Preparation method of high-dispersion submicron rutile type titanium dioxide microspheres
By adding acid and amine surfactant to the titanium sulfate solution, combined with hydrothermal reaction and doping regulation, rutile-type titanium dioxide microspheres with narrow particle size and high spherical shape were prepared, which solved the problem of particle size in the sulfuric acid method. The quality of titanium dioxide and blast furnace slag resource utilization have been improved.
Patent Information
- Application Number
- CN202411004457.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
AI Technical Summary
The existing sulfuric acid method produces titanium dioxide with uneven particle size and poor morphology, resulting in low product quality and low blast furnace slag resource utilization, which cannot effectively improve pigment performance.
By adding acid to the titanium sulfate solution, adding amine cationic surfactant, conducting hydrothermal reactions to form highly dispersed hydrated titanium dioxide microspheres, and calcining is regulated by doping to obtain a narrow particle size , rutile-type titanium dioxide microspheres with high spherical shape.
The production of high-quality titanium dioxide is achieved, the pigment performance is improved, the titanium yield and resource utilization is improved, and the production cost is reduced. The resulting titanium dioxide microspheres are not easy to sinter, and have high dispersion and high purity.
Smart Images

Figure HDA0004962596920000011
Abstract
Description
Technical Field
[0001] The present invention relates to the field of materials, and in particular to a method for preparing highly dispersed submicron rutile titanium dioxide microspheres. Background Art
[0002] Titanium dioxide (TiO2), commonly known as titanium dioxide, is the third largest inorganic chemical product after synthetic ammonia and phosphorus chemicals. It has excellent optical properties and is the best white pigment. It is widely used in coatings, plastics, cosmetics and other fields. There are three common phases: anatase, rutile and brookite.
[0003] The production methods of titanium dioxide widely used in industry include sulfuric acid method and chlorination method. The production of titanium dioxide by chlorination method has high requirements for raw materials (quality> 90wt%), and its insufficient source limits its further development. Therefore, for a long time in the future, the sulfuric acid method will still dominate the titanium dioxide industry. The steps of producing titanium dioxide by sulfuric acid method include: sulfuric acid and titanium ore react and dissolve to form a sulfated titanium solution (referred to as titanium liquid), which is heated and hydrolyzed to form a hydrated titanium dioxide precipitate (meta-titanic acid), which is calcined and post-treated to obtain a titanium dioxide product. The advantages of sulfuric acid method are mature technology, simple production equipment, and low requirements for raw materials. It only requires titanium ore with a titanium dioxide taste of> 50wt%, and industrial sulfuric acid with a concentration of> 85wt%. The disadvantage is that due to the limitation of the process, the obtained titanium dioxide is agglomerated and sintered, so the product quality is not high. At present, the comprehensive production capacity of titanium dioxide in my country is sufficient, but there are problems of homogeneity, oversupply of low-end and medium-end products, and insufficient high-end products. Therefore, upgrading the mainstream sulfuric acid method titanium dioxide production process, improving product quality and building brands will be one of the focuses of future industry development.
[0004] The properties of titanium dioxide include whiteness and tinting power, which are related to the purity, particle size, dispersibility and physical phase of titanium dioxide. The white color of titanium dioxide comes from the scattering of visible light. When the particle size is around 230nm, the particle size distribution is narrow, the particle sphericity is high, and the physical phase is rutile, the light scattering is the strongest, and it has the best whiteness and tinting power. The color-developing impurities in titanium dioxide will make titanium dioxide appear colored and reduce its whiteness. Therefore, the industry has very strict requirements on the content of color-developing impurities in titanium dioxide, which generally cannot be higher than 30ppm. At present, there is a mature solution reduction method for purity control in the production of sulfuric acid titanium dioxide, and there is also a mature doping process for phase control. If you want to further improve the performance of the pigment, the key is to regulate the particle size distribution and morphology of titanium dioxide. Most of the regulation methods are optimized for a certain process of the sulfuric acid method, mainly including the hydrolysis of titanyl sulfate solution and the calcination of metatitanic acid. Summary of the invention
[0005] The inventors found that the synthesis of high-quality sulfuric acid titanium dioxide in the prior art is mainly based on the optimization of the original production process, which cannot fundamentally overcome the disadvantages of the sulfuric acid method, that is, the metatitanic acid formed in the hydrolysis process is a particle formed by the agglomeration of primary particles, with a large average particle size and a wide particle size distribution, which makes the particle growth speed inconsistent and sintered during calcination, resulting in uneven product particle size and poor morphology. Therefore, the improvement of the performance of the improved process pigment is relatively limited. The spray hydrolysis method overcomes the problem of internal particle agglomeration of metatitanic acid, but spray hydrolysis can only be used for systems with very high purity. For industrial titanium liquids with high impurity content, it may be difficult to ensure that the product impurity content meets the standard.
