Iron-manganese modified biochar for removing low-concentration phosphorus-containing wastewater as well as preparation method and application of iron-manganese modified biochar

By precipitating iron-manganese oxides on the surface of biochar and combining their oxidation properties, the problem of low adsorption capacity of existing biochar phosphorus removal adsorbents is solved, efficient removal of low concentration of phosphorus and organic degradation, and the efficiency of wastewater treatment is improved and economical, reducing environmental pollution.

CN118904287APending Publication Date: 2024-11-08TIANJIN CHENGJIAN UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411027817.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing biochar phosphorus removal adsorbents have problems with low adsorption capacity and easy dissolution, making it difficult to effectively remove low-concentration phosphorus-containing wastewater, and are costly, which affects the efficiency of wastewater treatment and environmental protection.

Method used

The preparation method of iron-manganese modified biochar is adopted, and the iron-manganese oxide precipitation is loaded on the surface of biochar, combining the high adsorption capacity of biochar and the oxidation performance of iron-manganese oxides, and the efficient removal of phosphorus and degradation of organic matter. Improve wastewater treatment efficiency and economical.

Benefits of technology

It realizes efficient removal of low-concentration phosphorus, reduces wastewater treatment costs and environmental pollution, improves adsorption capacity and catalytic degradation performance, and is simple to operate, low cost, and has stability and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904287A_ABST
    Figure CN118904287A_ABST
Patent Text Reader

Abstract

The invention provides iron and manganese modified biochar for removing low-concentration phosphorus-containing wastewater and a preparation method and application of the iron and manganese modified biochar, and belongs to the field of low-concentration phosphorus-containing wastewater treatment and the field of water ecological remediation. S2, preparing carbonized powder; s3, treating the carbonized powder: grinding the carbonized powder prepared in the S2, and sieving with a 100-mesh sieve; s4, preparing reaction solutions: preparing a manganese solution a and an iron solution b respectively; s5, mixing the reaction solution and carbonized powder: dropwise adding the solution a into the solution b, adding the carbonized powder sieved in the S3 into the mixed solution, quickly stirring, and standing for aging; s6, high-temperature drying: putting carbonized powder in S5 into a high-temperature drying oven for drying; the preparation method is simple, operation is easy and convenient, the preparation cost is low, no harm is caused to the human body, no secondary pollution is caused, the adsorption performance on total phosphorus is high, and the modified biochar has high practical application potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of treatment of low-concentration phosphorus-containing wastewater and water ecological restoration, and particularly relates to an iron-manganese modified biochar for removing low-concentration phosphorus-containing wastewater, and a preparation method and application thereof. Background Art

[0002] Wastewater treatment is one of the environmental issues that cannot be ignored in modern society. With the acceleration of industrialization and the continuous advancement of urbanization, wastewater contains a large amount of organic and inorganic pollutants, among which phosphorus is a common pollutant. High concentrations of phosphorus can lead to eutrophication of water bodies, cause excessive growth of algae, destroy the balance of water ecology, and even pose potential risks to human health.

[0003] Biochar is a porous carbon-containing material prepared by pyrolysis and carbonization of biomass raw materials. Its morphological structure is relatively stable and rich in carbon. Its original purpose is to be used for carbon fixation. As one of a series of "black carbon" materials, biochar specifically refers to the carbon fixation medium derived from sustainable biomass raw materials. Biomass raw materials that can be used to prepare biochar include a variety of crop wastes and by-products, such as rice straw, wheat straw, corn cobs, vegetable leaves, etc., in addition to waste wood, feces and municipal sludge. Thermochemical technologies for converting biomass raw materials into biomass energy or biochar are mainly divided into three categories: pyrolysis (including fast and slow pyrolysis), gasification, and carbonization under other specific conditions.

