Continuous copper alloy strip preparation method
Through saw cutting and friction stir welding technology, combined with the use of arc-induced blocks, the problems of poor continuity and welding deformation oxidation in copper alloy strip production are solved, and efficient continuous production of copper alloy strips and high-quality welded joints are achieved.
Patent Information
- Application Number
- CN202411307295.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-19
AI Technical Summary
Poor continuity in the production process of copper alloy strips leads to low production efficiency. Traditional welding methods have welding deformation and oxidation problems, affecting product quality.
The copper alloy slab is cut by a sawing machine and friction stir welding is performed. The arc-induced block is used to ensure joint integrity, and the continuous production of copper alloy strips is achieved through multiple welding and annealing processes.
The production efficiency and material yield of copper alloy strips are improved, welding deformation and oxidation are avoided, and high-quality welded joints are obtained, ensuring product stability and material yield.
Smart Images

Figure CN118905576A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper alloy strip production, and in particular to a continuous copper alloy strip preparation method. Background Art
[0002] Copper alloy strips have good electrical conductivity, thermal conductivity and processing performance. They are widely used in the manufacture of printed circuit boards, radiators, connectors, connectors and other components in the electronics, communications, automotive and aerospace industries. However, compared with the continuous casting and rolling process of steel plates and strips, the continuity of the copper alloy plate and strip production process is poor. Since copper alloys are more easily oxidized at high temperatures and their high thermal conductivity leads to faster cooling, the ingot size is limited, so the length of the hot-rolled slab obtained by hot rolling is limited, which limits the efficiency of large-scale production of copper alloy plates and strips. In order to improve the continuity of the copper alloy strip production process, multiple hot-rolled slabs can be connected together to increase the length of the strip for continuous cold rolling and annealing in the subsequent process, thereby improving production efficiency. By connecting multiple hot-rolled slabs, longer continuous cold rolling and annealing processes can be achieved, reducing downtime and conversion time in production, and improving the operating stability and efficiency of the production line.
[0003] The current connection methods of hot-rolled copper alloy slabs mainly include mechanical connection, melting welding, etc. Among them, the connection strength of mechanical connection methods such as meshing is limited, and defects are easily generated at the connection during subsequent cold rolling, annealing, etc., affecting production stability. However, traditional welding methods such as arc welding have a large heat input, especially for thicker hot-rolled slabs (more than 10mm), which requires a higher welding current, resulting in severe oxidation of the welded joints and more serious welding deformation, which in turn affects the shape of the hot-rolled slab and is not conducive to the subsequent cold rolling process. Although the heat input of laser welding is much lower than arc welding, the welding deformation is smaller, and the molten pool is protected by inert gas during welding, and the oxidation situation is relatively less serious, the absorption rate of copper and its alloys to lasers is extremely low (the absorption rate of solid copper to welding lasers with a wavelength of 1064nm is only 3-5%), so the welding of large-sized copper alloy thick plates requires extremely high laser power, and the equipment investment cost is very high. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for preparing a continuous copper alloy strip.
[0005] The present invention adopts the following technical solution: a method for preparing a continuous copper alloy strip, the method comprising:
[0006] Step 1, melting and casting the copper alloy raw material to generate a copper alloy ingot, and hot rolling and milling the copper alloy ingot in sequence to obtain a copper alloy slab, and any one of the copper alloy slabs is used as a front slab;
[0007] Step 2, selecting another copper alloy slab that meets the size error as the rear slab, placing the front slab and the rear slab one after the other, and using a sawing machine to cut the tail of the front slab and the head of the rear slab at a preset angle in sequence;
[0008] Step 3: tightly splice the cut end face of the front slab with the cut end face of the rear slab, use a preset arc-starting block to abut on both sides of the joint between the front slab and the rear slab, and press and fix the tail of the front slab, the head of the rear slab and the arc-starting block;
[0009] Step 4, performing friction stir welding on the joint between the front slab and the rear slab, wherein the end point and the starting point of the friction stir welding are respectively on the arc-starting blocks on the left and right sides;
[0010] Step 5, cleaning the burrs and flash of the joint between the front plate blank and the rear plate blank after the friction stir welding, and removing the arc-starting blocks on the left and right sides to obtain a copper alloy welding plate;
[0011] Step 6: using the copper alloy welding plate as a front slab, repeating steps 2 to 5 until the copper alloy welding plate reaches a target length, and rolling up the copper alloy welding plate that has reached the target length to obtain a copper alloy slab coil;
[0012] Step seven, uncoiling the copper alloy slab coil, and sequentially performing rough rolling, primary annealing, intermediate rolling, secondary annealing, finish rolling, and final annealing to obtain a continuous copper alloy strip.