[0006] Titanium-containing blast furnace slag is a by-product produced during the smelting process of vanadium-titanium magnetite blast furnace. It has a high titanium content (22-25%, TiO2), a low utilization rate (<10%), and a cumulative stockpile of over 80 million tons, with an annual increase of nearly 4 million tons. It is an important secondary titanium resource. Patent CN112047377A discloses a method for preparing high-purity titanium dioxide from titanium-containing blast furnace slag. The method allows 80-95% concentrated sulfuric acid to react with titanium-containing blast furnace slag at a mass ratio of 1.7-2.2:1, an acid hydrolysis temperature of 80-180°C, and a reaction time of 0.5-3 hours. The obtained solid is dissolved in water and filtered to remove silicon and calcium impurities, and a solution containing impurities of titanium oxide sulfate (TiO2: 25-60g / L, MgSO4: 30-50g / L, Al2(SO4)3: 50-80g / L, acid-titanium ratio of 2.2-3.3) is obtained, and the titanium leaching rate reaches 88%, but the obtained titanium dioxide is non-pigment grade and has low value. In order to solve the technical problems in the prior art, the present invention proposes a new method for synthesizing titanium dioxide microspheres based on titanium oxide sulfate solution. The method is based on the utilization of titanium-containing blast furnace slag, and the impurities of titanium oxide sulfate solution prepared therefrom are used as raw materials. The acid-titanium ratio is increased by adding acid to the solution to promote dissolution and deposition, the particle agglomeration is hindered by adsorption of amine cationic surfactants, and the reaction is accelerated by hydrothermal hydrolysis to make the titanium yield greater than 98%, thereby obtaining hydrated titanium dioxide microspheres (270-345±40-66nm). The obtained hydrated titanium dioxide microspheres are filtered and washed, and the phase change and dispersibility of titanium dioxide during calcination are regulated by doping, and calcined at 750-950°C for 2-8h to obtain rutile titanium dioxide microspheres (219-296±33-57nm, TiO2>98wt%, rutile ratio>96%). The method is based on waste utilization and high titanium yield. At the same time, the obtained titanium dioxide microspheres have narrow particle size distribution, high sphericity, and are not easy to sinter, which is conducive to the production of high-quality titanium dioxide and high-value resource utilization of titanium-containing blast furnace slag.
[0007] In a first aspect of the present invention, the present invention provides a method for preparing rutile titanium dioxide microspheres. According to an embodiment of the present invention, the method comprises:
[0008] 1) performing an acid treatment and a first mixing treatment on a solution containing heterosulfate titanyl to obtain a solution 1;
[0009] 2) adding an amine cationic surfactant to the solution 1, and performing a second mixing treatment to obtain a solution 2;
[0010] 3) subjecting the solution 2 to a hydrothermal reaction to obtain hydrated titanium dioxide microspheres;
[0011] 4) calcining the hydrated titanium dioxide microspheres to obtain the rutile titanium dioxide microspheres.
[0012] According to the method of the embodiment of the present invention, first, acid is added to the solution containing miscellaneous sulfuric acid titanium oxide and stirred to obtain a solution 1 with a high acid-titanium ratio, which can promote the dissolution and deposition of hydrated titanium dioxide and adjust the shape. Since the spherical surface energy is the smallest, hydrated titanium dioxide microspheres are finally formed; secondly, an amine cationic surfactant is added to solution 1 and stirred to obtain solution 2, so as to achieve surface modification of primary particles and control their agglomeration, thereby ensuring the monodispersity of hydrated titanium dioxide microspheres (270-345±40-66nm); further, the high temperature environment of the hydrothermal reaction is used to promote the hydrolysis of titanyl sulfate in the solution, thereby ensuring a high titanium hydrolysis rate (>98%). After washing the hydrated titanium dioxide, doping is used to regulate the phase and dispersibility of titanium dioxide, and rutile titanium dioxide microspheres (219-296±33-57nm, TiO2>98wt%, rutile ratio>96%) are obtained after roasting. Therefore, the preparation method of highly dispersed submicron rutile titanium dioxide microspheres of the present invention is based on the utilization of titanium-containing blast furnace slag and has a high titanium yield, which is beneficial to reducing costs and resource recycling. In addition, the obtained rutile titanium dioxide microspheres have a narrow particle size distribution, high sphericity, and are not easy to sinter, which can improve the pigment properties of titanium dioxide, thereby being beneficial to the production of high-quality titanium dioxide and the high-value resource utilization of titanium-containing blast furnace slag.
