffraction is to determine the crystal form of the particles; the characterization method of Figure (c) is dynamic light scattering (DLS) to measure the particle size, and the characterization method of Figure (d) is energy spectrum analysis (EDS) in scanning electron microscopy; the function of energy spectrum analysis is to observe the distribution of each element.

[0066] Depend on Figure 1 It can be seen from the different colors in Figure (a) that the light-colored part is the barium titanate shell layer and the dark-colored part is the barium glass powder. It can be seen that the particles prepared in this application are core-shell particles. It can be seen from the double peaks at 45° in Figure (b) that the crystal form of the particles prepared in this application is a tetragonal phase. It can be seen from Figure (c) that the average particle size of the core-shell particles is about 1000 nm. It can be seen from Figure (d) that the Ti element is distributed on the surface of the particles prepared in this application, indicating that the barium titanate is wrapped on the surface of the barium glass powder.

[0067] From the above characterization results, it can be seen that the surface morphology, crystal type and element distribution prove that the particles prepared in the present application are core-shell particles of tetragonal phase, barium titanate coated with barium glass powder.

[0068] (2) Characterization results of piezoelectric catalytic performance - quantitative testing The results are as follows Figure 2 shown. Figure 2 This is an electron spin resonance (ESR) test, which is a qualitative test for reactive oxygen species. Figures (a) and (c) are test graphs for hydroxyl radicals, and Figures (b) and (d) are test graphs for superoxide radicals. If there is a peak, it means that reactive oxygen species are generated; the control group water in Figures (a) and (c) also produces a little reactive oxygen species, which may be due to the spontaneous breakage of water molecules under ultrasound; no reactive oxygen species are generated in the control group dimethyl sulfoxide (DMSO) in Figures (b) and (d), because ultrasound does not produce reactive oxygen species in DMSO.

[0069] Depend on Figure 2 As shown in Figures (c) and (d), BT@BAG can generate obvious free radical signals in both water and DMSO after being stimulated by ultrasound. By comparing Figures (a) and (c), and Figures (b) and (d), it can be found that BT@BAG exhibits piezoelectric catalytic ability similar to that of BT NPs.

[0070] In Figures (a) and (c), when only ultrasound conditions were applied to the control water without BT NPs or BT@BAG, some hydroxyl radical signals were detected in the control water, which may be due to the spontaneous breakage of water molecules under ultrasound. After adding BT NPs or BT@BAG and applying ultrasound conditions, stronger hydroxyl radical signals were detected. This is because after mechanical stimulation, the surface of BT NPs or BT@BAG undergoes redox reaction with water to generate free radicals. At this time, the amount of free radicals generated is greater than the amount of free radicals generated by spontaneous breakage of water molecules. Therefore, after adding BTNPs or BT@BAG, a higher peak is shown in the spectrum.

[0071] Among them, in Figures (b) and (d), when only ultrasound conditions were applied to the control group DMSO without the addition of BT NPs or BT@BAG, no superoxide radical signal was detected in the control group DMSO. This is because there are no water molecules in DMSO and DMSO itself will not produce free radicals when subjected to ultrasound, so no free radical signal was detected.

[0072] (3) Dye degradation test-quantitative test In order to further quantitatively analyze the amount of free radicals generated by BT@BAG, dye degradation tests were subsequently carried out.

[0073] The results are as follows Figure 3 shown. Figure 3 In the figure, (a) shows the test results of BT@BAG, (b) shows the test results of BT NPs; (c) shows the percentage of remaining dye of the two particles.

[0074] Depend on Figure 3As shown in Figure (a), the surface of the Rhodamine B solution is obviously purple when no ultrasonic conditions are applied, and the highest absorption peak is shown at 550nm in the absorbance spectrum; when the ultrasonic conditions are applied, BT@BAG begins to produce free radicals to degrade the dye, and the free radicals react with Rhodamine B to degrade Rhodamine B. As the reaction time increases, the color of the Rhodamine B solution gradually becomes lighter, and the signal peak in the absorbance spectrum gradually weakens. After 30 minutes of ultrasonic treatment, the color of the Rhodamine B solution is significantly different from the color of the Rhodamine B solution without ultrasonic conditions, indicating that the amount of free radicals generated is proportional to the ultrasonic time.

