Rolling adjusting method for two-pass cold-rolled variable-thickness plate
By calculating the transition zone slope in variable thickness rolling and assigning the rolling ratio, combining the rolling mill and tension control model, the problems of large thickness difference and short transition zone in variable thickness rolling are solved, and good control of plate thickness and plate shape is achieved .
Patent Information
- Application Number
- CN202411205720.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the variable thickness rolling process, the existing technology cannot effectively deal with the situation where the thickness difference between adjacent equal thickness sections is too large and the transition zone length is short, resulting in the inability to complete the sheet thickness control at one time, and it is difficult to reasonably distribute the rolling during two rolling passages. proportional ratio.
By obtaining the parameters of variable thickness rolling, calculate the actual slope of the transition zone and compare it with the preset slope. If the actual slope is greater than the preset slope, the rolling ratio will be allocated for two rolling. Otherwise, one rolling will be performed and the rolling mill will jump The model, transition section roll joint control model and tension control differential model control control control process to ensure good connection between the thickness of the plate and the shape of the plate.
The target control of plate thickness is achieved, ensuring good connection between the various thickness sections of the outlet and the transition section, and improving the stability and accuracy of the rolling process.
Smart Images

Figure CN118904931A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of variable thickness plate rolling, in particular to a two-pass cold-rolled variable thickness plate rolling adjustment method. Background Art
[0002] Variable-thickness rolled blanks (VRB) are mainly derived from the automotive industry's demand for lightweight and high-performance materials. During the steel plate rolling process, the gap between the rollers is controlled to change the plate thickness in the rolling direction, and the material thickness can be freely adjusted. By optimizing the thickness distribution, variable-thickness plates can improve the mechanical properties and durability of parts, and there is a continuous transition zone between plates of different thicknesses, with uniform performance and no sudden changes.
[0003] In variable thickness rolling, it may happen that the variable thickness control of the plate cannot be completed in one pass due to the short length of the transition zone and the large thickness difference between adjacent equal thickness sections. Therefore, it is necessary to reasonably allocate the rolling ratio and perform two passes of rolling. A method for adjusting the plate shape of rolled variable thickness plates, which pre-changes the bending roll force of the rolling mill by the amount of strip reduction, detects the actual rolling force and then corrects the bending roll force, and performs rolling according to the corrected bending roll force. A method for cold rolling variable thickness plates, which uses variable thickness rolling in the first pass to mark the beginning and end joints of each contour cycle at the outlet, or identifies the mark before rolling into the roll gap in the second pass, thereby determining the position of the strip for rolling.
[0004] In variable thickness rolling, the existing scheme does not consider that when the thickness difference between adjacent equal thickness sections is small and the transition zone length is sufficient, rolling can be completed in one go. If the difference between the two thicknesses is too large and the transition zone is short, how to deal with the situation that variable thickness rolling cannot be completed in one go? If the rolling is divided into two passes, how to reasonably allocate the rolling ratio in the two passes. In view of the above problems, the present invention provides a rolling adjustment strategy for cold rolled variable thickness plates. Summary of the invention
[0005] The purpose of the present invention is to provide a two-pass cold-rolled variable thickness plate rolling adjustment method to solve the problems existing in the above-mentioned prior art. Whether one-time rolling forming can be achieved is judged according to the length of the transition section and the thickness difference of adjacent equal thickness sections. If the one-time rolling forming conditions are not met, the rolling ratio is distributed by controlling the reduction rate and two-pass rolling is performed, thereby achieving the purpose of good connection between the equal thickness sections and the transition sections at the outlet and good plate shape.
[0006] To achieve the above object, the present invention provides the following solutions:
[0007] A two-pass cold-rolled variable thickness plate rolling adjustment method, comprising:
[0008] Acquiring parameters of variable thickness rolling, the parameters including: process parameters, plate and strip parameters and rolling mill parameters;
[0009] Based on the parameters, obtaining an actual slope of the transition zone;
[0010] The actual slope is compared with the preset slope. If the actual slope is greater than the preset slope, the rolling ratio is allocated and the plate thickness control is completed through two rollings. Otherwise, the plate thickness control is completed through one rolling.
[0011] Optionally, the actual slope of the transition zone is:
[0012]
[0013] Among them, k i is the actual slope of the transition zone, the subscript i is the secondary value of the transition zone, and h n is the thickness of the first equal thickness segment, h n+1 is the thickness of the second equal thickness segment, L n is the length of the transition zone.