[0013] According to an embodiment of the present invention, the above method may further include at least one of the following additional technical features:
[0014] According to an embodiment of the present invention, the assorted sulfate-containing titanyl solution comprises 25-60 g / L TiO2, 30-50 g / L MgSO4 and 50-80 g / L Al2(SO4)3. According to an embodiment of the invention, the assorted sulfate-containing titanyl solution is a solution obtained by acid decomposing and dissolving titanium-containing blast furnace slag in water, which can be obtained according to Chinese patent application CN112047377A.
[0015] According to an embodiment of the present invention, the acid-titanium ratio of the heterosulfate-containing titanyl solution is 2.2-3.3.
[0016] According to an embodiment of the present invention, the acid-titanium ratio of the solution after the acid treatment is 3.5-6.5. The inventors found that within this acid-titanium ratio range, the dissolution and deposition of hydrated titanium dioxide during the hydrothermal reaction can be promoted, thereby promoting the formation of microspheres.
[0017] According to an embodiment of the present invention, the acid added in the acid treatment is sulfuric acid or hydrochloric acid.
[0018] According to an embodiment of the present invention, the concentration of the sulfuric acid is 98 wt %.
[0019] According to an embodiment of the present invention, the concentration of the hydrochloric acid is 36 wt %.
[0020] According to an embodiment of the present invention, the first mixing process is performed at room temperature.
[0021] According to an embodiment of the present invention, the first mixing process is performed by stirring at a speed of 300 rpm for 2 hours.
[0022] According to an embodiment of the present invention, the amine cationic surfactant includes at least one of ethylenediamine, triethanolamine, dodecylamine, tetramethylammonium bromide, and hexadecyltrimethylammonium bromide. According to an embodiment of the present invention, the agglomeration of primary particles is controlled by directional adsorption / coordination of the surfactant with the primary particles, thereby improving the dispersibility of water and titanium dioxide.
[0023] According to an embodiment of the present invention, the concentration of the amine cationic surfactant is 0.005-0.15 wt %.
[0024] According to an embodiment of the present invention, the second mixing process is performed at room temperature.
[0025] According to an embodiment of the present invention, the second mixing process is performed by stirring at a speed of 300 rpm for 2 hours.
[0026] According to an embodiment of the present invention, the temperature of the hydrothermal reaction is 110-180° C. According to an embodiment of the present invention, a high-temperature hydrothermal environment is utilized to promote the hydrolysis of titanyl sulfate and achieve a high titanium hydrolysis rate.
[0027] According to an embodiment of the present invention, the hydrothermal reaction time is 1-10 hours. According to an embodiment of the present invention, within this time range, the hydrolysis of titanyl sulfate is promoted to achieve a high titanium hydrolysis rate.
[0028] According to an embodiment of the present invention, the method further comprises washing the hydrated titanium dioxide microspheres before calcining the hydrated titanium dioxide microspheres.
[0029] According to an embodiment of the present invention, the washing treatment is performed by washing twice with 5% dilute sulfuric acid and then washing twice with clean water.
[0030] According to an embodiment of the present invention, the amount of the dilute sulfuric acid is at least 30 ml per gram of hydrated titanium dioxide.
[0031] According to an embodiment of the present invention, the amount of clean water used is at least 30 ml per gram of hydrated titanium dioxide.
[0032] According to an embodiment of the present invention, the washing process is repeated 3 times.
[0033] According to an embodiment of the present invention, the calcination treatment is carried out by adding calcination seeds. It should be noted that calcination seeds are commonly used additives in the calcination process of sulfuric acid titanium dioxide production, which are rutile titanium dioxide microcrystals of tens of nanometers, used to promote the phase change of anatase titanium dioxide during high-temperature calcination. The preparation technology of calcination seeds is mature, and the titanate method is commonly used in industry. The steps for preparing calcination seeds by the titanate method can be referred to "Titanium Dioxide Production Technology Questions and Answers" (Chen Chaohua, 1998.04, Chemical Industry Press), which are mainly: metatitanic acid reacts with titanium hydroxide solution to form sodium metatitanate, which is filtered and washed and then treated with hydrochloric acid to adjust the pH, and the calcination seed colloidal solution is obtained after dilution.