[0013] A method for preparing a continuous copper alloy strip according to an embodiment of the present invention can avoid the influence of the adverse texture formed in the hot rolling process on the performance of the welding joint to a certain extent by cutting the tail of the front slab and the head of the rear slab at a preset angle, thereby improving the strength and toughness of the joint, and then connecting multiple copper alloy slabs together by stir friction welding, and then performing subsequent cold rolling, annealing and other processes, thereby realizing continuous production of copper alloy strips, greatly improving production efficiency, and improving product yield and stability; at the same time, compared with the traditional copper alloy slab connection method, the present invention adopts stir friction welding, a solid phase welding method, to avoid serious welding deformation and oxidation, and obtain a high-quality welded joint with a strength and plasticity close to that of the parent material; and arc-starting blocks are used on both sides of the slab joint position during the welding process to ensure that the joints of the two copper alloy slabs are completely connected, and there is no need to cut the unwelded portions of the two side edges, only the arc-starting blocks need to be cut, further ensuring the product yield.
[0014] Furthermore, in step one, the smelting temperature is between 1060°C and 1300°C, the casting temperature is between 1010°C and 1250°C, the preheating temperature of hot rolling is between 720°C and 950°C, the final rolling temperature of hot rolling is between 550°C and 750°C, and the reduction rate of hot rolling is between 80% and 95%.
[0015] Furthermore, the dimensional error includes a thickness error and a width error, wherein the thickness error is ±0.3 mm and the width error is ±20 mm.
[0016] Furthermore, the step of using a sawing machine to sequentially cut the tail of the front slab and the head of the rear slab at a preset angle specifically includes:
[0017] A sawing machine is used to cut the tail of the front slab and the head of the rear slab in sequence, wherein the horizontal angle between the running direction of the saw blade of the sawing machine and the width direction of the front slab or the rear slab is between 10° and 20°, and the sawing machine cuts the front slab and the rear slab to the same size.
[0018] Furthermore, the composition of the arc-striking block is consistent with the composition of the front slab or the composition of the rear slab, and the thickness of the arc-striking block is consistent with the thickness of the front slab or the thickness of the rear slab.
[0019] Furthermore, when the friction stir welding is performed on the joint between the front slab and the rear slab, the rotation speed of the stirring head is between 600 r / min and 1000 r / min.
[0020] Furthermore, when friction stir welding is performed on the joint between the front slab and the rear slab, the moving speed of the stirring head on the arc striking block is between 20 mm / min and 40 mm / min, and the moving speed of the stirring head on the joint between the front slab and the rear slab is between 100 mm / min and 120 mm / min.
