Preparation method of novel biomass porous graphene potassium ion battery negative electrode material

By preparing biomass porous graphene materials using white radish as a precursor, the problems of structural collapse and low diffusion rate of potassium-ion battery anode materials during charging and discharging were solved, achieving high-efficiency potassium-ion battery performance and stability at a low cost.

CN118908193AActive Publication Date: 2024-11-08CHINA UNIV OF GEOSCIENCES (BEIJING)
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411032815.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-08
Estimated Expiration
2044-07-30
Patent Text Reader

Abstract

The invention relates to a preparation method of a novel biomass porous graphene potassium ion battery negative electrode material, and belongs to the technical field of potassium ion battery preparation. Inspired by unique sheet structures and chemical components of cell membranes and cell walls, porous graphene with high torsion resistance is designed as an efficient negative electrode material of the potassium ion battery. The preparation method is characterized in that cheap and easily available white radish is adopted as a main raw material, firstly, a biomass graphite material is obtained after soaking, carbonization and vacuum hot pressed sintering, and then the biomass porous graphene negative electrode material (WHBG) is prepared through an improved Hummers method. The porous graphene potassium ion battery negative electrode material prepared by the method has excellent electrochemical performance, good conductivity and good cycling stability. The required raw materials are easy to obtain, and the material prepared by the process can solve the problems of poor structural stability and low K < + > diffusion rate of the traditional graphite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a novel biomass porous graphene potassium ion battery negative electrode material, belonging to the technical field of potassium ion battery preparation. Background Art

[0002] As humans over-exploit and use fossil energy such as coal, oil, and natural gas, the living environment has been unprecedentedly polluted. The mining process has caused geological damage and pollution, and the use has also brought a series of environmental problems such as greenhouse effect, air pollution, and water pollution. Therefore, the exploration and development of green new energy has become an inevitable trend in the green development of society. In recent years, lithium-ion batteries have been widely used in energy storage systems in various scenarios, and the demand for them is increasing day by day. However, the reserves of lithium ore resources are limited and the mining process will also cause environmental pollution. Therefore, it is urgent to seek a new energy storage system with abundant resources, low prices, and excellent performance.

[0003] Carbonaceous materials have the advantages of being environmentally friendly, low cost and widely available for potassium ion battery anode materials. However, the commonly used graphite anode has a slow K + Kinetic and structural instability limit the performance of potassium ion batteries. As a member of carbon materials, the advantage of using biomass as a carbon source is that it can directly prepare nanostructured carbon negative electrode materials with pores, and exhibit excellent non-stoichiometric capacity and rate performance, and reduce material costs. However, biomass carbon-based negative electrodes also face similar challenges as traditional graphite materials. + The ions are large in size and their volume changes during charge and discharge are serious, which will lead to faster structural collapse and capacity decay of the electrode. In addition, the long and tortuous diffusion path and small effective electrochemical active surface area lead to K + The diffusion rate is very low, which limits the reaction kinetics and rate capability, showing a low practical specific capacity.

[0004] Therefore, the present invention combines the above problems, and based on the unique thin sheet structure and chemical composition of biomass cell membrane and cell skin, a series of biomass carbon-based negative electrode materials are synthesized and prepared using white radish as a biomass precursor. Experiments have shown that the negative electrode material has good electrochemical properties, providing a new way to design efficient carbon-based negative electrode materials for practical applications in potassium ion batteries. Summary of the invention

[0005] The purpose of the present invention is to further apply the current new energy storage system and enhance the potassium storage performance of potassium ion carbon-based negative electrode materials, and propose a new process for preparing biomass porous graphene (WHBG) using white radish as a biomass precursor, a heat treatment method and an improved Hummers method.