[0034] According to an embodiment of the present invention, the doping ratio is calculated based on the metal oxide of the element, and titanium dioxide: calcined crystal seed: potassium salt: phosphate salt: aluminum salt is 100:6:0.6:0.1:0.3. According to an embodiment of the present invention, the doping ratio (calcined crystal seed: potassium salt (K2CO3): phosphate salt (H3PO4): aluminum salt (AlCl3) = 100:6:0.6:0.1:0.3. As a result, the phase change of titanium dioxide during calcination can be promoted, sintering can be reduced, and the dispersion and phase of the titanium dioxide product can be ensured.
[0035] According to an embodiment of the present invention, the temperature of the calcination treatment is 750-950°C. The inventors have found that within this temperature range, the transformation of titanium dioxide from anatase to rutile can be achieved with almost no sintering. Too low a temperature will lead to a reduced phase transition rate and insufficient rutile conversion rate; too high a temperature will lead to sintering and agglomeration of titanium dioxide grains, resulting in reduced dispersibility.
[0036] According to an embodiment of the present invention, the calcination treatment time is 2-8 hours.
[0037] In another aspect of the present invention, the present invention provides a method for preparing rutile titanium dioxide microspheres. According to an embodiment of the present invention, the method comprises:
[0038] S100: adding acid to the solution containing titanyl sulfate to increase the acid-titanium ratio of the solution, and stirring to obtain solution 1.
[0039] According to an embodiment of the present invention, in this step, by adding acid to the mixed sulfate-containing titanyl solution and stirring, the acid-titanium ratio of the solution is increased to obtain a mixed sulfate-containing titanyl solution with a high acid-titanium ratio. The high concentration of acid can promote the dissolution and deposition of titanium dioxide in the hydrothermal reaction, so that the obtained hydrated titanium dioxide is spherical.
[0040] According to an embodiment of the present invention, the composition of the titanium oxysulfate solution is: TiO2: 25-60 g / L, MgSO4: 30-50 g / L, Al2(SO4)3: 50-80 g / L, and the acid-titanium ratio is 2.2-3.3.
[0041] According to an embodiment of the present invention, the acid added to the solution is 98 wt % sulfuric acid or 36 wt % hydrochloric acid.
[0042] According to an embodiment of the present invention, the acid-titanium ratio of the solution needs to be increased to 3.5-6.5 after adding acid.
[0043] According to an embodiment of the present invention, stirring is performed at a rate of 300 rpm for 2 hours at room temperature.
[0044] According to an embodiment of the present invention, the method further comprises:
[0045] S200: adding an amine cationic surfactant to solution 1, and stirring to obtain solution 2.
[0046] According to an embodiment of the present invention, in this step, an amine-type cationic surfactant is added to the solution containing heterosulfate titanium dioxide and stirred. During the hydrolysis process, the surfactant reacts with the primary particles of hydrated titanium dioxide to form adsorption / coordination, thereby controlling the agglomeration of the primary particles during the hydrothermal reaction, achieving improved dispersibility, and thus obtaining highly dispersed hydrated titanium dioxide microspheres.
[0047] According to an embodiment of the present invention, the concentration of the added amine cationic surfactant in the solution is 0.005-0.15 wt %.
[0048] According to an embodiment of the present invention, the amine-based cationic surfactant includes at least one of ethylenediamine, triethanolamine, dodecylamine, tetramethylammonium bromide, and hexadecyltrimethylammonium bromide.
[0049] According to an embodiment of the present invention, stirring is performed at a rate of 300 rpm for 2 hours at room temperature.
[0050] According to an embodiment of the present invention, the method further comprises:
[0051] S300: placing solution 2 in a hydrothermal reactor and sealing it, and performing a hydrothermal reaction to obtain a precipitate of hydrated titanium dioxide microspheres.
[0052] According to an embodiment of the present invention, in this step, the high temperature environment of the hydrothermal reaction is utilized to accelerate the hydrolysis of titanyl sulfate in the solution, thereby ensuring a high titanium hydrolysis rate, shortening the hydrolysis time and improving efficiency.
[0053] According to an embodiment of the present invention, the hydrothermal reaction is carried out at 110-180° C. for 1-10 h.
[0054] According to an embodiment of the present invention, the method further comprises:
[0055] S400: After filtering, washing, and doping, water and titanium dioxide microspheres are calcined to obtain rutile titanium dioxide microspheres.