[0075] Compared with the degradation effect of BT NPs in Figure (b), the residual rate of BT NPs for the degradation of Rhodamine B dye is 22%, while the residual rate of BT@BAG for the degradation of Rhodamine B dye is 14%, and the two show similar piezoelectric catalytic capabilities.

[0076] In summary, based on the above-mentioned characterization results of piezoelectric catalytic performance and the test results of dye degradation, it can be preliminarily proved that the BT@BAG core-shell particles prepared in this application can be regarded as piezoelectric fillers due to the piezoelectric shell layer on their surface and have piezoelectric catalytic ability.

[0077] 2. Characterization of antibacterial properties of core-shell particles In order to explore the antibacterial ability of core-shell particles, 1 mL of 1×10 4 CFU / mL of Staphylococcus aureus (S. aureus) and Streptococcus mutans (S. mutans) were co-cultured with core-shell particles, and the ultrasonic conditions were set to 4 min, 1 MHz, 1.5 W / cm 2 (Simulating daily toothbrushing time of 4 minutes and ultrasonic toothbrush power), after ultrasonication, 100 μL of bacterial solution was drawn from the well plate, and the residual bacteria were determined by the plate coating method.

[0078] Test results such as Figure 4 and Figure 5 shown. Figure 4 and Figure 5 In the table, US- indicates no ultrasonic treatment and no material added; US+ indicates ultrasonic treatment and no material added; BAG US+ indicates ultrasonic treatment and addition of BAG; BT NPs US+ indicates ultrasonic treatment and addition of BT NPs; BT@BAG US+ indicates ultrasonic treatment and addition of BT@BAG.

[0079] Depend on Figure 4 and Figure 5It can be seen that when ultrasonic treatment was not performed, the growth of S. aureus and S. mutans on the culture plate showed a uniform distribution; when ultrasonic treatment was performed for 4 minutes, the colony status of S. aureus and S. mutans did not change significantly, and they were still evenly distributed on the culture plate, which shows that under the conditions of ultrasonic treatment, the growth of bacteria was not negatively affected, and it can be inferred that ultrasonic treatment itself has no inhibitory effect on bacteria.

[0080] In addition, when BAG was added to the ultrasonic treatment environment, S. aureus and S. mutans were still able to maintain normal growth, indicating that even under ultrasonic treatment, BAG did not produce free radicals sufficient to kill bacteria. Therefore, the possibility that BAG was toxic to bacteria under ultrasound can be ruled out.

[0081] However, when BT@BAG was introduced into the ultrasonic treatment environment, the situation changed significantly. BT@BAG produced free radicals under the action of ultrasound, which reacted with the bacterial cell membrane, resulting in damage to the structural integrity of the cell membrane and ultimately causing the death of the bacteria. BT@BAG also showed antibacterial ability similar to that of BT NPs, with the antibacterial performance reaching 100%.

[0082] From the above results, it can be seen that the BT@BAG prepared in the present application shows similar results to BT NPs in terms of piezoelectric catalytic performance and antibacterial performance. Therefore, it can be confirmed that the BT@BAG prepared in the present application can replace BT NPs as a piezoelectric filler and be used in composite resins.

[0083] At the same time, in order to determine whether the BT@BAG prepared in this application can continue to exert good antibacterial properties in the composite resin and whether it can serve as a reinforcing filler to maintain the mechanical properties of the composite resin, this application further adds BT@BAG to the composite resin and measures the various properties of the composite resin.

[0084] Example 2 This embodiment provides a composite resin. The composite resin includes the core-shell particles provided in embodiment 1.

[0085] The preparation method of the composite resin specifically comprises the following steps: Bis-GMA and TEGDMA were mixed at a mass ratio of 6:4, and a 2wt% photoinitiator system (1.0wt% CQ+1.0wt% EDB) of the pure resin system was added, and 60wt% of the core-shell particles were added at the same time. The specific mixing method is as follows: first, an appropriate amount of BT@BAG was added to anhydrous ethanol for dispersion, and then the diluted resin TEGDMA and Bis-GMA were added, and mixed evenly in a mortar, and a certain amount of initiator and co-initiator were added and mixed evenly, and the mixture was passed through three rollers, and the ethanol was completely evaporated during the operation.

[0086] Performance test 2 The composite resin prepared in the above example was subjected to the following tests: The amount of core-shell particles added to the composite resin was 60 wt%.