[0004] In recent years, biochar has attracted widespread attention as a new type of material in the field of wastewater treatment. Biochar has porosity, high specific surface area and good adsorption properties, which can effectively remove organic and inorganic pollutants in wastewater. Especially in phosphorus removal, biochar has good adsorption capacity and can quickly fix phosphorus ions in wastewater on its surface. Liang MN, Yan LL, Wang DQ et al. found in the article Novel iron manganese oxide modified mulberry biochar for the adsorption of phosphorus in aqueous solution (Desalination and Water Treatment, 2020, 189: 357-366) that biochar prepared with iron manganese oxide has excellent adsorption properties for phosphorus in solution.

[0005] However, there are some problems with the biochar phosphorus removal adsorbents currently on the market, such as low adsorption capacity and easy solubility. Therefore, it is urgent to develop new phosphorus removal adsorbents with high adsorption capacity, strong stability and renewability, in order to achieve low-carbon, environmentally friendly and sustainable sewage treatment technology, improve the efficiency of sewage treatment and save operating costs. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention proposes a method for preparing iron-manganese modified biochar for treating low-concentration phosphorus-containing wastewater. A new type of wastewater treatment material is developed by combining biochar and iron-manganese oxides, which not only utilizes the high adsorption capacity of biochar, but also gives full play to the oxidation and phosphorus removal capabilities of iron-manganese oxides.

[0007] The present invention adopts the following technical solutions to solve the above problems:

[0008] A method for preparing iron-manganese modified biochar for removing low-concentration phosphorus-containing wastewater, the method comprising the following steps:

[0009] S1: preparing corncob powder: crushing corncobs to obtain corncob powder;

[0010] S2: preparing carbonized powder: pyrolyzing corn cob powder under anoxic conditions by introducing N2, cooling to room temperature after pyrolysis, and grinding to obtain carbonized powder;

[0011] S3: Processing the carbonized powder: Grinding the carbonized powder prepared in S2 and passing it through a 100-mesh sieve;

[0012] S4: Prepare reaction solution: prepare manganese solution and iron solution separately, dissolve NaOH and KMnO4 crystals in deionized water to prepare manganese solution, called solution a, dissolve FeSO4 and FeCl3 crystals in deionized water to prepare iron solution, called solution b;

[0013] S5: Mixing the reaction solution and the carbonized powder: taking a certain amount of solution b and placing it in a 500 mL beaker, slowly dropping a certain amount of solution a into solution b under rapid stirring, then adding the sieved carbonized powder in S3 into the mixed solution, and rapidly stirring and then standing for aging to allow the carbonized powder to fully contact with the mixed solution;

[0014] S6: high temperature drying: the carbonized powder in S6 that is in full contact with the mixed solution is filtered out using qualitative filter paper, and then placed in a high temperature oven for drying;

[0015] S7: preparing modified biochar: taking out the carbonized powder after high temperature drying in S7, grinding it and passing it through a 100-mesh sieve to obtain iron-manganese modified biochar.

[0016] Furthermore, in S2, the heating rate of the corn cob powder for pyrolysis is 10°C / min, the temperature is raised to 500°C, and the pyrolysis is continued at this temperature for 120 minutes.

[0017] Furthermore, in S4, the FeSO4 crystals are FeSO4·7H2O, and the FeCl3 crystals are FeCl3·6H2O.

[0018] Furthermore, in S4, the molar ratio of KMnO4, FeSO4·7H2O, FeCl3·6H2O and NaOH is 1:3:3:14.

[0019] Furthermore, in S5, the rapid stirring reaction time is 60 minutes, and the static aging time is 8 hours.

[0020] Furthermore, in S6, the drying temperature is 105° C. and the time is 4 hours.

[0021] The present invention also provides an iron-manganese modified biochar obtained by the above preparation method.

[0022] The present invention also provides an application of iron-manganese modified biochar in sewage treatment technology.

[0023] Furthermore, the sewage is low-concentration phosphorus-containing sewage.

[0024] Advantages of the present invention:

[0025] This patent aims to provide a new type of biochar phosphorus removal adsorbent. This patent will combine biochar and iron-manganese oxides to develop a new type of wastewater treatment material, which not only utilizes the high adsorption capacity of biochar, but also exerts the oxidation and phosphorus removal capabilities of iron-manganese oxides; by organically combining the two, it can achieve efficient removal of phosphorus in wastewater and degradation of organic matter, improve the efficiency and economy of wastewater treatment, and promote environmental protection and sustainable development; this method is simple to operate, low cost, and will not damage the properties and structure of the biochar itself.