[0014] Optionally, the plate thickness control is completed by one rolling process including:
[0015] Based on the rolling mill bounce model, the roll gap value of the first equal thickness section is preset;
[0016] Based on the roll gap value of the first equal thickness section, rolling of the first equal thickness section is performed;
[0017] After the first equal thickness section is rolled, the roller is lifted or pressed down, and the variable thickness area begins to be generated with the end point of the first equal thickness section as the zero point;
[0018] Based on the transition section roll gap control model, tension control differential model and flow velocity model, the roll gap change speed is controlled to complete the rolling in the transition zone and enter the second equal thickness section.
[0019] Optionally, the transition section roll gap control model is:
[0020]
[0021] Among them, h n is the thickness of the first equal thickness segment, h n+1 is the thickness of the second equal thickness segment, L n is the length of transition zone, F is rolling force, K′ is rolling mill stiffness, T(x t ) is the transition section roll gap control function, x t is the coordinate change value of the transition section;
[0022] The tension control differential model is:
[0023]
[0024] Among them, σ is the tensile stress of the rolled piece, t is the time, E is the elastic modulus of the rolled piece, and L0 is the length of the rolled piece;
[0025] The flow velocity model is:
[0026]
[0027] Among them, v r is the roller speed, h′ c is the roll gap change speed, v0 is the entry speed of the rolled piece, v1 is the exit speed of the rolled piece, h0 is half of the entry thickness of the rolled piece, h1 is half of the exit thickness of the rolled piece, θ n is the neutral angle, x n is the horizontal coordinate value corresponding to the neutral angle, -x0 is the horizontal coordinate of the inlet position, -x1 is the horizontal coordinate of the outlet position, h″ n It is half of the thickness of the plate at the neutral angle.
[0028] Optionally, the plate thickness control is completed by two rolling steps including:
[0029] Based on the incoming material thickness H, the target thickness h n 、h n+1 , and the total reduction rate is Set the first rolling thickness to h' n , h′ n+1 , corresponding to the first pass reduction rate The second rolling thickness is h n 、h n+1 , corresponding to the second pass reduction rate
[0030] Based on the first-pass rolling thickness and the first-pass rolling reduction rate, performing the first-pass rolling;
[0031] Based on the second-pass rolling thickness and the second-pass rolling reduction rate, the second-pass rolling is performed.
[0032] Optionally, performing a first-pass rolling based on the first-pass rolling thickness and the first-pass rolling reduction ratio; comprising:
[0033] Based on the rolling mill bounce model, the roll gap value of the first equal thickness section of the first pass is preset, and the first equal thickness section of the first pass is rolled;
[0034] After the first equal thickness section of the first pass is rolled, the roller starts to lift or press down, and the end point of the first equal thickness section of the first pass is taken as the zero point, and the first variable thickness zone begins to be generated. Based on the transition section roll gap control model, the tension control differential model and the flow velocity model, the roll gap change speed is controlled to complete the rolling of the first variable thickness zone, and the rolling of the second equal thickness section of the first pass begins. When the second equal thickness rolling is completed, the first pass is completed.
[0035] Optionally, the first rolling thickness is h′ n , h′ n+1 , the following conditions must be met:
[0036] h n+1 <h′ n+1 ≤2k′L n +h′ n , when the equal sign is obtained, it is h′ n+1 Maximum value;
[0037] At the same time h′ n >h n+1 -2k′L n .
[0038] Optionally, based on the second rolling thickness and the second rolling reduction rate, performing the second rolling comprises:
[0039] Based on the rolling mill bounce model, the roll gap value of the first equal thickness section of the second pass is preset, and the first equal thickness section of the second pass is rolled;
[0040] After the first equal thickness section of the second pass is rolled, the rollers begin to lift or press down, and the end point of the first equal thickness section of the second pass is taken as the zero point, and the second variable thickness zone begins to be generated. Based on the transition section roll gap control model, the tension control differential model and the flow velocity model, the roll gap change speed is controlled to complete the rolling of the second variable thickness zone, and the rolling of the second equal thickness section of the second pass begins. When the second equal thickness rolling is completed, the second pass ends.