[0021] Further, in the step 7, the reduction rate of the rough rolling is between 70% and 90%, the temperature of the primary annealing is between 500° C. and 600° C., the holding time of the primary annealing is between 5h and 8h, the reduction rate of the intermediate rolling is between 60% and 80%, the temperature of the secondary annealing is between 450° C. and 500° C., the holding time of the secondary annealing is between 5h and 8h, and the reduction rate of the finishing rolling is between 10% and 50%;
[0022] Wherein, if the copper alloy strip is a soft strip, the temperature of the final annealing is 400° C. to 470° C., and the time of the final annealing is between 5 h and 8 h;
[0023] If the copper alloy strip is a hard strip, the final annealing is not necessary. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0025] Figure 1 This is a flow chart of the method for preparing a continuous copper alloy strip of Example 1;
[0026] Figure 2 The process structure diagram of friction stir welding in Example 1;
[0027] Figure 3 Schematic diagram of the morphology and position of each region in the microstructure of the friction stir welded joint in Example 1;
[0028] Figure 4 The micro-Vickers hardness diagram of different areas of the friction stir welded joint in Example 1;
[0029] Figure 5 The microstructure morphology of different areas of the friction stir welded joint in Example 1;
[0030] Figure 6 Schematic diagram of average grain size in different regions of the friction stir welded joint in Example 1;
[0031] Figure 7 This is a graph showing the tensile properties test results of the weld area of the stir friction welding joint in Example 1. DETAILED DESCRIPTION
[0032] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the embodiments of the present invention, and should not be construed as limiting the present invention.
[0033] In the description of the embodiments of the present invention, it should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0034] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the embodiments of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0035] In the embodiments of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the embodiments of the present invention can be understood according to specific circumstances.
[0036] Example 1
[0037] Reference Figure 1 The first embodiment of the present invention is a method for preparing a continuous copper alloy strip, the method comprising:
[0038] S1: melting and casting the copper alloy raw material to generate a copper alloy ingot, and hot rolling and milling the copper alloy ingot in sequence to obtain a copper alloy slab, and any copper alloy slab is used as a front slab;
[0039] Furthermore, the copper alloy raw material is melted at a temperature of 1060°C to 1300°C and cast at 1010°C to 1250°C; the preheating temperature of hot rolling is between 720°C and 950°C, the final rolling temperature of hot rolling is between 550°C and 750°C, and the reduction rate of hot rolling is between 80% and 95%.
[0040] In this embodiment, H65 brass is selected as the copper alloy raw material, that is, H65 brass strip is finally prepared; specifically, the H65 brass raw material is smelted at a temperature of 1060°C to 1200°C, and then cast at 1010°C to 1080°C to generate H65 brass ingot; then the H65 brass ingot is hot rolled and milled in sequence to obtain H65 brass slab; wherein, the preheating temperature of hot rolling is between 720°C and 900°C, the final rolling temperature of hot rolling is between 550°C and 700°C, and the reduction rate of hot rolling is 90%. In specific implementation, the reduction rate of hot rolling can also be 85%, 86%, 87%, 88%, 89%, etc., but is not limited thereto.
[0041] S2: another copper alloy slab that meets the size error is selected as the rear slab, the front slab and the rear slab are placed one after the other, and the tail of the front slab and the head of the rear slab are cut in turn at a preset angle using a sawing machine;
[0042] Furthermore, the dimensional error includes thickness error and width error, wherein the thickness error is ±0.3 mm and the width error is ±20 mm;
[0043] Furthermore, the step of using a sawing machine to sequentially cut the tail of the front slab and the head of the rear slab at a preset angle specifically includes:
[0044] A sawing machine is used to cut the tail of the front slab and the head of the rear slab in sequence, wherein the horizontal angle between the running direction of the saw blade of the sawing machine and the width direction of the front slab or the rear slab is between 10° and 20°, and the sawing machine cuts the front slab and the rear slab to the same size; specifically, the sawing machine starts cutting along the right-angle ends of the front slab and the rear slab, which can avoid the influence of the adverse texture formed in the hot rolling process on the performance of the welded joint to a certain extent and improve the strength and toughness of the joint, and fully considers saving materials and improving the yield rate of copper alloy strip products.
[0045] In this embodiment, the thickness of an H65 brass slab used as the front slab is 16.3 mm, the thickness of an H65 brass slab used as the first rear slab is 16.1 mm, the width of the front slab is 440.3 mm, the width of the rear slab is 445.5 mm, and the length of the stirring head for friction stir welding is 16.0 mm; the horizontal angle between the running direction of the saw blade of the sawing machine and the width direction of the front slab or the rear slab is 18°. After cutting is completed, the front slab is controlled to move backward until it is in close contact with the rear slab to complete the splicing. The gap between the cut end faces of the front slab and the rear slab is controlled to be within 0.2 mm.