[0056] According to an embodiment of the present invention, in this step, doping and calcination are utilized to promote the rutile conversion of the titanium dioxide microspheres, while controlling the sintering thereof to ensure the physical phase and dispersibility of the final product.
[0057] According to an embodiment of the present invention, the hydrated titanium dioxide needs to be washed twice with at least 30 ml (per gram of hydrated titanium dioxide) of 5% dilute sulfuric acid, and then washed twice with at least 30 ml (per gram of hydrated titanium dioxide) of clean water.
[0058] According to an embodiment of the present invention, the doping ratio (in terms of metal oxides of elements) is titanium dioxide: calcined seed crystals: potassium salt (K2CO3): phosphate salt (H3PO4): aluminum salt (AlCl3) = 100:6:0.6:0.1:0.3.
[0059] According to an embodiment of the present invention, the calcination of the hydrated titanium dioxide is carried out at 750-950° C. for 2-8 hours.
[0060] In another aspect of the present invention, the present invention also provides a rutile titanium dioxide microsphere. The rutile titanium dioxide microsphere according to the embodiment of the present invention is prepared according to the method described above. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0062] Figure 1 This is a scanning electron microscope photograph of the highly dispersed submicron rutile titanium dioxide microspheres (130°C, reaction 8h) / titanium dioxide microspheres (850°C, calcination 4h) prepared in Example 1 and its particle size distribution diagram (obtained by counting the diameters of 200 particles in the scanning electron microscope photograph). DETAILED DESCRIPTION
[0063] The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but should not be construed as limiting the present invention.
[0064] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0065] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.
[0066] Example 1
[0067] 1) The composition of the raw material titanium dioxide solution containing miscellaneous sulfates is: TiO2: 46 g / L, MgSO4: 43 g / L, Al2(SO4)3: 66 g / L, and the acid-titanium ratio is 2.8. 98 wt% sulfuric acid is added to the solution to increase the acid-titanium ratio of the solution to 3.5, and the solution is stirred at 300 rpm for 2 hours at room temperature to obtain solution 1.
[0068] 2) Add ethylenediamine to solution 1 to a concentration of 0.02 wt %, and stir at 300 rpm for 2 h at room temperature to obtain solution 2.
[0069] 3) Solution 2 was sealed in a hydrothermal reactor and subjected to hydrothermal reaction at 130° C. for 8 h to obtain hydrated titanium dioxide microspheres with a particle size distribution of 270±40 nm and a titanium hydrolysis rate of 98.5%.
[0070] 4) Filter the hydrated titanium dioxide, wash it twice with 5% dilute sulfuric acid and clean water respectively, at least 30 ml each time (per gram of hydrated titanium dioxide), and dope it according to the ratio of titanium dioxide: calcined seed: potassium salt (K2CO3): phosphate salt (H3PO4): aluminum salt (AlCl3) = 100:6:0.6:0.1:0.3, and calcine it at 850°C for 4h to obtain rutile titanium dioxide microspheres (219±33nm, TiO2 purity 98.6wt%, rutile ratio 96.5%). The scanning electron microscope photos of the rutile titanium dioxide microspheres (130°C, reaction 8h) / titanium dioxide microspheres (850°C, 4h calcination) and their particle size distribution diagram (obtained by counting the diameters of 200 particles in the scanning electron microscope photos) are shown in Figure 1 .
[0071] Example 2
[0072] 1) The composition of the raw material titanium dioxide solution containing miscellaneous sulfates is: TiO2: 60 g / L, MgSO4: 49 g / L, Al2(SO4)3: 77 g / L, and the acid-titanium ratio is 2.4. 98 wt% sulfuric acid is added to the solution to increase the acid-titanium ratio of the solution to 6.5, and the solution is stirred at 300 rpm for 2 hours at room temperature to obtain solution 1.
[0073] 2) Add triethanolamine to solution 1 to a concentration of 0.1 wt %, and stir at 300 rpm for 2 h at room temperature to obtain solution 2.
[0074] 3) Solution 2 was sealed in a hydrothermal reactor and subjected to hydrothermal reaction at 180° C. for 4 h to obtain hydrated titanium dioxide microspheres with a particle size distribution of 285±44 nm and a titanium hydrolysis rate of 98.2%.