[0041] The beneficial effects of the present invention are:
[0042] The method for cold rolling variable thickness plates of the present invention analyzes the tension of one-pass rolling and two-pass rolling and the thickness control of the rolled product, and considers whether the plate rolling meets the one-pass rolling forming conditions and how to reasonably distribute the rolling ratio through the thickness difference of two equal thickness sections and the length of the transition section when the one-pass rolling forming conditions are not met, so as to achieve the target thickness of the plate and the purpose of good plate shape of each equal thickness section and transition section at the outlet. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0044] Figure 1 A schematic flow chart of a two-pass cold-rolled variable thickness plate rolling adjustment method according to an embodiment of the present invention;
[0045] Figure 2 A schematic diagram of a variable thickness rolling process according to an embodiment of the present invention;
[0046] Figure 3 A schematic diagram of variable thickness rolling according to an embodiment of the present invention;
[0047] Figure 4 A schematic diagram of a transition zone coordinate axis according to an embodiment of the present invention;
[0048] Figure 5 A schematic diagram of a variable thickness rolling deformation zone according to an embodiment of the present invention;
[0049] Figure 6 Schematic diagram of target plate thickness according to an embodiment of the present invention. DETAILED DESCRIPTION
[0050] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0051] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0052] like Figure 1 As shown, this embodiment provides a two-pass cold-rolled variable thickness plate rolling adjustment method, comprising:
[0053] Obtaining the parameters of variable thickness rolling, including: process parameters, plate and strip parameters and rolling mill parameters;
[0054] Based on the parameters, the actual slope of the transition zone is obtained;
[0055] The actual slope is compared with the preset slope. If the actual slope is greater than the preset slope, the rolling ratio is allocated and the plate thickness control is completed through two rollings. Otherwise, the plate thickness control is completed through one rolling.
[0056] The adjustment method provided in this embodiment determines whether one-pass rolling forming can be achieved based on the length of the transition section and the thickness difference of adjacent equal-thickness sections. If the one-pass rolling forming conditions are not met, the rolling ratio is distributed by controlling the reduction rate and two-pass rolling is performed to achieve the purpose of good connection between the equal-thickness sections and the transition sections at the outlet and good plate shape.
[0057] Specifically, the variable thickness plate rolling can be achieved by one-pass rolling or two-pass rolling, such as Figure 3 As shown. It includes n+1 equal thickness sections and n transition sections (n is greater than zero and is an integer). If the thickness difference between adjacent equal thickness sections is too large and the length of the transition zone is short, it may not be possible to roll the steel piece into shape in one step. During the variable thickness rolling process, a curve is formed on the surface of the rolled piece in the transition zone. This curve connects the two equal thickness sections. This curve can be a straight line, a curve, or an arc connection. When the shape of the transition zone is a straight line, it is relatively simple and easy to implement. It is applicable to both longer and shorter transition zones. Therefore, by calculating the straight line slope k of the transition zone i With the determined rolling mill slope k i ′, when the calculated slope of the transition zone straight line k i Less than the rolling mill slope k i ′, it is determined that one-time rolling forming can be achieved. When the calculated slope of the transition zone straight line k i Not less than the rolling mill slope k i ', it is necessary to reasonably distribute the rolling reduction and carry out two passes of rolling. The first pass will initially process the rolled piece into an intermediate product of a certain shape and size, reducing the thickness difference of equal thickness sections. The second pass will continue the processing on the basis of the first pass, and further process the intermediate product into a final product that meets the requirements to complete the control of variable thickness plate rolling.
[0058] Furthermore, the actual slope of the transition region is:
[0059]
[0060] Among them, k i is the actual slope of the transition zone, the subscript i is the secondary value of the transition zone, and h n is the thickness of the first equal thickness segment, h n+1 is the thickness of the second equal thickness segment, L n is the length of the transition zone.
[0061] Specifically, the actual slope is compared with the preset slope. If the actual slope is greater than the preset slope, allocating the rolling ratio includes:
[0062] Collect and input the process, plate and mill parameters of variable thickness rolling, and set the length and thickness according to the target plate shape of each equal thickness section of the variable thickness plate to be rolled, which includes n+1 equal thickness sections, n transition sections, H n Represents the segment number of equal thickness segment, T n Represents the number of transition sections. The subscript n is the value of the equal thickness section and transition section, and n>0 and is an integer.
[0063] When the first section of equal thickness is rolled, the roll gap is pressed downward during rolling, and the workpiece becomes thinner. When the roll gap is lifted upward, the workpiece becomes thicker. A curve is formed on the surface of the workpiece, which connects the two sections of equal thickness. The curve can be a straight line, a curve, or an arc. When the shape of the transition zone is a straight line, it is relatively simple and easy to implement. It can be applied to both longer and shorter transition zones.