[0026] 1. By optimizing the preparation process of biochar and improving its surface properties, the phosphorus ions in wastewater can be efficiently removed and recycled, thus reducing the cost of wastewater treatment and environmental pollution;

[0027] 2. The raw materials of this patent come from solid waste, which helps to achieve resource recycling and reuse. By separating and reusing recyclable materials, the demand for waste landfill and incineration can be reduced, reducing the occupation of landfills and pollution to the environment;

[0028] 3. After iron and manganese oxides are precipitated and loaded on the surface of biochar, they can provide more active sites and adsorption sites, increase the contact area between biochar and target pollutants, and improve the adsorption capacity of biochar;

[0029] 4. Iron-manganese oxides have catalytic and oxidative properties, which can improve the adsorption performance and catalytic degradation ability of biochar. There is a synergistic effect between the precipitation of iron-manganese oxides and biochar. The precipitated iron-manganese oxides can enhance the adsorption capacity of biochar and reduce the wrapping effect of biochar, making it easier to contact and adsorb the target substance, thereby enhancing its phosphorus removal effect.

[0030] 5. When the biochar prepared by this method is used for phosphorus removal, the iron ions in the iron-manganese oxide can form an iron-phosphate complex with orthophosphate, thereby achieving the removal of orthophosphate; in addition, the iron-manganese oxide can also convert orthophosphate into an insoluble precipitate through oxidation, further reducing the concentration of orthophosphate.

[0031] 6. The present invention is simple to operate, low in cost, and harmless to the human body during the preparation process. It has high stability and can exist in water for a long time and ensure the phosphorus removal effect.

[0032] 7. Compared with the existing iron-manganese modified biochar invention, the advantage of the present invention is that the iron-manganese modified biochar prepared under the same substance ratio and the iron-manganese modified biochar in the comparative document have the same adsorption time. The maximum adsorption capacity of low-concentration phosphate of the present invention can reach 8.051 mg / g, while the maximum adsorption capacity of the iron-manganese modified biochar can only reach 3.369 mg / g, indicating that the adsorption effect of the iron-manganese modified biochar on low-concentration phosphate is much better than that of the iron-manganese modified biochar prepared under the same substance ratio. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The exemplary embodiments of the present invention are described in more detail with reference to the accompanying drawings, so that the above-mentioned objects, features and advantages of the present invention become more apparent. In the exemplary embodiments of the present invention, the same reference numerals generally represent the same components.

[0034] Figure 1 is a flow chart of the preparation method of the present invention;

[0035] Figure 2 This is the scanning electron microscope image of the iron-manganese modified biochar;

[0036] Figure 3 (a) is the Raman spectrum characterization of the unmodified biochar of Example 2. D / I G The analysis curve of

[0037] Figure 3 (b) is the Raman spectroscopy characterization of the iron-manganese modified biochar of Example 2. D / I G The analysis curve of

[0038] Figure 4 The adsorption kinetic curve of the iron-manganese modified biochar of Example 3, including pseudo-first-order kinetics and pseudo-second-order kinetics;

[0039] Figure 5 (a) is the adsorption / desorption curve of the specific surface area of ​​the unmodified biochar of Example 4;

[0040] Figure 5 (b) is the adsorption / desorption curve of the specific surface area characterization of the iron-manganese modified biochar of Example 4;

[0041] Figure 6 The adsorption amount of different types of biochar changes over time in Example 6. DETAILED DESCRIPTION

[0042] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. The words "include", "including", "have", "contain" and the like used herein are open terms, which refer to including but not limited to the listed contents.

[0043] It should be noted that the professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, the various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.