[0087] 1. Antibacterial performance test of composite resin with core-shell particles The proportion of the composite resin components is: Bis-GMA 20wt%; TEGDMA 20wt%; inorganic filler (BAG, BT NPs, BT@BAG) 60wt%. Among them, the photoinitiator accounts for 2wt% of the resin system. The composite resin is co-cultured with bacteria, and ultrasonic conditions are applied to it (ultrasonic conditions are as shown above), and the bacterial solution is aspirated for plate drawing to observe the antibacterial effect.

[0088] (1) The results are as follows Figure 6 and Figure 7 shown. Figure 6 and Figure 7 In the table, US- means no ultrasonic treatment and no material added; US+ means ultrasonic treatment and no material added; 60 BAG US+ means ultrasonic treatment and addition of 60 wt% BAG; 60 BTUS+ means ultrasonic treatment and addition of 60 wt% BT NPs; 60 BT@BAG US+ means ultrasonic treatment and addition of 60 wt% BT@BAG.

[0089] Depend on Figure 6 and Figure 7It can be seen that there are a large number of colonies in the 60 BAG test results, which show the same results as the test results without ultrasonic treatment and only with ultrasonic treatment, indicating that the simple addition of BAG and the application of ultrasonic conditions have no effect on the growth of bacteria. When 60wt% BT NPs are added to the composite resin, a continuous piezoelectric phase is formed in the composite resin. After being stimulated by ultrasound, free radicals are generated to react with bacteria to kill bacteria. Therefore, there is no colony growth in the culture plate of 60 BT, achieving a good antibacterial effect. At the same time, there is no colony in the culture plate of 60 BT@BAG, indicating that the addition of BT@BAG achieves the same antibacterial results as BT NPs, confirming that BT@BAG can be used as a piezoelectric filler to replace BTNPs and added to the composite resin to achieve the purpose of antibacterial composite resin.

[0090] (2) At the same time, the present application also conducted SEM testing on the results of the above antibacterial test.

[0091] The results are as follows Figure 8 shown.

[0092] like Figure 8 As shown in the figure, the bacterial cell membranes of 60 BAG, no ultrasonic treatment, and only ultrasonic treatment without adding materials are intact, and the bacterial morphology is smooth and round, indicating that the bacteria are not attacked by free radicals. In contrast, the bacterial cell membranes of 60 BT and 60 BT@BAG are ruptured, and the bacterial morphology shrinks and collapses. These morphological changes are evidence of the attack of free radicals on the bacteria, indicating that sufficient free radicals are generated in the composite resins with 60 BT and 60 BT@BAG, causing the bacterial cell membrane to rupture and the cytoplasm to flow out, thus causing death. The results of the SEM image are consistent with those of the plate coating method.

[0093] (3) Characterization results of piezoelectric catalytic performance The results are as follows Fig. 9 shown. Fig. 9 This is an electron spin resonance (ESR) test, which is a qualitative test of active oxygen. Figures (a) and (c) are test graphs of hydroxyl radicals, and Figures (b) and (d) are test graphs of superoxide radicals.

[0094] like Fig. 9As shown, the 60 BT composite resin constitutes a piezoelectric continuous phase, so hydroxyl radicals and superoxide radicals are generated after applying ultrasound, and the signals of the two radicals are shown in the spectrum; for the 60 BT@BAG composite resin, since the barium glass powder added to the composite resin has barium titanate on its surface, it has a similar effect to barium titanate. After applying ultrasound, the spectrum also shows the signals of hydroxyl radicals and superoxide radicals, achieving a piezoelectric catalytic effect similar to that of adding pure barium titanate, indicating that the composite resin with the core-shell particles prepared in this application has good free radical generation ability.

[0095] (II) Mechanical properties test of composite resin In summary, when BT@BAG is added to the composite resin as a piezoelectric filler, BT@BAG exhibits piezoelectric catalytic ability and antibacterial ability similar to that of pure barium titanate. In order to further explore whether BT@BAG has a mechanical enhancement effect, its mechanical properties were tested.

[0096] (1) The flexural strength and flexural modulus of composite resins with different materials added were tested.

[0097] The results are as follows Fig.10 shown.