[0064] like Figure 4 As shown, the rolling end point of the first equal thickness section is taken as the origin, and the horizontal axis is x t , transition section roller gap function:
[0065] T(x t )=h c +F(x t )
[0066] h c is the rolling mill bounce equation,
[0067] F(x t ) is x t A linear function, F(x t ) = k i x t ;
[0068] h s is the target thickness difference between adjacent equal-thickness segments, h s =h n+1 -h n ;
[0069] k i is the slope of the transition zone, and the subscript i is the value of the transition section. h s =h n+1 -h n ;
[0070] where h n 、h n+1 is the thickness of the equal thickness segment, L n H n With H n+1 The length of the middle transition section, F is the rolling force, and K′ is the rolling mill stiffness.
[0071] Considering that if the thickness difference h of adjacent equal-thickness segments s Too large and the transition zone length L n If you want to roll the steel sheet with variable thickness in one pass, the rolling mill's pressure system must be highly flexible and responsive. In this case, variable thickness control may not be completed in one pass. During the rolling process, the rolled piece works together through the pressure system, speed control system, and tension control system to ensure the stability and accuracy of the rolling process. Therefore, a transition zone slope k is determined considering the limitations of existing rolling equipment (such as roll sensitivity, pressure system, speed control system, and tension control system) and process technology. i ′, such as when the roller sensitivity is high and the pressure reduction system control accuracy is high, the slope k i ′ is larger, that is, a variable thickness rolling process with a larger thickness difference can be achieved in a shorter transition zone. For rolled products whose pressure reduction control system is not sensitive enough and need to withstand a larger load, a gentler transition zone slope is required to reduce stress concentration.
[0072] By judging Whether satisfied.
[0073] If the slope of the transition zone meets the given conditions, the plate thickness control can be completed in one rolling process.
[0074] If the slope of the transition zone does not meet the given conditions, the plate thickness control cannot be completed through one rolling process and needs to be divided into two rolling processes.
[0075] Furthermore, the plate thickness control is completed by one rolling process including:
[0076] Based on the rolling mill bounce model, the roll gap value of the first equal thickness section is preset;
[0077] Based on the roll gap value of the first equal thickness section, rolling of the first equal thickness section is performed;
[0078] After the first equal thickness section is rolled, the roller is lifted or pressed down, and the variable thickness area begins to be generated with the end point of the first equal thickness section as the zero point;
[0079] Based on the transition section roll gap control model, tension control differential model and flow velocity model, the roll gap change speed is controlled to complete the rolling in the transition zone and enter the second equal thickness section.
[0080] Specifically, in this embodiment, when the transition zone slope When the conditions are met, the plate thickness control can be completed in one rolling. The first equal thickness section H n The thickness is h n The second equal thickness segment H n+1 The thickness is h n+1 , the length of the transition zone is L n, through the mill bounce equation, The roll gap value of the first equal thickness section is preset. When the first equal thickness section is rolled, the roll begins to rise or press down. The end point of the first equal thickness section is taken as the zero point, and the variable thickness zone begins to be generated. The roll gap control function of the transition section is:
[0081]
[0082] x t Starting from zero, the roll gap value begins to change.
[0083] During the variable thickness rolling process, the change in the roll gap speed will cause the outlet position of the rolled piece to shift, the second flow rate in the deformation zone to be unequal, and the tension to be unstable. Stable tension is the prerequisite for precise thickness control. Therefore, the primary goal during the variable thickness rolling process is to ensure the stability of the tension and avoid affecting the quality and precision of the rolled piece due to unstable tension.
[0084] Tension control differential equation:
[0085]
[0086] Among them, σ is the tensile stress of the rolled piece, t is the time, E is the elastic modulus of the rolled piece, L0 is the length of the rolled piece, and the original length of the rolled piece under no tension condition is l0.
[0087] The key to tension control is to control the speed of the workpiece inlet and outlet, and the essence of speed control is to control the roll speed or linear speed of the workpiece. In the past, researchers relied on the forward slip coefficient model to establish the relationship between the linear speed of the roll and the exit speed of the workpiece. For the static rolling process, it is a good method to establish the relationship between the roll speed and the workpiece speed through the forward slip coefficient. However, in the variable thickness rolling process, due to the change in the roll gap speed, this will cause the exit position of the workpiece to shift and the second flow rate in the deformation zone to be unequal. Therefore, the relationship between the roll speed and the exit and entrance speed of the workpiece is written according to the flow velocity model:
[0088]
[0089] Among them, v r is the roller speed, h′ c is the roll gap change speed, v0 is the entry speed of the rolled piece, v1 is the exit speed of the rolled piece, h0 is half of the entry thickness of the rolled piece, h1 is half of the exit thickness of the rolled piece, θ n is the neutral angle, x n is the horizontal coordinate value corresponding to the neutral angle, -x0 is the horizontal coordinate of the inlet position, -x1 is the horizontal coordinate of the outlet position, h″ n It is half of the thickness of the plate at the neutral angle.