[0044] The reason why the present invention adopts the method of loading iron and manganese oxide on the surface of biochar for modification is that, first, iron and manganese modification can make full use of the synergistic effect of iron and manganese, and form iron and manganese oxide loading on the surface of biochar through coprecipitation reaction, so as to comprehensively exert the adsorption and catalytic properties of the two metal oxides, enhance the synergistic effect, and improve the modification effect. Secondly, iron and manganese both play an important role in environmental governance, and the use of iron or manganese alone for modification may not meet the needs of removing low-concentration phosphorus. Iron and manganese modification can simultaneously utilize the properties of two metal oxides, and is suitable for the treatment of sewage and wastewater to remove low-concentration phosphorus.

[0045] The ingredients of the modified biochar include biochar, sodium hydroxide solution, potassium permanganate solution, ferric chloride solution, ferrous sulfate solution and deionized water.

[0046] Example 1

[0047] like Figure 1 As shown, a method for preparing iron-manganese modified biochar for removing low-concentration phosphorus-containing wastewater comprises the following steps:

[0048] S1: preparing corncob powder: crushing corncobs to obtain corncob powder;

[0049] S2: Preparation of carbonized powder: Pyrolysis of corn cob powder was performed under anoxic conditions by introducing N2 at a heating rate of 10°C / min to 500°C, and the temperature was maintained at this temperature for 120 min. After pyrolysis, the powder was cooled to room temperature and then ground to obtain carbonized powder.

[0050] S3: Processing the carbonized powder: Grinding the carbonized powder prepared in S2 and passing it through a 100-mesh sieve;

[0051] S4: Prepare reaction solution: prepare manganese solution and iron solution separately, dissolve 8.4g NaOH and 2.37g KMnO4 crystals in 200mL deionized water to prepare manganese solution, called solution a, dissolve 12.51g FeSO4·7H2O and 12.16g FeCl3·6H2O crystals in 200mL deionized water to prepare iron solution, called solution b, the molar ratio of KMnO4, FeSO4·7H2O, FeCl3·6H2O and NaOH is 1:3:3:14;

[0052] S5: Mixing reaction solution and carbonized powder: taking a certain amount of solution b and placing it in a 500 mL beaker, slowly adding a certain amount of solution a dropwise into solution b under rapid stirring, then adding the sieved carbonized powder in S3 into the mixed solution, and rapidly stirring the reaction for 60 min and then standing and aging for 8 h to allow the carbonized powder to fully contact with the mixed solution;

[0053] S6: high temperature drying: the carbonized powder in S6 that is in full contact with the mixed solution is filtered out using qualitative filter paper, and then placed in a high temperature oven at 105° C. for 4 hours for drying;

[0054] S7: preparing modified biochar: taking out the carbonized powder after high temperature drying in S7, grinding it and passing it through a 100-mesh sieve to obtain iron-manganese modified biochar.

[0055] like Figure 2 As shown, after iron and manganese oxides are precipitated and loaded on the surface of biochar, they can provide more active sites and adsorption sites, increase the contact area between biochar and target pollutants, and improve the adsorption capacity of biochar.

[0056] In order to determine the optimal amount of substance in each solution in the preparation method, the present invention conducts experiments on the molar ratio of three different solutions on biochar before determining the modified biochar preparation method, wherein the molar ratios of KMnO4, FeSO4·7H2O, FeCl3·6H2O and NaOH are 2:3:3:14, 1:3:3:14 and 1:6:6:14, respectively. Except for S4, the remaining steps and methods remain consistent. Subsequently, the biochar prepared with the three different amounts of solution substances and the unmodified biochar are subjected to phosphorus adsorption tests to analyze their phosphorus removal performance.

[0057] 0.1 g of the modified biochar prepared in this example was added to 50 mL of a 50 mg / L phosphorus solution and stirred in a shaker for adsorption for 12 hours, and then the phosphorus concentration in the solution was measured.

[0058] Comparative Example 1

[0059] In S4, the molar ratio of KMnO4, FeSO4·7H2O, FeCl3·6H2O and NaOH is 2:3:3:14, and the remaining steps are the same as in Example 1 to obtain modified biochar 1. 0.1 g of modified biochar 1 is added to 50 mL of a 50 mg / L phosphorus solution, stirred and adsorbed in a shaker for 12 hours, and then the phosphorus concentration in the solution is measured.