[0098] Depend on Fig.10 It can be seen that in terms of flexural strength, the flexural strength of the composite resin with 60wt% BAG added reached 118MPa, indicating that BAG, as a reinforcing filler, can provide mechanical properties enhancement for the composite resin. In contrast, the flexural strength of the composite resin with 60wt% BT NPs added was severely reduced to only 58MPa, which was 51% lower than the flexural strength of the composite resin with 60wt% BAG added. This shows that the addition of barium titanate cannot provide active help to the mechanical properties of the composite resin. Although the flexural strength of the composite resin with 60wt% BT@BAG added was 15% lower than that of the barium glass powder, it can still reach 100MPa, which meets the national standard for the flexural strength of composite resins (80MPa).

[0099] In terms of flexural modulus, the flexural modulus of the composite resin with 60wt% BAG can reach 4.8GPa, indicating that BAG, as a reinforcing filler, can provide mechanical properties enhancement for the composite resin. In contrast, the flexural modulus of the composite resin with 60wt% BTNPs also dropped severely, only 2.2GPa, which was 54% lower than that of the composite resin with 60wt% BAG. This also shows that the addition of barium titanate cannot provide active help to the mechanical properties of the composite resin. Although the flexural modulus of the composite resin with 60wt% BT@BAG dropped by 20% compared with barium glass powder, it can still reach 3.8GPa, but still shows good modulus performance.

[0100] (2) After the three-point bending test of the composite resin with different materials, the resin specimens were collected and their cross-sections were observed. The cross-section SEM images are shown in Figure 2. Fig.11 shown.

[0101] from Fig.11 It can be seen that when 60wt% BAG is added, it is evenly dispersed in the resin matrix without agglomerates, and each particle is wrapped by the resin. This uniform dispersion is beneficial to improving the mechanical properties of the composite resin. When 60wt% BT NPs is added, on the one hand, since there is no silane coupling bond grafted on its surface, it has poor encapsulation in the composite resin and many particles are exposed. On the other hand, since it has no effect on enhancing the mechanical properties, the mechanical properties of the composite resin are very poor. When 60wt% BT@BAG is added, it is evenly dispersed in the composite resin, and no bubbles or holes are observed. At the same time, due to the presence of the BAG core, it can help the mechanical properties of the composite resin, thereby maintaining good mechanical properties. Although the filler is not silane coupled, it can still be evenly dispersed in the resin matrix by observing the cross section, and there is no splitting at the interface, and no agglomeration or bubbles appear.

[0102] 3. Biocompatibility test of composite resin (1) In order to confirm the biocompatibility of composite resins in oral applications, the proliferation of L929 cells in the extracts of composite resins with different materials added was tested using the CCK-8 method.

[0103] The results are as follows Fig.12 shown. Fig.12 In the figure, TCPS represents the control group without adding materials, BAG represents the composite resin with 60wt% BAG added; BT NPs represents the composite resin with 60wt% BT NPs added; BT@BAG represents the composite resin with 60wt% BT@BAG added.

[0104] Depend on Fig.12 The test results show that the absorbance shows an increasing trend at 1, 3, and 5 days, indicating that the cells can grow stably under these conditions, and the growth rate of each group is similar to that of the blank group, indicating that the introduction of 60wt% piezoelectric filler will not affect the basic properties of the composite resin. All groups of resins show good biocompatibility.

[0105] From the above results, it can be seen that the CCK-8 test results show that the extracts of the above-mentioned various composite resins have no effect on cell proliferation. (2) To further evaluate the cell growth and biocompatibility of the composite resin, the composite resin and L929 cells were co-cultured for five days, and cell survival was characterized by fluorescent staining.

[0106] The results are as follows Fig.13 shown. Fig.13 In the figure, TCPS represents the control group without adding materials, BAG represents the composite resin with 60wt% BAG added; BT represents the composite resin with 60wt% BT NPs added; BT@BAG represents the composite resin with 60wt% BT@BAG added.

[0107] Depend on Fig.13 It can be seen that L929 cells can proliferate normally on the above-mentioned composite resins. Since the cells were planted in the composite resin by dripping, the cells in the control group grew densely and had a higher cell density than those in the control group. In addition, there was a certain height difference in the composite resin, and the cells grew for a long time, resulting in stratification. Some cells were brighter and some were darker, which was not a problem of cell viability.

[0108] Based on the above, it can be seen that the addition of various fillers will not have a negative impact on the biocompatibility of composite resins.

[0109] 4. Composite resin remineralization performance test To test the remineralization properties of composite resins incorporating different materials.