[0075] 4) Filter the hydrated titanium dioxide, wash it twice with 5% dilute sulfuric acid and clean water, at least 30 ml each time (per gram of hydrated titanium dioxide), and dope it in the ratio of titanium dioxide: calcined seed: potassium salt (K2CO3): phosphate salt (H3PO4): aluminum salt (AlCl3) = 100:6:0.6:0.1:0.3, and calcine it at 850°C for 4h to obtain rutile titanium dioxide microspheres (234±38nm, TiO2 purity 98.8wt%, rutile ratio 96.8%).
[0076] Example 3
[0077] 1) The composition of the raw material titanium dioxide sulfate solution is: TiO2: 25 g / L, MgSO4: 32 g / L, Al2(SO4)3: 55 g / L, and the acid-titanium ratio is 3.4. 36% wt% hydrochloric acid is added to the solution to increase the acid-titanium ratio of the solution to 4.5, and the solution is stirred at 300 rpm for 2 hours at room temperature to obtain solution 1.
[0078] 2) Add a mixture of dodecylamine and hexadecyltrimethylammonium bromide (mass ratio 1:1) to solution 1 to a concentration of 0.005 wt %, and stir at 300 rpm for 2 h at room temperature to obtain solution 2.
[0079] 3) Solution 2 was sealed in a hydrothermal reactor and subjected to hydrothermal reaction at 160° C. for 5 h to obtain hydrated titanium dioxide microspheres with a particle size distribution of 275±42 nm and a titanium hydrolysis rate of 99.4%.
[0080] 4) Filter the hydrated titanium dioxide, wash it twice with 5% dilute sulfuric acid and clean water, at least 30 ml each time (per gram of hydrated titanium dioxide), and dope it in the ratio of titanium dioxide: calcined seed: potassium salt (K2CO3): phosphate salt (H3PO4): aluminum salt (AlCl3) = 100:6:0.6:0.1:0.3, and calcine it at 750°C for 8h to obtain rutile titanium dioxide microspheres (236±34nm, TiO2 purity 98.1wt%, rutile ratio 96.0%).
[0081] Example 4
[0082] 1) The composition of the raw material titanium dioxide solution containing miscellaneous sulfates is: TiO2: 55 g / L, MgSO4: 47 g / L, Al2(SO4)3: 72 g / L, and the acid-titanium ratio is 2.4. 98 wt% sulfuric acid is added to the solution to increase the acid-titanium ratio of the solution to 4.5, and the solution is stirred at 300 rpm for 2 hours at room temperature to obtain solution 1.
[0083] 2) Add a mixture of dodecylamine and tetramethylammonium bromide (mass ratio 1:1) to solution 1 to make its concentration 0.08 wt %, and stir at 300 rpm for 2 h at room temperature to obtain solution 2.
[0084] 3) Solution 2 was placed in a sealed hydrothermal reactor and subjected to hydrothermal reaction at 180° C. for 2 h to obtain hydrated titanium dioxide microspheres with a particle size distribution of 322±40 nm and a titanium hydrolysis rate of 99.5%.
[0085] 4) Filter the hydrated titanium dioxide, wash it twice with 5% dilute sulfuric acid and clean water, at least 30 ml each time (per gram of hydrated titanium dioxide), and dope it in the ratio of titanium dioxide: calcined seed: potassium salt (K2CO3): phosphate salt (H3PO4): aluminum salt (AlCl3) = 100:6:0.6:0.1:0.3, and calcine it at 950°C for 2h to obtain rutile titanium dioxide microspheres (277±48nm, TiO2 purity 98.2wt%, rutile ratio 99.2%).
[0086] Example 5
[0087] 1) The composition of the raw material titanium dioxide solution containing miscellaneous sulfates is: TiO2: 43 g / L, MgSO4: 36 g / L, Al2(SO4)3: 59 g / L, and the acid-titanium ratio is 3.0. 98 wt% sulfuric acid is added to the solution to increase the acid-titanium ratio of the solution to 4.5, and the solution is stirred at 300 rpm for 2 hours at room temperature to obtain solution 1.
[0088] 2) Add hexadecyltrimethylammonium bromide and triethanolamine (mass ratio 1:1) to solution 1 to make its concentration 0.08 wt %, and stir at 300 rpm for 2 h at room temperature to obtain solution 2.
[0089] 3) Solution 2 was placed in a sealed hydrothermal reactor and subjected to hydrothermal reaction at 180° C. for 2 h to obtain hydrated titanium dioxide microspheres with a particle size distribution of 345±66 nm and a titanium hydrolysis rate of 99.5%.