[0060] Comparative Example 2

[0061] In S4, the molar ratio of KMnO4, FeSO4·7H2O, FeCl3·6H2O and NaOH is 1:6:6:14, and the remaining steps are the same as in Example 1 to obtain modified biochar 2. 0.1 g of modified biochar 2 is added to 50 mL of a 50 mg / L phosphorus solution, stirred and adsorbed in a shaker for 12 hours, and then the phosphorus concentration in the solution is measured.

[0062] Comparative Example 3

[0063] 0.1 g of unmodified biochar was added to 50 mL of a 50 mg / L phosphorus solution and stirred in a shaker for 12 hours, and then the phosphorus concentration in the solution was measured.

[0064] The phosphorus removal rates of Example 1 and Comparative Examples 1-3 are shown in Table 1:

[0065] Table 1 Phosphorus removal results of different biochars

[0066]

[0067]

[0068] In summary, the removal rates of phosphorus in the solution by the modified biochars in Example 1, Comparative Example 1 and Comparative Example 2 are all higher than those of the unmodified biochars, and the removal rate of the modified biochar in Example 1 is increased by 91.92% compared with that of the modified biochar 1 in Comparative Example 1, while the removal rate of the high-concentration modified biochar 2 in Comparative Example 2 is only increased by 5.50% compared with that in Example 1; therefore, considering the cost issue, the molar ratio of the solutions used in Example 1 is optimal, that is, the molar ratio of KMnO4, FeSO4·7H2O, FeCl3·6H2O and NaOH is 1:3:3:14.

[0069] Example 2

[0070] To explore the carbon structure and structural characteristics of biochar, Raman spectroscopy was performed on unmodified biochar and iron-manganese modified biochar. The peak analysis of the characterization results was as follows: Figure 2 As shown:

[0071] From the figure analysis, we can see that the I D / I G =0.824, biochar after iron and manganese modification I D / I G =0.889, i.e. the amorphous carbon in the modified biochar (I D ) relative to the crystallized graphite phase (I G ) content increased. This shows that the iron and manganese loading increased the defect degree of biochar and increased the reaction active sites, thus having good catalytic degradation performance.

[0072] Example 3

[0073] according to Figure 4 From the modified biochar phosphate adsorption kinetics shown, it can be concluded that the adsorption process of phosphate by the iron-manganese modified biochar phosphorus removal agent in the present invention presents two stages: first, a rapid adsorption stage, and then a slow adsorption stage. When the adsorption time is 50 minutes, the adsorption rate of phosphate by the iron-manganese modified biochar phosphorus removal adsorbent is extremely fast; and when the adsorption time exceeds 2 hours, the adsorption amount of phosphate almost no longer increases, which indicates that the iron-manganese modified biochar phosphorus removal adsorbent has reached adsorption equilibrium.

[0074] It is worth noting that in the present invention, the pseudo-first-order kinetic model of the iron-manganese modified zeolite is closer to perfection than the pseudo-second-order kinetic model (R 2 This indicates that the modified product is more consistent with the pseudo-first-order kinetic model.

[0075] Example 4

[0076] In order to explore the specific surface area characteristics of the adsorbent, BET characterization was carried out on unmodified biochar and iron-manganese modified biochar. The adsorption and desorption curves are shown in Figure 2. Figure 5 As shown:

[0077] From the specific surface area results of unmodified biochar and modified biochar, we can see that the specific surface area of ​​iron-manganese modified biochar is 86.7165 m 2 / g, the specific surface area of ​​unmodified zeolite is 44.8792m 2 / g, the specific surface area increased by 93.2%, indicating that after the specific surface area of ​​the modified biochar increased, its ability to adsorb phosphate was greatly enhanced.