[0090] When x t Increase to x t =L n At this time, the transition zone ends and the rolling enters the second equal thickness section. The incoming material thickness is H and the reduction is (Hh n )、(Hh n+1 ), at this time, the variable thickness rolling of the first constant thickness section and the second constant thickness section has been completed.
[0091] Furthermore, the plate thickness control is completed by two rolling steps including:
[0092] Based on the incoming material thickness H, the target thickness h n 、h n+1 , and the total reduction rate is Set the first rolling thickness to h' n , h′ n+1 , corresponding to the first pass reduction rate The second rolling thickness is h n 、h n+1 , corresponding to the second pass reduction rate
[0093] Based on the first-pass rolling thickness and the first-pass rolling reduction rate, performing the first-pass rolling;
[0094] Based on the second-pass rolling thickness and the second-pass rolling reduction rate, the second-pass rolling is performed.
[0095] Based on the first-pass rolling thickness and the first-pass rolling reduction rate, the first-pass rolling is performed; including:
[0096] Based on the rolling mill bounce model, the roll gap value of the first equal thickness section of the first pass is preset, and the first equal thickness section of the first pass is rolled;
[0097] After the first equal thickness section of the first pass is rolled, the roller starts to lift or press down, and the end point of the first equal thickness section of the first pass is taken as the zero point, and the first variable thickness zone begins to be generated. Based on the transition section roll gap control model, the tension control differential model and the flow velocity model, the roll gap change speed is controlled to complete the rolling of the first variable thickness zone, and the rolling of the second equal thickness section of the first pass begins. When the second equal thickness rolling is completed, the first pass is completed.
[0098] Based on the second-pass rolling thickness and the second-pass reduction rate, the second-pass rolling includes:
[0099] Based on the rolling mill bounce model, the roll gap value of the first equal thickness section of the second pass is preset, and the first equal thickness section of the second pass is rolled;
[0100] After the first equal thickness section of the second pass is rolled, the rollers begin to lift or press down, and the end point of the first equal thickness section of the second pass is taken as the zero point, and the second variable thickness zone begins to be generated. Based on the transition section roll gap control model, the tension control differential model and the flow velocity model, the roll gap change speed is controlled to complete the rolling of the second variable thickness zone, and the rolling of the second equal thickness section of the second pass begins. When the second equal thickness rolling is completed, the second pass ends.
[0101] Specifically, in this embodiment, when the transition zone slope When the conditions are not met, the thickness difference is too large, the transition zone length is insufficient, and one variable thickness rolling cannot complete the thickness control of the plate, so it needs to be divided into two rolling passes.
[0102] Incoming material thickness H, target thickness h n 、h n+1 The total reduction rate is The first rolling thickness is h′ n , h′ n+1 , the corresponding reduction rate is The second rolling thickness is h n 、h n+1 , the corresponding reduction rate is
[0103] Determine the distribution of pass reduction. During the cold rolling process, as the work hardening of the strip increases, the deformation resistance of the material also gradually increases. Therefore, in the first pass of cold rolling, since the material is relatively thick and the deformation resistance is relatively small, a larger reduction rate can be used for rolling. Therefore, under the following conditions, the first pass should be rolled as much as possible to ensure the final plate shape and thickness accuracy.
[0104] The first rolling thickness is h′ n , h′ n+1 , the following conditions must be met:
[0105] h n+1 <h′ n+1 ≤2k′L n +h′ n , when the equal sign is obtained, it is h′ n+1 Maximum value.
[0106] At the same time h′ n >h n+1 -2k′L n .
[0107] The first rolling thickness is h' n , h′ n+1 , through the mill bounce equation, The roll gap value of the first equal thickness section of the first pass is preset. After the first equal thickness section is rolled, the roll begins to rise or press down. The end point of the first equal thickness section is taken as the zero point, and the variable thickness zone begins to be generated. The roll gap control function of the transition section is:
[0108]
[0109] x t Starting from zero, the roll gap value begins to change.