[0046] S3: tightly splicing the cut end face of the front slab with the cut end face of the rear slab, using a preset arc-starting block to abut against both sides of the joint between the front slab and the rear slab, and pressing and fixing the tail of the front slab, the head of the rear slab and the arc-starting block;
[0047] Furthermore, the composition of the arc-striking block is consistent with the composition of the front slab or the composition of the rear slab, and the thickness of the arc-striking block is consistent with the thickness of the front slab or the thickness of the rear slab; this can ensure that the joints of the two copper alloy slabs are completely connected, and there is no need to cut the unwelded parts of the two side edges, only the arc-striking block needs to be cut, which further ensures the product yield.
[0048] In this embodiment, H65 brass plates are selected as arc-starting blocks (two pieces on the left and right), the length of the arc-starting blocks is 120.5 mm, the width is 50.3 mm, and the thickness is 16.2 mm; the tail of the front slab to be welded, the head of the rear slab and the arc-starting blocks are pressed downward, and at the same time, the left and right arc-starting blocks are close to the two sides of the slab and support them.
[0049] S4: Stir friction welding is performed on the joint between the front slab and the rear slab, and the end point and the starting point of the stir friction welding are respectively on the arc-starting blocks on the left and right sides;
[0050] Furthermore, when friction stir welding is performed on the joint between the front slab and the rear slab, the rotation speed of the stirring head is between 600 r / min and 1000 r / min.
[0051] Furthermore, when friction stir welding is performed on the joint between the front slab and the rear slab, the moving speed of the stirring head on the arc striking block is between 20 mm / min and 40 mm / min, and the moving speed of the stirring head on the joint between the front slab and the rear slab is between 100 mm / min and 120 mm / min.
[0052] In this embodiment, friction stir welding is performed on the H65 brass slab (the joint between the front slab and the rear slab), and the starting point and end point of the welding are respectively on the left and right arc-striking blocks; the stirring head rotates at a high speed of 600 r / min on the arc-striking block, and starts to move to the other side after the stirring shoulder turns red. The moving speed on the arc-striking block is controlled at 30 mm / min, and the moving speed on the H65 brass slab is controlled at 100 mm / min.
[0053] S5: cleaning the burrs and flashes of the joint between the front plate blank and the rear plate blank after the stirring and grinding welding, and removing the arc-starting blocks on the left and right sides to obtain the copper alloy welding plate.
[0054] In this embodiment, after welding is completed, burrs and flash are cleaned and arc-starting blocks on both sides are cut off to obtain an H65 brass welding plate.
[0055] S6: using the copper alloy welding plate as a front slab, repeating steps S2 to S5 until the copper alloy welding plate reaches a target length, and rolling up the copper alloy welding plate that has reached the target length to obtain a copper alloy slab coil.
[0056] In this embodiment, after the H65 brass weld plate that has been repeatedly subjected to friction stir welding reaches a target length, it can be rolled up to obtain an H65 brass sheet blank coil.
[0057] S7: uncoiling the copper alloy slab coil, and sequentially performing rough rolling, primary annealing, intermediate rolling, secondary annealing, finish rolling, and final annealing to obtain a continuous copper alloy strip;
[0058] Further, the reduction rate of rough rolling is between 80% and 90%, the temperature of primary annealing is between 500°C and 600°C, the holding time of primary annealing is between 5h and 8h, the reduction rate of intermediate rolling is between 60% and 80%, the temperature of secondary annealing is between 450°C and 500°C, the holding time of secondary annealing is between 5h and 8h, and the reduction rate of finishing rolling is between 10% and 50%;
[0059] If the copper alloy strip is a soft strip, the final annealing temperature is 400° C. to 470° C., and the final annealing time is between 5 h and 8 h; if the copper alloy strip is a hard strip, no final annealing is required.