[0078] Example 5

[0079] In order to study the elemental composition characteristics of biochar adsorbents, unmodified biochar and iron-manganese modified biochar were characterized by XRF using the environmental soil mode. Each sample was tested 3 times and the average value of each element was taken. The test results are shown in Table 2:

[0080] Table 2 Test results

[0081]

[0082] It can be seen that the iron element increased 21.16 times after modification compared to before modification. The manganese element increased 30.72 times after modification compared to before modification. This shows that the loading of iron and manganese oxides on biochar is relatively firm. In addition, the modified biochar has more chlorine and sulfur elements than the unmodified biochar, with contents of 286.284ppm and 250.357ppm respectively. The content of potassium element decreased after modification. There are two possible reasons: first, the chemical solution used in the modification process may cause part of the potassium element to be eluted from the biochar, thereby reducing its content; second, during the modification process, iron and manganese oxides may react chemically with the potassium element in the biochar to form other compounds or precipitates, resulting in a decrease in the potassium content.

[0083] Example 6

[0084] In order to compare the adsorption effect of iron-magnesium modified biochar and iron-manganese modified biochar on low concentration phosphate, iron-magnesium modified biochar and iron-manganese modified biochar were prepared under the same molar ratio of 1:3:3:14, and 0.1g of unmodified biochar, iron-magnesium modified biochar, iron-manganese modified biochar and 50mL of 20mg / L phosphate solution were weighed respectively, and the mixture was shaken at a constant temperature of 25℃ and 150r / min in a water bath shaker. Samples were taken at different times (10min, 20min, 30min, 1h, 2h, 4h, 6h), and the phosphate concentration of the water sample was detected after passing through a 0.45μm microporous filter membrane. Figure 6 It can be seen that under the same adsorption time, the maximum adsorption capacity of the present invention for low-concentration phosphate can reach 8.051 mg / g, while the maximum adsorption capacity of iron-magnesium modified biochar can only reach 3.369 mg / g, which increases the maximum adsorption capacity by 138.9%. Therefore, the present invention has more advantages.

[0085] According to the above content, the preparation method provided in Example 1 of the present invention has the following advantages:

[0086] (1) After the iron-manganese oxides are precipitated and loaded on the surface of biochar, they can provide more active sites and adsorption sites, increasing the contact area and adsorption capacity between biochar and the target substance. In addition, iron-manganese oxides also have catalytic and oxidative properties, which can further improve the adsorption performance and catalytic degradation ability of biochar. There is a synergistic effect between the precipitation of iron-manganese oxides and biochar. The precipitated iron-manganese oxides can enhance the adsorption capacity of biochar, while also reducing the encapsulation effect of biochar, making it easier to contact with the target substance and enhancing its phosphorus removal effect.

[0087] (2) When the biochar prepared by this method is used for phosphorus removal, the iron ions in the iron-manganese oxide can form an iron-phosphate complex with orthophosphate, thereby achieving the removal of orthophosphate. In addition, the iron-manganese oxide can also convert orthophosphate into insoluble precipitates through oxidation, further reducing the concentration of orthophosphate.

[0088] (3) The present invention is simple to operate, the preparation cost of modified biochar is low, and the modified raw materials are harmless to the human body. It is a green, environmentally friendly and sustainable biochar modification method.

[0089] (4) The unit adsorption capacity of phosphate by the biochar adsorbent of the present invention can reach up to 9.738 mg / g, and it has good adsorption and removal performance for low-concentration phosphate, specifically, it can effectively remove phosphate less than 20 mg / L. The patent of the present invention provides theoretical guidance on biochar for the practical application of filler to enhance phosphorus removal performance.

[0090] (5) The specific surface area of ​​the iron-manganese modified biochar of the present invention is 86.7165 m 2 / g, compared with the specific surface area of ​​44.8792m2 of biochar before modification. 2 / g increased by 93.2%, indicating that its ability to adsorb phosphate was greatly increased.

[0091] (6) Compared with other methods on the market that use biochar modified by loading binary oxides for phosphorus removal, such as biochar modified by loading iron and magnesium oxides, magnesium chloride is corrosive to human skin and eyes, and may cause burns and tissue damage after contact. Inhalation of magnesium chloride solution vapor or mist may cause irritation to the respiratory tract and lungs, causing coughing, dyspnea and pulmonary edema. In addition, studies have shown that high concentrations of magnesium chloride may cause cancer in humans. Therefore, this patent is more in line with the experimental requirements of the preparation process in terms of safety.