[0006] To achieve the above object, the technical solution of the present invention is as follows:

[0007] The present invention is a method for preparing a biomass porous graphene potassium ion battery negative electrode material, comprising the following steps:

[0008] S1, first cutting the white radish into small cubes, then soaking them in deionized water for pretreatment to remove soluble impurities, and then putting the soaked white radish cubes into a drying oven for drying to ensure that the water in the biological cells can evaporate quickly to form a contracted structure;

[0009] S2, carbonizing the precursor obtained in step S1 and mixing it with Fe2O3, and then sintering it by vacuum hot pressing to obtain a biomass graphite material;

[0010] S3, after mixing the biomass graphite obtained in step S2 with NaNO3, slowly add concentrated H2SO4 and stir, then place the mixed solution in an ice bath and add KMnO4, and then heat it in a water bath;

[0011] S4. Add a small amount of 30% H2O2 to the solution in step S3 to remove excess KMnO4, and finally centrifuge, dry and reduce the mixture to obtain WHBG.

[0012] Specifically, in step S1, the size of the white radish pieces is 2x2 cm-4x4 cm, the thickness is 1-2 cm, the deionized water soaking time is 30-120 min, the drying temperature is 80° C.-120° C., and the insulation time is 12-24 h;

[0013] Specifically, in step S2, the carbonization temperature is 400-600°C, the carbonization atmosphere is one of argon and nitrogen, and the heating rate is 2-5°C min -1 , the holding time is 2-6h, the Fe2O3 content is 0.1-10wt.%, the hot pressing furnace pressure is 1-1.5MPa, the hot pressing temperature is 2000-2400℃, and the holding time is 1-2h;

[0014] Specifically, in step S3, the mass ratio of biomass graphite to NaNO3 is 0.5:1-1:1, the volume of concentrated H2SO4 is 30-60mL, the stirring time is 1-2h, the KMnO4 content is 2-4g, the water bath temperature is 35-100℃, and the stirring time is 30-60min;

[0015] Specifically, in step S4, the concentration of H2O2 is 30-70%, the centrifuge speed is 6000-10000 rpm, the drying temperature is 60-100°C, and the drying time is 12-24 hours.

[0016] The further claimed potassium ion battery preparation process comprises the following steps:

[0017] (1) The prepared biomass porous graphene material, conductive carbon black and binder (PVDF) are mixed in a mass ratio of 6:2:2-8:1:1 and an appropriate amount of N-methylpyrrolidone (NMP) is added to form a slurry, which is then coated on a copper foil current collector. The electrode sheet is dried in a vacuum drying oven at 80-110°C for 12 hours, and after drying, it is cut into 9-12 mm electrode sheets for standby use.

[0018] (2) CR2032 button cells were used to assemble the battery. The entire battery assembly process was completed in a glove box with a water and oxygen content of less than 0.01 ppm. Metal potassium was used as the positive electrode, the separator was Whatman GF / D glass fiber, the electrolyte was 0.8M KPF6 inDEC / EC, and the negative electrode was the above-mentioned electrode sheet. The assembly order was negative electrode shell, metal potassium foil, separator (fully wetted with electrolyte), electrode sheet, gasket, spring and positive electrode shell. The button cell was tested after being left to rest.

[0019] Compared with the prior art, the present invention provides a novel method for preparing a negative electrode material of a potassium ion battery made of biomass porous graphene (WHBG), which has the following benefits:

[0020] 1. The porous graphene material prepared by the present invention has excellent rate performance and cycle stability; at 25mAg -1 The initial discharge capacity at the current density is 1464 mAh g -1 , then at 1A g -1 Ultra-long cycles were carried out at the current density, and the capacity retention rate was 93.5% compared with the 11th cycle, which can meet the needs of practical applications.

[0021] 2. The biomass porous graphene material prepared by this method is low-cost and easy to obtain, and the hot pressing sintering method can retain the honeycomb-like wrinkled morphology in the original white radish material and avoid the accumulation of graphene, thereby obtaining high reversible capacity and stability.

[0022] 3. WHBG with wrinkles and pores has mechanical stability during charge and discharge due to its dual stress buffering effect. The nanopores promote K + diffusion. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is further described below with specific embodiments, but is not limited to the following implementation cases.

[0024] Example 1

[0025] (1) Cut the white radish into 2x2 cm cubes with a thickness of 2 cm, and then soak them in deionized water for 60 min to remove soluble impurities; dry the soaked white radish cubes in a drying oven at 80° C. for 12 h, so that the water in the biological cells can evaporate quickly to form a contracted structure;

[0026] (2) The precursor obtained in step (1) was placed in a tube furnace with an Ar gas atmosphere at 2°C min -1 The temperature was raised to 600℃ at a heating rate and carbonized for 4h. The carbonized precursor was mixed with 0wt.% Fe2O3, and then the temperature was quickly raised to 2200℃ in a hot press furnace at 1.15MPa and kept for 1h to finally obtain a biomass graphite precursor.