[0060] In this embodiment, the H65 brass slab coil is unrolled, and then rough rolling, primary annealing, intermediate rolling, secondary annealing, finishing rolling, and final annealing are performed in sequence to obtain a continuous H65 brass strip, wherein the reduction ratio of rough rolling is 80%, the temperature of primary annealing is between 500°C and 550°C, the holding time of primary annealing is 6.5h, the reduction ratio of intermediate rolling is 60%, the temperature of secondary annealing is between 450°C and 500°C, the holding time of secondary annealing is 6.5h, and the reduction ratio of finishing rolling is 30%; if the H65 brass strip required for production is a soft strip, the temperature of the final annealing is 420°C to 470°C, and the time of the final annealing is 6.5h; If the H65 brass strip required for production is a hard strip, no final annealing is required; in specific implementation, the reduction rate of rough rolling can also be 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, etc., but not limited to this; the reduction rate of intermediate rolling can also be 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, etc., but not limited to this; the reduction rate of finish rolling can also be 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 31%, 32%, 33%, 34%, 35%, etc., but not limited to this.
[0061] In this embodiment, the friction stir welding process is as follows Figure 2 As shown, the high-temperature stirring head is embedded in the H65 brass blank and moves along the joint line between the front blank and the rear blank, with the front blank being the forward side and the rear blank being the backward side; Figure 3The overall morphology of the H65 brass slab welded joint is similar to an inverted "Ω". It is found that the interface on the advancing side of the weld is obvious, while the interface on the retreating side is fuzzy. In addition, no obvious defects are found on the weld surface, indicating that the weld structure is relatively dense. Figure 4 It can be seen that the micro-Vickers hardness of different areas of the friction stir welded joint is higher than that of the H65 brass base material, weld nugget zone (WNZ): 96.7HV0.1; thermo-mechanical affected zone (TMAZ): 92.8HV0.1; heat affected zone (HAZ): 91.0HV0.1; base material zone (BM): 82.9HV0.1.
[0062] according to Figure 5 and Figure 6 It can be seen that, affected by the stirring action of the stirring head, the grain size of the weld nugget zone (WNZ) is significantly smaller than that of the other three areas. The grain sizes of the thermomechanical affected zone (TMAZ), heat affected zone (HAZ) and parent material zone (BM) increase successively. The average grain sizes of different areas are as follows: the weld nugget zone (WNZ) is 16.2μm, the thermomechanical affected zone (TMAZ) is 23.2μm, the heat affected zone (HAZ) is 27.6μm, and the parent material zone (BM) is 46.6μm.
[0063] Depend on Figure 7 It can be seen that the tensile strength of the H65 brass slab base material is 351MPa and the elongation is 63%. The tensile strength of the stir friction welding joint weld is 339MPa and the elongation is 48%, which are similar to the base material; the stir friction welding joint has not cracked or damaged after cold rolling deformation with a reduction rate of more than 80%, and the tensile strength of the joint is 372MPa and the elongation is 50%; the final strip yield can be increased by 5%, and the deviation of the tensile strength can be reduced by 10Mpa to 20Mpa.
[0064] The continuous copper alloy strip preparation method of the present invention can avoid the influence of the adverse texture formed in the hot rolling process on the performance of the welding joint to a certain extent by cutting the tail of the front slab and the head of the rear slab at a preset angle, thereby improving the strength and toughness of the joint, and then connecting multiple copper alloy slabs together by stir friction welding, and then performing subsequent cold rolling, annealing and other processes, so as to achieve continuous production of copper alloy strips, greatly improve production efficiency, and improve product yield and stability; at the same time, compared with the traditional copper alloy slab connection method, the present invention adopts stir friction welding, a solid phase welding method, to avoid serious welding deformation and oxidation, and obtain a high-quality welded joint with a strong plasticity close to that of the parent material; and arc-starting blocks are used on both sides of the slab joint position during the welding process to ensure that the joints of the two copper alloy slabs are completely connected, and there is no need to cut the unwelded parts of the two side edges, only the arc-starting blocks need to be cut, which further ensures the product yield.