[0110] The test method is as follows: Preparation of mineralization solution: Prepare 1.5 times simulated body fluid (1.5SBF), specifically, add 0.417gCaCl2·2H2O to 20mL deionized water and dissolve it for use; measure 800mL deionized water, heat it to 37°C, and add 11.994g NaCl, 0.525g NaHCO3, 0.336g KCl, 0.342g K2HPO4·3H2O, 0.458g MgCl2·6H2O, and 0.107g Na2SO4 in sequence. After complete dissolution, add 7.004g Tris, and then use Tris-HCl to adjust the pH value of the entire solution system to between 7-8, add the above-prepared CaCl2 solution, adjust the pH value to 7.4, and stir evenly to obtain 1.5 SBF.

[0111] Composite resin remineralization experiment: The composite resin disc was polished with 200 mesh, 400 mesh, and 2000 mesh sandpaper in sequence for later use. 10 mL of 1.5SBF was added to a 50 mL centrifuge tube, and the polished composite resin disc was placed in it. The centrifuge tube was moved to a 37°C constant temperature water bath stirring box. The mineralization liquid was sucked out and new mineralization liquid was added every day. The composite resin sheet was taken out after three days of mineralization. After washing and drying, the surface morphology of the resin was characterized using SEM.

[0112] The results are as follows Fig.14 As shown. Fig.14 The results showed that after three days of mineralization, the composite resin surface with BAG added failed to form an obvious mineralized layer, and the resin was still exposed. In contrast, the composite resin surface with BT NPs and BT@BAG particles had formed a complete mineralized layer. Due to its high surface potential, the negative charge on the resin surface served as a nucleation site to adsorb Ca 2+ On the resin surface, the remineralization process of the composite resin is promoted.

[0113] Energy dispersive X-ray spectroscopy (EDS) analysis showed that the mineralized layer on the resin surface contained calcium and phosphorus elements, and the calcium-phosphorus ratio was 1.68-1.7. It can be inferred that hydroxyapatite is formed on the surface. Hydroxyapatite is the main inorganic component of teeth. Its formation on the resin surface proves that the composite resin can simulate the remineralization process.

[0114] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A core-shell particle with piezoelectric effect, characterized in that: The core-shell particles are of a core-shell structure with barium glass powder as the core and barium titanate as the outer layer.

2. The core-shell particle with piezoelectric effect according to claim 1, characterized in that: The particle size of the barium glass powder is 500-1000nm The core-shell particle with piezoelectric effect according to claim 1, characterized in that the shell structure composed of the barium titanate has a thickness of 150-200 nm.

3. A method for preparing the core-shell particles according to any one of claims 1 to 3, characterized in that: The preparation method specifically comprises the following steps: (1) preparing solution I, solution II and solution III respectively; dissolving barium acetate in acetic acid at 50-60° C. to prepare solution I; adding tetrabutyl titanate to acetic acid and then adding acetylacetone to prepare solution II; dispersing barium glass powder in acetic acid solution to prepare solution III; (2) adding the cooled solution I and solution III to solution II and stirring to obtain a barium titanate precursor sol; (3) The barium titanate precursor sol is rotary evaporated, sintered, and naturally cooled to room temperature to obtain core-shell particles.

4. The preparation method according to claim 4, characterized in that: The molar ratio of the barium acetate to the tetrabutyl titanate is 1:1; Optionally, the weight ratio of the barium glass powder added into the reaction system to the barium titanate generated in the reaction system is 1:

3.

5. The preparation method according to claim 4, characterized in that: The temperature cannot drop during the dissolution of the barium acetate; Optionally, the preparation method is carried out under normal pressure.

6. The preparation method according to claim 4, characterized in that: The stirring time is 18-21h; Optionally, the sintering temperature is 1050-1100°C; Optionally, the sintering time is 3-5h.

7. Use of the core-shell particles according to any one of claims 1 to 3 as composite resin fillers for dental restoration.

8. A composite resin, characterized in that: The composite resin comprises the core-shell particles according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Preparation method of core-shell type highly dielectric filler from barium titanate-doped multi-walled carbon nanotubes

    CN104609465A

  • Preparation method and application of titanium dioxide coated barium titanate core-shell structure nanowire ceramic

    CN114210316A

  • Premixed injectable antibacterial piezoelectric active self-curing biological ceramic as well as preparation method and application thereof

    CN117982537A

  • Dental compositions containing core-shell polymers with low modulus cores

    US20050124762A1

  • Dental filler and compositions

    US20140275326A1