[0027] (3) Take 0.6g of the biomass graphite precursor obtained in step (2), mix it with 1.0g of NaNO3 and add it to a beaker, and slowly add 50mL of H2SO4 and stir for 1h. Place the mixed beaker in an ice bath, slowly add 3.0g of KMnO4 and stir for 2h. Then heat the water bath to 35°C, stir for 30min, and then slowly add 150mL of deionized water;

[0028] (4) Following step (3), the reaction system was heated to 98°C and poured into 200 mL of deionized water at 60°C while hot. 5 mL of 30% H2O2 was added dropwise to remove excess KMnO4. The reaction mixture was centrifuged at 6000 rpm and the product was transferred to a forced air drying oven at 60°C for 24 h to dry and reduce to obtain WHBG.

[0029] The biomass porous graphene negative electrode material prepared in Example 1 has a high conductivity at 25 mA g -1 The initial discharge capacity at the current density is 423 mAh g -1 , at 25mA g -1 After 150 cycles, it can still retain 178 mAh g -1 , then at 1A g -1 Ultra-long cycling was carried out at a current density of 1.5047 W / m, and the capacity retention rate was 65.5% compared with the 11th cycle. The potassium ion battery assembled with the WHBG negative electrode material prepared in Example 1 has a stable cycle capacity and can meet application requirements.

[0030] Example 2

[0031] (1) Cut the white radish into 2x2 cm cubes with a thickness of 1 cm, and then soak them in deionized water for 60 min to remove soluble impurities; dry the soaked white radish cubes in a drying oven at 80° C. for 12 h, so that the water in the biological cells can evaporate quickly to form a contracted structure;

[0032] (2) The precursor obtained in step (1) was placed in a tube furnace with an Ar gas atmosphere at 2°C min -1 The temperature was raised to 600℃ at a heating rate and carbonized for 4h. The carbonized precursor was mixed with 2wt.% Fe2O3, and then the temperature was quickly raised to 2200℃ in a hot press furnace at 1.15MPa and kept for 1h to finally obtain a biomass graphite precursor.

[0033] (3) Take 0.6g of the biomass graphite precursor obtained in step (2), mix it with 1.0g of NaNO3, add it to a beaker, and slowly add 50mL of H2SO4, and stir for 1h. Place the mixed beaker in an ice bath, slowly add 3.0g of KMnO4, and stir for 2h. Then heat the water bath to 35°C, stir for 30min, and then slowly add 150mL of deionized water;

[0034] (4) Following step (3), the reaction system was heated to 98°C and poured into 200 mL of deionized water at 60°C while hot. 5 mL of 30% H2O2 was added dropwise to remove excess KMnO4. The reaction mixture was centrifuged at 6000 rpm and the product was transferred to a forced air drying oven at 60°C for 24 h to dry and reduce to obtain WHBG.

[0035] The biomass porous graphene negative electrode material prepared in Example 2 has a high conductivity at 25 mA g -1 The initial discharge capacity at the current density is 636 mAh g -1 , at 25mA g -1 After 150 cycles, it can still retain 241mAh g -1 , at 1A g -1 Ultra-long cycling was carried out at a current density of 1.5447 W / m2. Compared with the 11th cycle, the capacity retention rate was 78.8%. The potassium ion battery assembled with the WHBG negative electrode material prepared in Example 2 has a stable cycle capacity and can meet application requirements.

[0036] Example 3

[0037] (1) Cut the white radish into 3x3 cm cubes with a thickness of 2 cm, and then soak them in deionized water for 60 min to remove soluble impurities; dry the soaked white radish cubes in a drying oven at 80° C. for 12 h to quickly evaporate the water in the biological cells and form a contracted structure;

[0038] (2) The precursor obtained in step (1) was placed in a tube furnace with an Ar gas atmosphere at 2°C min -1 The temperature was raised to 600℃ at a heating rate and carbonized for 4h. The carbonized precursor was mixed with 5wt.% Fe2O3, and then the temperature was quickly raised to 2200℃ in a hot press furnace at 1.15MPa and kept for 1h to finally obtain a biomass graphite precursor.