[0065] Example 2
[0066] In this embodiment, H70 brass is selected as the copper alloy raw material, that is, H70 brass strip is finally prepared; specifically, the H70 brass raw material is smelted at a temperature of 1100°C to 1300°C, and then cast at 1040°C to 1150°C to generate H70 brass ingot; then the H70 brass ingot is hot rolled and milled in sequence to obtain H70 brass slab; wherein, the preheating temperature of hot rolling is between 800°C and 950°C, the final rolling temperature of hot rolling is between 550°C and 700°C, and the reduction rate of hot rolling is 95%. In specific implementation, the reduction rate of hot rolling can also be 90%, 91%, 92%, 93%, 94%, etc., but is not limited thereto.
[0067] In this embodiment, the thickness of an H70 brass slab used as the front slab is 16.5 mm, the thickness of an H70 brass slab used as the first rear slab is 16.2 mm, the width of the front slab is 440.1 mm, the width of the rear slab is 443.5 mm, and the length of the stirring head for friction stir welding is 16.2 mm; the horizontal angle between the running direction of the saw blade of the sawing machine and the width direction of the front slab or the rear slab is 10°. After cutting, the front slab is controlled to move backward until it is in close contact with the rear slab to complete the splicing. The gap between the cut end faces of the front slab and the rear slab is controlled to be within 0.2 mm.
[0068] In this embodiment, H70 brass plates are selected as arc-starting blocks (two pieces on the left and right), the length of the arc-starting blocks is 122.5 mm, the width is 51.2 mm, and the thickness is 16.3 mm; the tail of the front slab to be welded, the head of the rear slab and the arc-starting blocks are pressed downward, and at the same time, the left and right arc-starting blocks are close to the two sides of the slab and support them.
[0069] In this embodiment, friction stir welding is performed on the H70 brass slab (the joint between the front slab and the rear slab), and the starting point and end point of the welding are respectively on the left and right arc-striking blocks; the stirring head rotates at a high speed of 800 r / min on the arc-striking block, and starts to move to the other side after the stirring shoulder turns red. The moving speed on the arc-striking block is controlled at 20 mm / min, and the moving speed on the H70 brass slab is controlled at 105 mm / min.
[0070] In this embodiment, after welding is completed, burrs and flash are cleaned and arc-starting blocks on both sides are cut off to obtain an H70 brass welding plate.
[0071] In this embodiment, after the H70 brass weld plate that has been repeatedly subjected to friction stir welding reaches a target length, it can be rolled up to obtain an H70 brass sheet blank coil.
[0072] In this embodiment, the H70 brass slab coil is unrolled, and then rough rolling, primary annealing, intermediate rolling, secondary annealing, finish rolling, and final annealing are performed in sequence to obtain a continuous H70 brass strip, wherein the reduction ratio of the rough rolling is 70%, the temperature of the primary annealing is between 500°C and 600°C, the holding time of the primary annealing is between 5h, the reduction ratio of the intermediate rolling is 70%, the temperature of the secondary annealing is between 450°C and 500°C, the holding time of the secondary annealing is 5h, and the reduction ratio of the finish rolling is 10%; if the H70 brass strip required for production is a soft strip, the temperature of the final annealing is 430°C to 470°C, and the time of the final annealing is 5h; if the H70 brass strip required for production is a soft strip, the temperature of the final annealing is 430°C to 470°C, and the time of the final annealing is 5h; The H70 brass strip is a hard strip, so there is no need for final annealing; in specific implementation, the reduction rate of rough rolling can also be 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80% and the like, but not limited thereto; the reduction rate of intermediate rolling can also be 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80% and the like, but not limited thereto; the reduction rate of finish rolling can also be 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25% and the like, but not limited thereto.
[0073] Example 3
[0074] In this embodiment, T2 copper is selected as the copper alloy raw material, that is, T2 copper strip is finally prepared; specifically, the T2 copper raw material is smelted at a temperature of 1100°C to 1300°C, and then cast at 1100°C to 1250°C to generate a T2 copper ingot; then the T2 copper ingot is hot rolled and milled in sequence to obtain a T2 copper slab; wherein, the preheating temperature of the hot rolling is between 850°C and 950°C, the final rolling temperature of the hot rolling is between 600°C and 750°C, and the reduction rate of the hot rolling is 80%. In specific implementation, the reduction rate of the hot rolling can also be 81%, 82%, 83%, 84%, 85%, etc., but is not limited to this.