[0090] 4) Filter the hydrated titanium dioxide, wash it twice with 5% dilute sulfuric acid and clean water, at least 30 ml each time (per gram of hydrated titanium dioxide), and dope it in the ratio of titanium dioxide: calcined seed: potassium salt (K2CO3): phosphate salt (H3PO4): aluminum salt (AlCl3) = 100:6:0.6:0.1:0.3, and calcine it at 950°C for 2h to obtain rutile titanium dioxide microspheres (296±57nm, TiO2 purity 98.1wt%, rutile ratio 98.8%).
[0091] Example 6
[0092] 1) The composition of the raw material titanium sulfate solution is: TiO2: 43 g / L, MgSO4: 36 g / L, Al2(SO4)3: 59 g / L, the acid-titanium ratio is 3.0, hexadecyltrimethylammonium bromide and triethanolamine (mass ratio 1:1) are added to make its concentration 0.08 wt%, and stirred at 300 rpm at room temperature for 2 h to obtain solution 1.
[0093] 2) Solution 1 was placed in a sealed hydrothermal kettle and subjected to hydrothermal reaction at 180° C. for 2 h to obtain hydrated titanium dioxide agglomerated particles with a particle size distribution of 1530±570 nm and a titanium hydrolysis rate of 99.7%.
[0094] 3) Filter the hydrated titanium dioxide, wash it twice with 5% dilute sulfuric acid and clean water, at least 30 ml each time (per gram of hydrated titanium dioxide), and dope it in the ratio of titanium dioxide: calcined seed: potassium salt (K2CO3): phosphate salt (H3PO4): aluminum salt (AlCl3) = 100:6:0.6:0.1:0.3, and calcine it at 950°C for 2h to obtain sintered rutile titanium dioxide (428±178nm, TiO2 purity 96.2wt%, rutile ratio 95.2%).
[0095] Example 7
[0096] 1) The composition of the raw material titanium dioxide solution containing miscellaneous sulfates is: TiO2: 43 g / L, MgSO4: 36 g / L, Al2(SO4)3: 59 g / L, and the acid-titanium ratio is 3.0. 98 wt% sulfuric acid is added to the solution to increase the acid-titanium ratio of the solution to 4.5, and the solution is stirred at 300 rpm for 2 hours at room temperature to obtain solution 1.
[0097] 2) Solution 2 was sealed in a hydrothermal kettle and subjected to hydrothermal reaction at 180° C. for 2 h to obtain hydrated titanium dioxide agglomerated particles with a particle size distribution of 2350±790 nm and a titanium hydrolysis rate of 98.2%.
[0098] 3) Filter the hydrated titanium dioxide, wash it twice with 5% dilute sulfuric acid and clean water, at least 30 ml each time (per gram of hydrated titanium dioxide), and dope it in the ratio of titanium dioxide: calcined seed: potassium salt (K2CO3): phosphate salt (H3PO4): aluminum salt (AlCl3) = 100:6:0.6:0.1:0.3, and calcine it at 950°C for 2h to obtain sintered rutile titanium dioxide (873±355nm, TiO2 purity 96.7wt%, rutile ratio 96.4%).
[0099] Example 8
[0100] 1) The composition of the raw material titanium dioxide solution containing miscellaneous sulfates is: TiO2: 43 g / L, MgSO4: 36 g / L, Al2(SO4)3: 59 g / L, and the acid-titanium ratio is 3.0. 98 wt% sulfuric acid is added to the solution to increase the acid-titanium ratio of the solution to 4.5, and the solution is stirred at 300 rpm for 2 hours at room temperature to obtain solution 1.
[0101] 2) Sodium dodecylbenzene sulfonate was added to solution 1 to a concentration of 0.08 wt %, and the mixture was stirred at 300 rpm for 2 h at room temperature to obtain solution 2.
[0102] 3) Solution 2 was sealed in a hydrothermal kettle and subjected to hydrothermal reaction at 180° C. for 2 h to obtain hydrated titanium dioxide agglomerated particles with a particle size distribution of 2030±710 nm and a titanium hydrolysis rate of 97.8%.
[0103] 4) Filter the hydrated titanium dioxide, wash it twice with 5% dilute sulfuric acid and clean water, at least 30 ml each time (per gram of hydrated titanium dioxide), and dope it in the ratio of titanium dioxide: calcined seed: potassium salt (K2CO3): phosphate salt (H3PO4): aluminum salt (AlCl3) = 100:6:0.6:0.1:0.3, and calcine it at 950°C for 2h to obtain sintered rutile titanium dioxide (824±330nm, TiO2 purity 98.0wt%, rutile ratio 97.2%).