[0039] (3) Take 0.6g of the biomass graphite precursor obtained in step (2), mix it with 1.0g of NaNO3, add it to a beaker, and slowly add 50mL of H2SO4, and stir for 1h. Place the mixed beaker in an ice bath, slowly add 3.0g of KMnO4, and stir for 2h. Then heat the water bath to 35°C, stir for 30min, and then slowly add 150mL of deionized water;

[0040] (4) Following step (3), the reaction system was heated to 98°C and poured into 200 mL of deionized water at 60°C while hot. 5 mL of 30% H2O2 was added dropwise to remove excess KMnO4. The reaction mixture was centrifuged at 6000 rpm and the product was transferred to a forced air drying oven at 60°C for 24 h to dry and reduce to obtain WHBG.

[0041] The biomass porous graphene negative electrode material prepared in Example 3 has a high conductivity at 25 mA g -1 The initial discharge capacity at the current density is 945 mAh g -1 , at 25mA g -1 After 150 cycles, it can still retain 356mAh g -1 , at 1A g -1 Ultra-long cycles were carried out at a current density of 1.5447 W / m, and compared with the 11th cycle, the capacity retention rate was 83.9%. The potassium ion battery assembled with the WHBG negative electrode material prepared in Example 3 has a stable cycle capacity and can meet application requirements.

[0042] Example 4

[0043] (1) Cut the white radish into 2x2 cm cubes with a thickness of 2 cm, and then soak them in deionized water for 60 min to remove soluble impurities; dry the soaked white radish cubes in a drying oven at 80° C. for 12 h, so that the water in the biological cells can evaporate quickly to form a contracted structure;

[0044] (2) The precursor obtained in step (1) was placed in a tube furnace with an Ar gas atmosphere at 2°C min -1 The temperature was raised to 600℃ at a heating rate and carbonized for 4h. The carbonized precursor was mixed with 8wt.% Fe2O3, and then the temperature was quickly raised to 2200℃ in a hot press furnace at 1.15MPa and kept for 1h to finally obtain a biomass graphite precursor.

[0045] (3) Take 0.6g of the biomass graphite precursor obtained in step (2), mix it with 1.0g of NaNO3, add it to a beaker, and slowly add 50mL of H2SO4, and stir for 1h. Place the mixed beaker in an ice bath, slowly add 3.0g of KMnO4, and stir for 2h. Then heat the water bath to 35°C, stir for 30min, and then slowly add 150mL of deionized water;

[0046] (4) Following step (3), the reaction system was heated to 98°C and poured into 200 mL of deionized water at 60°C while hot. 5 mL of H2O2 was added dropwise to remove excess KMnO4. The reaction mixture was centrifuged at 6000 rpm and the product was transferred to a forced air drying oven at 60°C for 24 h to obtain WHBG.

[0047] The biomass porous graphene negative electrode material prepared in Example 4 has a high conductivity at 25 mA g -1 The initial discharge capacity at the current density is 1464 mAh g -1 , at 25mA g -1 After 150 cycles, it can still retain 410mAh g -1 , at 1A g -1 Ultra-long cycles were carried out at a current density of 1.504 × 10·m3 / s. Compared with the 11th cycle, the capacity retention rate was 93.5%. The potassium ion battery assembled with the WHBG negative electrode material prepared in Example 4 has a stable cycle capacity and can meet application requirements.

[0048] Example 5

[0049] (1) Cut the white radish into 4x4 cm cubes with a thickness of 1 cm, and then soak them in deionized water for 60 min to remove soluble impurities; dry the soaked white radish cubes in a drying oven at 80° C. for 12 h, so that the water in the biological cells can evaporate quickly to form a contracted structure;

[0050] (2) The precursor obtained in step (1) was placed in a tube furnace with an Ar gas atmosphere at 2°C min -1 The temperature was raised to 600℃ at a heating rate and carbonized for 4h. The carbonized precursor was mixed with 10wt.% Fe2O3, and then the temperature was quickly raised to 2200℃ in a hot press furnace at 1.15MPa and kept for 1h to finally obtain a biomass graphite precursor.