[0110] The tension control differential equation is:
[0111]
[0112] where σ b is the unit back tension of the rack, E i is the elastic modulus of the rolled piece.
[0113]
[0114] where σ b is the unit post tension of the frame, h0 is the entrance thickness of the frame, is the rack unit back tension at time τ, is the entrance thickness of the rack at time τ.
[0115] While the roll gap value changes, the tension control model is used to ensure that the tension behind the stand unit remains unchanged, avoiding cracking of the rolled piece due to unstable tension.
[0116]
[0117] When x t Increase to x t =L n At this time, the rolling of the transition zone ends and the rolling of the second equal thickness section begins. When the second equal thickness rolling is completed, the first rolling pass ends and the second rolling pass begins.
[0118] In the second rolling, the shape and size of the rolled piece are relatively stable because the rolled piece has been preliminarily processed. At the end of the first rolling, the thickness of the rolled piece is h' n , h′ n+1 , the target thickness of the second pass rolled piece is h n 、h n+1 , through the mill bounce equation, The rolling force variation of the ΔF stand is pre-set, and the roll gap value of the first equal thickness section of the second pass is set. After the first equal thickness rolling is completed, the rolling enters the transition section, and the rolls begin to rise or press down. The roll gap control function of the transition section is:
[0119]
[0120] As t increases from zero, the roll gap value begins to change.
[0121] Tension control differential equation:
[0122]
[0123] While the roll gap value changes, the back tension value is kept stable by changing the roll speed value.
[0124]
[0125] When x t Increase to x t =L n At this time, the rolling of the transition zone ends, the roll gap is no longer lifted or pressed down, and the second equal thickness section begins rolling.
[0126] When the second equal thickness rolling is completed, the second variable thickness rolling is completed, and the intermediate product of the first pass is further processed into a final product that meets the requirements. After the two rolling passes are completed, the plate shape variable thickness control is completed.
[0127] The present embodiment is further described in detail below. Figure 2 As shown;
[0128] Assume that the target shape of the variable thickness plate to be rolled is as follows: Figure 6 As shown, it includes two equal thickness sections and one transition section, the initial thickness of the rolled piece is H=8mm, the target thickness of the first equal thickness section is h1=2mm, the target thickness of the second equal thickness section is h2=6mm, and the length of the transition section is L1=50mm.
[0129] (1) Collect and input the process, plate and mill parameters of variable thickness rolling, and set the length and thickness according to the target plate shape of each equal thickness section of the variable thickness plate to be rolled, which includes two equal thickness sections, one transition section, H n Represents the segment number of equal thickness segment, T n Represents the number of the transition segment, where n>0 and is an integer.
[0130] (2) When the first section of equal thickness is rolled, the roll gap is lifted upward during rolling, and the workpiece becomes thicker. A curve is formed on the surface of the workpiece, which connects the two sections of equal thickness. This curve can be a straight line.
[0131] (3) Determine the slope of the transition zone by taking into account the limitations of rolling equipment (such as roll sensitivity, pressure reduction system, speed control system and tension control system, etc.) and process technology. That is, for every 1mm difference in thickness between adjacent equal thickness sections, a transition zone of at least 50mm is required.
[0132] (4) Determine whether to perform one-pass rolling or two-pass rolling. The material thickness is H = 8 mm, the target thickness of the first equal thickness section is h1 = 2 mm, the target thickness of the second equal thickness section is h2 = 6 mm, and the length of the transition section is L1 = 50 mm. Therefore, the slope of the transition section is The thickness difference is too large and the transition zone length is not enough. One variable thickness rolling cannot complete the thickness control of the plate, so two variable thickness rolling passes are required.
[0133] (5) Determine the pass reduction distribution. The first pass rolling thickness is h′1 and h′2 respectively. When the following conditions are met, the first pass rolling is as long as possible to ensure the final plate shape and thickness accuracy.
[0134] Requirements:
[0135] h2=6mm <h′2≤2k′L1+h′1=2+h′1
[0136] h′1>h2-2k′L1=6mm-2mm=4mm
[0137] Therefore, the target thickness of the first pass is determined to be h′1=5mm, h′2=7mm. The reduction amount Δh′1=3mm, Δh′2=1mm, and the total reduction rate is
[0138] (6) At the beginning of the first rolling, the target plate thickness is h′1=5mm, h′2=7mm. When the first equal thickness rolling begins, the roll gap value is set in advance by the rolling mill bounce equation. The rolling mill bounce equation is: Where h1 is the thickness of the first equal thickness section, F1 is the rolling force, and K is the rolling mill stiffness.