[0104] It can be seen from Examples 1-5 that the titanium hydrolysis rate of the heterosulfate-containing titanyl solution is high (>98%), and the final hydrated titanium dioxide microspheres (270-345±40-66nm) and rutile submicron titanium dioxide microspheres (219-296±33-57nm) have a narrow particle size distribution, high purity (TiO2>98wt%), rutile ratio>96%, and high sphericity, and are not easy to sinter.
[0105] It can be seen from Example 6 that without adding acid to increase the acid-titanium ratio, the particle size distribution of the prepared rutile titanium dioxide is too high, the purity is low, and the rutile ratio is too high.
[0106] It can be seen from Example 7 that without adding a cationic surfactant, the particle size distribution of the prepared rutile titanium dioxide is very high.
[0107] It can be seen from Example 8 that the particle size distribution of the rutile titanium dioxide prepared by adding a non-amine cationic surfactant is very high.
[0108] It can be seen that the preparation method of highly dispersed submicron rutile titanium dioxide microspheres of the present invention is not only based on waste utilization and high titanium yield, which is beneficial to reducing costs and resource recycling, but also the obtained titanium dioxide microspheres have a narrow particle size distribution, high sphericity, and are not easy to sinter, which can improve the pigment properties of titanium dioxide, thereby being beneficial to the production of high-quality titanium dioxide and the high-value resource utilization of titanium-containing blast furnace slag.
[0109] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0110] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing rutile titanium dioxide microspheres, characterized in that: include: 1) performing an acid treatment and a first mixing treatment on a solution containing heterosulfate titanyl to obtain a solution 1; 2) adding an amine cationic surfactant to the solution 1, and performing a second mixing treatment to obtain a solution 2; 3) subjecting the solution 2 to a hydrothermal reaction to obtain hydrated titanium dioxide microspheres; 4) calcining the hydrated titanium dioxide microspheres to obtain the rutile titanium dioxide microspheres.
2. The method according to claim 1, characterized in that The titanium dioxide solution containing heterosulfate comprises 25-60 g / L of TiO2, 30-50 g / L of MgSO4 and 50-80 g / L of Al2(SO4)3; Optionally, the acid-titanium ratio of the heterosulfate-containing titanyl solution is 2.2-3.3; Optionally, the acid-to-titanium ratio of the solution after the acid treatment is 3.5-6.5; Optionally, the acid added in the acid treatment is sulfuric acid or hydrochloric acid; Optionally, the concentration of the sulfuric acid is 98wt%; Optionally, the concentration of the hydrochloric acid is 36 wt %.
3. The method according to claim 1, characterized in that The first mixing process is carried out at room temperature; Optionally, the first mixing process is performed by stirring at a rate of 300 rpm for 2 hours.
4. The method according to claim 1, characterized in that: The amine cationic surfactant includes at least one of ethylenediamine, triethanolamine, dodecylamine, tetramethylammonium bromide, and hexadecyltrimethylammonium bromide; Optionally, the concentration of the amine cationic surfactant is 0.005-0.15 wt %.
5. The method according to claim 1, characterized in that The second mixing process is carried out at room temperature; Optionally, the second mixing treatment is performed by stirring at a speed of 300 rpm for 2 hours.
6. The method according to claim 1, characterized in that The temperature of the hydrothermal reaction is 110-180°C; Optionally, the hydrothermal reaction time is 1-10 h.
7. The method according to claim 1, characterized in that The method further comprises washing the hydrated titanium dioxide microspheres before calcining the hydrated titanium dioxide microspheres; Optionally, the washing treatment is carried out by washing twice with 5% dilute sulfuric acid and then washing twice with clean water; Optionally, the amount of dilute sulfuric acid is at least 30 ml per gram of hydrated titanium dioxide; Optionally, the amount of clean water is at least 30 ml per gram of hydrated titanium dioxide; Optionally, the washing treatment is repeated 3 times.
8. The method according to claim 1, characterized in that The calcination treatment is carried out by adding calcination seeds; Optionally, the doping ratio is calculated based on the metal oxide of the element, titanium dioxide: calcined seed crystal: potassium salt: phosphate salt: aluminum salt is 100:6:0.6:0.1:0.
3.
9. The method according to claim 1, characterized in that: The calcination temperature is 750-950°C; Optionally, the calcination treatment time is 2-8 hours.
10. A rutile titanium dioxide microsphere, characterized in that: The rutile titanium dioxide microspheres are prepared according to the method according to any one of claims 1-9.