[0051] (3) Take 0.6g of the biomass graphite precursor obtained in step (2), mix it with 1.0g of NaNO3, add it to a beaker, and slowly add 50mL of H2SO4, and stir for 1h. Place the mixed beaker in an ice bath, slowly add 3.0g of KMnO4, and stir for 2h. Then heat the water bath to 35°C, stir for 30min, and then slowly add 150mL of deionized water;

[0052] (4) Following step (3), the reaction system was heated to 98°C and poured into 200 mL of deionized water at 60°C while hot. 5 mL of 30% H2O2 was added dropwise to remove excess KMnO4. The reaction mixture was centrifuged at 6000 rpm and the product was transferred to a forced air drying oven at 60°C for 24 h to dry and reduce to obtain WHBG.

[0053] The biomass porous graphene negative electrode material prepared in Example 5 has a high conductivity at 25 mA g -1 The initial discharge capacity at the current density is 1167 mAh g -1 , at 25mA g -1 After 150 cycles, 372 mAh g -1 , at 1A g -1 Ultra-long cycles were carried out at a current density of 1.5447 W / m, and the capacity retention rate was 82.6% compared with the 11th cycle. The potassium ion battery assembled with the WHBG negative electrode material prepared in Example 5 has a stable cycle capacity and can meet application requirements.

[0054] Although the present invention has been described in detail above by general description and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements can be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all belong to the scope of protection claimed by the present invention.

Claims

1. A method for preparing a novel biomass porous graphene potassium ion battery negative electrode material, characterized in that: The preparation method of the negative electrode material of the potassium ion battery comprises the following steps: S1, first cutting the white radish into small cubes, then soaking them in deionized water for pretreatment to remove soluble impurities, and then putting the soaked white radish cubes into a drying oven for drying to ensure that the water in the biological cells can evaporate quickly to form a contracted structure; S2, carbonizing the precursor obtained in step S1 and mixing it with Fe2O3, and then sintering it by vacuum hot pressing to obtain a biomass graphite material; S3, after mixing the biomass graphite obtained in step S2 with NaNO3, slowly add concentrated H2SO4 and stir, then place the mixed solution in an ice bath and add KMnO4, and then heat it in a water bath; S4. Add a small amount of 30% H2O2 to the solution in step S3 to remove excess KMnO4, and finally centrifuge, dry and reduce the mixture to obtain a biomass porous graphene material.

2. The method for preparing a novel biomass porous graphene potassium ion battery negative electrode material according to claim 1, characterized in that: The size of the white radish pieces is 2x2 cm-4x4 cm, the thickness is 1-2 cm, the deionized water soaking time is 30-120 min, the drying temperature is 80°C-120°C, and the insulation time is 12-24 h.

3. The method for preparing a novel biomass porous graphene potassium ion battery negative electrode material according to claim 1, characterized in that: In step S2, the carbonization temperature is 400-600°C, the carbonization atmosphere is one of argon and nitrogen, and the heating rate is 2-5°C min -1 , the holding time is 2-6h, the Fe2O3 content is 0.1-10wt.%, the hot pressing furnace pressure is 1-1.5MPa, the hot pressing temperature is 2000-2400℃, and the holding time is 1-2h.

4. The method for preparing a novel biomass porous graphene potassium ion battery negative electrode material according to claim 1, characterized in that: In step S3, the mass ratio of biomass graphite and NaNO3 is 0.5:1-1:1, the volume of concentrated H2SO4 is 30-60mL, the stirring time is 1-2h, the KMnO4 content is 2-4g, the water bath temperature is 35-100℃, and the stirring time is 30-60min.

5. The method for preparing a novel biomass porous graphene potassium ion battery negative electrode material according to claim 1, characterized in that: In step S4, the concentration of H2O2 is 30-70%, the centrifuge speed is 6000-10000 rpm, the drying temperature is 60-100°C, and the drying time is 12-24 hours.

Citation Information

Patent Citations

  • Porous metal-doped carbon composite material, and preparation method and application thereof

    CN108963207A