[0075] In this embodiment, the thickness of a T2 copper slab used as the front slab is 15.8 mm, the thickness of the T2 copper slab used as the first rear slab is 15.6 mm, the width of the front slab is 440.2 mm, the width of the rear slab is 442.5 mm, and the length of the stirring head for stir friction welding is 15.5 mm; the horizontal angle between the running direction of the saw blade of the sawing machine and the width direction of the front slab or the rear slab is 20°. After cutting is completed, the front slab is controlled to move backward until it is in close contact with the rear slab to complete the splicing, and the gap between the cut end faces of the front slab and the rear slab is controlled within 0.2 mm.
[0076] In this embodiment, T2 copper plates are selected as arc-starting blocks (two pieces on the left and right), the length of the arc-starting blocks is 125.5 mm, the width is 50.2 mm, and the thickness is 15.8 mm; the tail of the front slab to be welded, the head of the rear slab and the arc-starting blocks are pressed downward, and at the same time, the left and right arc-starting blocks are close to the two sides of the slab and supported.
[0077] In this embodiment, friction stir welding is performed on the T2 copper slab (the joint between the front slab and the rear slab), and the starting point and end point of the welding are respectively on the left and right arc-striking blocks; the stirring head rotates at a high speed of 1000r / min on the arc-striking block, and starts to move to the other side after the stirring shoulder turns red. The moving speed on the arc-striking block is controlled at 40mm / min, and the moving speed on the T2 copper slab is controlled at 120mm / min.
[0078] In this embodiment, after welding is completed, burrs and flash are cleaned and arc-starting blocks on both sides are cut off to obtain a T2 copper welding plate.
[0079] In this embodiment, after the T2 copper welding plate that has been repeatedly subjected to friction stir welding reaches a target length, it can be rolled up to obtain a T2 copper plate blank coil.
[0080] In this embodiment, the T2 copper slab coil is unrolled, and then rough rolling, primary annealing, intermediate rolling, secondary annealing, finishing rolling, and final annealing are performed in sequence to obtain a continuous T2 copper strip, wherein the reduction ratio of rough rolling is 90%, the temperature of primary annealing is between 500°C and 600°C, the holding time of primary annealing is between 8h, the reduction ratio of intermediate rolling is 80%, the temperature of secondary annealing is between 450°C and 500°C, the holding time of secondary annealing is 8h, and the reduction ratio of finishing rolling is 50%; if the T2 copper strip required for production is a soft strip, the temperature of final annealing is 400°C to 450°C, and the time of final annealing is 8h; If the T2 copper strip required for production is a hard strip, final annealing is not required; in specific implementation, the reduction rate of rough rolling can also be 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89% and the like, but not limited to this; the reduction rate of intermediate rolling can also be 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79% and the like, but not limited to this; the reduction rate of finish rolling can also be 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49% and the like, but not limited to this.
[0081] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0082] Under the premise that no conflict occurs, those skilled in the art may freely combine and superimpose the above-mentioned additional technical features.