[0139] When the first equal thickness section is rolled, the roller starts to rise, and the end point of the first equal thickness section is taken as the zero point, and the variable thickness area begins to be generated, such as Figure 4 , the transition section roll gap control function is:
[0140]
[0141] x t Starting from zero, the roll gap value begins to change.
[0142] In the variable thickness rolling process, due to the change in the roll gap speed, this will cause the outlet position of the rolled piece to shift, the flow rate in the deformation zone to be unequal, and the tension to be unstable. Stable tension is the prerequisite for accurate thickness control. Therefore, the primary goal in the variable thickness rolling process is to ensure the stability of the tension to avoid affecting the quality and precision of the rolled piece due to unstable tension. Figure 5 shown.
[0143] The differential equation for tension control is:
[0144]
[0145] where σ b is the unit back tension of the rack, E i is the elastic modulus of the rolled piece.
[0146]
[0147] where σ b is the unit post tension of the frame, h0 is the entrance thickness of the frame, is the rack unit back tension at time τ, is the entrance thickness of the rack at time τ.
[0148] The key to tension control is to control the speed of the workpiece inlet and outlet, and the essence of speed control is to control the roll speed or linear speed of the workpiece. In the past, researchers relied on the forward slip coefficient model to establish the relationship between the linear speed of the roll and the exit speed of the workpiece. For the static rolling process, it is a good method to establish the relationship between the roll speed and the workpiece speed through the forward slip coefficient. However, in the variable thickness rolling process, due to the change in the roll gap speed, this will cause the exit position of the workpiece to shift and the second flow rate in the deformation zone to be unequal. Therefore, the relationship between the roll speed and the exit and entrance speed of the workpiece is written according to the flow velocity model:
[0149]
[0150] Among them, v r is the roller speed, h′ c is the roll gap change speed, v0 is the entry speed of the rolled piece, v1 is the exit speed of the rolled piece, h0 is half of the entry thickness of the rolled piece, h1 is half of the exit thickness of the rolled piece, θ n is the neutral angle, x n is the horizontal coordinate value corresponding to the neutral angle, -x0 is the horizontal coordinate of the inlet position, -x1 is the horizontal coordinate of the outlet position, h″ n It is half of the thickness of the plate at the neutral angle.
[0151] When x t Increase to x t =100mm, the transition zone ends and the rolling enters the second equal thickness section. The roll gap value no longer changes, and the second equal thickness section starts rolling. When the second equal thickness rolling is completed, the first rolling pass ends and the second rolling pass starts.
[0152] (7) At the beginning of the second rolling, since the rolled piece has been preliminarily processed, its shape and size are relatively stable, and the target plate thickness is h1 = 2 mm and h2 = 6 mm. The roll gap value of the first equal thickness section of the second rolling pass is set in advance by the rolling mill bounce equation. Where ΔF is the rolling force variation of the stand.
[0153] When the first equal thickness section is rolled, the rolling enters the transition section, the rolls begin to rise, and the roll gap control function of the transition section is:
[0154]
[0155] x t Starting from zero, the roll gap value begins to change.
[0156] The tension control differential equation is:
[0157]
[0158] While the roll gap value changes, the back tension value is kept stable by changing the roll speed value.
[0159]
[0160] When x t Increase to x t =100mm, the rolling in the transition zone ends, the roll gap is no longer lifted or pressed down, and the second equal thickness section begins rolling.
[0161] When the second equal thickness rolling is completed, the second variable thickness rolling is completed, and the intermediate product of the first pass is further processed into a final product that meets the requirements. After the two rolling passes are completed, the plate shape variable thickness control is finally completed.
[0162] The above embodiments are only descriptions of the preferred embodiments of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should fall within the protection scope determined by the claims of the present invention.
Claims
1. A two-pass cold-rolled variable thickness plate rolling adjustment method, characterized in that: include: Acquiring parameters of variable thickness rolling, the parameters including: process parameters, plate and strip parameters and rolling mill parameters; Based on the parameters, obtaining an actual slope of the transition zone; The actual slope is compared with the preset slope. If the actual slope is greater than the preset slope, the rolling ratio is allocated and the plate thickness control is completed through two rollings. Otherwise, the plate thickness control is completed through one rolling.
2. The two-pass cold-rolled variable thickness plate rolling adjustment method according to claim 1, characterized in that: The actual slope of the transition region is: Among them, k i , the subscript i is the transition zone value, h n is the thickness of the first equal thickness segment, h n+1 is the thickness of the second equal thickness segment, L n is the length of the transition zone.