[0092] The present invention is described in detail above through the embodiments, but the contents are only preferred embodiments of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made according to the scope of application of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for preparing iron-manganese modified biochar for removing low-concentration phosphorus-containing wastewater, characterized in that: The method comprises the following steps: S1: preparing corncob powder: crushing corncobs to obtain corncob powder; S2: preparing carbonized powder: pyrolyzing corn cob powder under anoxic conditions by introducing N2, cooling to room temperature after pyrolysis, and grinding to obtain carbonized powder; S3: Processing the carbonized powder: Grinding the carbonized powder prepared in S2 and passing it through a 100-mesh sieve; S4: Prepare reaction solution: prepare manganese solution and iron solution separately, dissolve NaOH and KMnO4 crystals in deionized water to prepare manganese solution, called solution a, dissolve FeSO4 and FeCl3 crystals in deionized water to prepare iron solution, called solution b; S5: Mixing the reaction solution and the carbonized powder: taking a certain amount of solution b and placing it in a 500 mL beaker, slowly dropping a certain amount of solution a into solution b under rapid stirring, then adding the sieved carbonized powder in S3 into the mixed solution, and rapidly stirring and then standing for aging to allow the carbonized powder to fully contact with the mixed solution; S6: high temperature drying: the carbonized powder in S5 that is in full contact with the mixed solution is filtered out using qualitative filter paper, and then placed in a high temperature oven for drying; S7: preparing modified biochar: taking out the carbonized powder after high temperature drying in S6, grinding it and passing it through a 100-mesh sieve to obtain iron-manganese modified biochar.

2. The method for preparing an iron-manganese modified biochar for removing low-concentration phosphorus-containing wastewater according to claim 1, characterized in that: In S2, the corncob powder is pyrolyzed at a heating rate of 10°C / min to 500°C, and the pyrolysis is continued at this temperature for 120 minutes.

3. The method for preparing an iron-manganese modified biochar for removing low-concentration phosphorus-containing wastewater according to claim 1, characterized in that: In S4, the FeSO4 crystals are FeSO4·7H2O, and the FeCl3 crystals are FeCl3·6H2O.

4. The method for preparing an iron-manganese modified biochar for removing low-concentration phosphorus-containing wastewater according to claim 3, characterized in that: In S4, the molar ratio of KMnO4, FeSO4·7H2O, FeCl3·6H2O and NaOH is 1:3:3:

14.

5. The method for preparing iron-manganese modified biochar for removing low-concentration phosphorus-containing wastewater according to claim 1, characterized in that: In S5, the rapid stirring reaction time is 60 min, and the static aging time is 8 h.

6. The method for preparing iron-manganese modified biochar for removing low-concentration phosphorus-containing wastewater according to claim 1, characterized in that: In S6, the drying temperature is 105°C and the time is 4 hours.

7. An iron-manganese modified biochar obtained according to the preparation method according to any one of claims 1 to 6.

8. Use of the iron-manganese modified biochar as claimed in claim 7 in sewage treatment technology.

9. The use according to claim 8, characterized in that: The sewage is low-concentration phosphorus-containing sewage.

Citation Information

Patent Citations

  • Preparation method of dephosphorization algae-control absorbent based on magnetic separation

    CN102974330A

  • Ferro-manganese binary metallic oxide modified haydite for removing phosphorus and preparation method thereof

    CN104984724A

  • Preparation method of biochar modified material for removing phosphorus in eutrophic water body

    CN109534432A

  • Preparation method and application of mulberry stem charcoal / Fe-Mn composite adsorbent

    CN110433772A

  • Modified zeolite dephosphorization adsorbent, preparation method thereof and application of modified zeolite dephosphorization adsorbent in dephosphorization of phosphorus-containing wastewater

    CN117960112A