[0083] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a continuous copper alloy strip, characterized in that: The method comprises: Step 1, melting and casting the copper alloy raw material to generate a copper alloy ingot, and hot rolling and milling the copper alloy ingot in sequence to obtain a copper alloy slab, and any one of the copper alloy slabs is used as a front slab; Step 2, selecting another copper alloy slab that meets the size error as the rear slab, placing the front slab and the rear slab one after the other, and using a sawing machine to cut the tail of the front slab and the head of the rear slab at a preset angle in sequence; Step 3: tightly splice the cut end face of the front slab with the cut end face of the rear slab, use a preset arc-starting block to abut on both sides of the joint between the front slab and the rear slab, and press and fix the tail of the front slab, the head of the rear slab and the arc-starting block; Step 4, performing friction stir welding on the joint between the front slab and the rear slab, wherein the end point and the starting point of the friction stir welding are respectively on the arc-starting blocks on the left and right sides; Step 5, cleaning the burrs and flash of the joint between the front plate blank and the rear plate blank after the friction stir welding, and removing the arc-starting blocks on the left and right sides to obtain a copper alloy welding plate; Step 6: using the copper alloy welding plate as a front slab, repeating steps 2 to 5 until the copper alloy welding plate reaches a target length, and rolling up the copper alloy welding plate that has reached the target length to obtain a copper alloy slab coil; Step seven, uncoiling the copper alloy slab coil, and sequentially performing rough rolling, primary annealing, intermediate rolling, secondary annealing, finish rolling, and final annealing to obtain a continuous copper alloy strip.
2. The method for preparing a continuous copper alloy strip according to claim 1, characterized in that: In step one, the smelting temperature is between 1060°C and 1300°C, the casting temperature is between 1010°C and 1250°C, the preheating temperature of hot rolling is between 720°C and 950°C, the final rolling temperature of hot rolling is between 550°C and 750°C, and the reduction rate of hot rolling is between 80% and 95%.
3. The method for preparing a continuous copper alloy strip according to claim 1, characterized in that: The dimensional error includes a thickness error and a width error, wherein the thickness error is ±0.3 mm and the width error is ±20 mm.
4. The method for preparing a continuous copper alloy strip according to claim 1, characterized in that: The steps of sequentially cutting the tail of the front slab and the head of the rear slab at a preset angle using a sawing machine specifically include: A sawing machine is used to cut the tail of the front slab and the head of the rear slab in sequence, wherein the horizontal angle between the running direction of the saw blade of the sawing machine and the width direction of the front slab or the rear slab is between 10° and 20°, and the sawing machine cuts the front slab and the rear slab to the same size.
5. The method for preparing a continuous copper alloy strip according to claim 1, characterized in that: The composition of the arc-striking block is consistent with the composition of the front slab or the composition of the rear slab, and the thickness of the arc-striking block is consistent with the thickness of the front slab or the thickness of the rear slab.
6. The method for preparing a continuous copper alloy strip according to claim 1, characterized in that: When friction stir welding is performed on the joint between the front slab and the rear slab, the rotation speed of the stirring head is between 600 r / min and 1000 r / min.
7. The method for preparing a continuous copper alloy strip according to claim 1, characterized in that: When friction stir welding is performed on the joint between the front slab and the rear slab, the moving speed of the stirring head on the arc striking block is between 20 mm / min and 40 mm / min, and the moving speed of the stirring head on the joint between the front slab and the rear slab is between 100 mm / min and 120 mm / min.
8. The method for preparing a continuous copper alloy strip according to claim 1, characterized in that: In the step 7, the reduction rate of the rough rolling is between 70% and 90%, the temperature of the primary annealing is between 500° C. and 600° C., the holding time of the primary annealing is between 5h and 8h, the reduction rate of the intermediate rolling is between 60% and 80%, the temperature of the secondary annealing is between 450° C. and 500° C., the holding time of the secondary annealing is between 5h and 8h, and the reduction rate of the finishing rolling is between 10% and 50%; Wherein, if the copper alloy strip is a soft strip, the temperature of the final annealing is 400° C. to 470° C., and the time of the final annealing is between 5 h and 8 h; If the copper alloy strip is a hard strip, the final annealing is not necessary.
Citation Information
Patent Citations
Cyclical ultrasonic impact process for maintaining welding joint
CN105643186A
Short-process production method for high-strength and high-conductivity copper alloy strips
CN107716885A
Coil type butt welding method of berylco alloy plate strip
CN110653478A
Friction stir welding method for thick copper plate and multi-layer copper foil
CN116352246A
Channel steel welding structure
CN221168172U
Cited By
Plastic forming preparation method for whole-bottom plate blank of carrier rocket storage tank
CN120828253A
Method for preparing a whole bottom plate blank of a launch vehicle tank
CN120828253B