3. The two-pass cold-rolled variable thickness plate rolling adjustment method according to claim 1, characterized in that: Plate thickness control through one rolling process includes: Based on the rolling mill bounce model, the roll gap value of the first equal thickness section is preset; Based on the roll gap value of the first equal thickness section, rolling of the first equal thickness section is performed; After the first equal thickness section is rolled, the roller is lifted or pressed down, and the variable thickness area begins to be generated with the end point of the first equal thickness section as the zero point; Based on the transition section roll gap control model, tension control differential model and flow velocity model, the roll gap change speed is controlled to complete the rolling in the transition zone and enter the second equal thickness section.
4. The two-pass cold-rolled variable thickness plate rolling adjustment method according to claim 3, characterized in that: The transition section roll gap control model is: Among them, h n is the thickness of the first equal thickness segment, h n+1 is the thickness of the second equal thickness segment, L n is the length of transition zone, F is rolling force, K′ is rolling mill stiffness, T(x t ) is the transition section roll gap control function, x t is the coordinate change value of the transition section; The tension control differential model is: Among them, σ is the tensile stress of the rolled piece, t is the time, E is the elastic modulus of the rolled piece, and L0 is the length of the rolled piece; The flow velocity model is: Among them, v r is the roller speed, h′ c is the roll gap change speed, v0 is the entry speed of the rolled piece, v1 is the exit speed of the rolled piece, h0 is half of the entry thickness of the rolled piece, h1 is half of the exit thickness of the rolled piece, θ n is the neutral angle, x n is the horizontal coordinate value corresponding to the neutral angle, x0 is the horizontal coordinate of the inlet position, x1 is the horizontal coordinate of the outlet position, h″ n It is half of the thickness of the plate at the neutral angle.
5. The two-pass cold-rolled variable thickness plate rolling adjustment method according to claim 4, characterized in that: Plate thickness control is accomplished through two rolling passes including: Based on the incoming material thickness H, the target thickness h n 、h n+1 , and the total reduction rate is Set the first rolling thickness to h' n , h′ n+1 , corresponding to the first pass reduction rate The second rolling thickness is h n 、h n+1 , corresponding to the second pass reduction rate Based on the first-pass rolling thickness and the first-pass rolling reduction rate, performing the first-pass rolling; Based on the second-pass rolling thickness and the second-pass rolling reduction rate, the second-pass rolling is performed.
6. The two-pass cold-rolled variable thickness plate rolling adjustment method according to claim 5, characterized in that: Based on the first-pass rolling thickness and the first-pass rolling reduction rate, the first-pass rolling is performed; including: Based on the rolling mill bounce model, the roll gap value of the first equal thickness section of the first pass is preset, and the first equal thickness section of the first pass is rolled; After the first equal thickness section of the first pass is rolled, the roller starts to lift or press down, and the end point of the first equal thickness section of the first pass is taken as the zero point, and the first variable thickness zone begins to be generated. Based on the transition section roll gap control model, the tension control differential model and the flow velocity model, the roll gap change speed is controlled to complete the rolling of the first variable thickness zone, and the rolling of the second equal thickness section of the first pass begins. When the second equal thickness rolling is completed, the first pass is completed.
7. The two-pass cold-rolled variable thickness plate rolling adjustment method according to claim 5, characterized in that: The first rolling thickness is h' n , h′ n+1 , the following conditions must be met: h n+1 <h′ n+1 ≤2k′L n +h′ n , when the equal sign is obtained, it is h′ n+1 Maximum value; At the same time h′ n >h n+1 -2k′L n .
8. The two-pass cold-rolled variable thickness plate rolling adjustment method according to claim 5, characterized in that: Based on the second-pass rolling thickness and the second-pass reduction rate, the second-pass rolling includes: Based on the rolling mill bounce model, the roll gap value of the first equal thickness section of the second pass is preset, and the first equal thickness section of the second pass is rolled; After the first equal thickness section of the second pass is rolled, the rollers begin to lift or press down, and the end point of the first equal thickness section of the second pass is taken as the zero point, and the second variable thickness zone begins to be generated. Based on the transition section roll gap control model, the tension control differential model and the flow velocity model, the roll gap change speed is controlled to complete the rolling of the second variable thickness zone, and the rolling of the second equal thickness section of the second pass begins. When the second equal thickness rolling is completed, the second pass ends.