Bismuth vanadate microbial photo-anode, preparation method thereof, microbial photoelectrolysis tank and wastewater treatment method
By inoculating the bismuth vanadate photoelectrode with Shewanella Oneidensis MR-1 electrochemical bacteria and combining it with a microbial photoelectrolysis cell, the problem of low efficiency in combining the photoelectrode and the bioelectrode was solved, achieving efficient photoelectric conversion and wastewater treatment.
Patent Information
- Application Number
- CN202411157175.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
AI Technical Summary
The low efficiency of combining existing photoelectrodes and bioelectrodes limits the energy conversion efficiency and wastewater degradation efficiency of photoelectrochemical systems, especially in microbial fuel cells where the power density is too low to meet the needs of industrial applications.
Bismuth vanadate microbial photoanodes are used. By inoculating the bismuth vanadate photoelectrode with Shewanella Oneidensis MR-1 electrochemical bacteria, electron-hole pairs are generated using the photocatalytic properties of bismuth vanadate, thereby enhancing electron transfer efficiency. This is combined with a microbial photoelectrolysis cell for wastewater treatment.
It significantly improves photoelectric conversion efficiency and wastewater treatment efficiency, increases current density and stability, extends service life, and achieves more efficient pollutant degradation and energy conversion.
Smart Images

Figure CN118908401A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of bioelectrochemistry and photoelectrochemistry, and specifically relates to a bismuth vanadate microbial photoanode and a preparation method thereof, a microbial photoelectrolysis cell and a wastewater treatment method. Background Art
[0002] Bioelectrochemistry has been extensively studied in terms of different materials, electron transfer mechanisms, cell structures, and optimal operating modes. In particular, in the field of microbial fuel cells (MFCs), electrochemical bacteria can extract electricity directly from biomass in wastewater. However, the power density of MFCs is still too low for industrial applications, which limits their potential for widespread use.
[0003] Combining bioelectrochemistry with photoelectrochemistry is a promising approach, for example, using solar-assisted microbial electrochemical cells (S-MECs). Specifically, S-MFCs using photoactive semiconductors as photoelectrodes can enhance the cathode reaction by increasing the cathode potential under solar radiation.
[0004] Shewanella oneidensis MR-1 (MR-1) is a model electrogenic microorganism in bioelectrochemical research. However, there are still few studies on the combination of bioelectrodes and photoelectrodes. Previous studies have reported the synergistic effect of semiconductor / electrochemical bacteria systems. For example, Qian et al. (Qian, F., Wang, H., Ling, Y., Wang, G., Thelen, MP, & Li, Y. (2014). Photoenhanced electrochemical interaction between Shewanella and a hematite nanowire photoanode. Nano letters, 14(6), 3688-3693.) first reported the use of ferric oxide (Fe2O3) photoelectrodes to show active electron transfer at the semiconductor / cell interface, which is achieved through an outer membrane protein called c-type cytochrome, thereby significantly enhancing the photocurrent under illumination. However, the current density that can be achieved in this study is still not competitive, and the overall design of the system still needs to be redesigned to improve the current density.
[0005] Therefore, although the concept of combining photoelectrodes with bioelectrodes has been proposed, the current efficiency of combining photoelectrodes with bioelectrodes is low. How to efficiently combine photoanodes and microbial anodes to achieve optimal energy conversion efficiency in practical applications is still an important research topic, and the current combination strategy has not yet been able to fully optimize the overall performance of the system. In addition, the stability, light capture efficiency, and interfacial electron transfer efficiency of the anode material need to be improved. These factors limit the long-term performance and practical application effects of the photoelectrochemical system.
[0006] Therefore, how to obtain a photoanode material that has a high degree of compatibility with microorganisms, good performance, and can be applied to photoelectrochemical wastewater degradation still requires further research. Summary of the invention
[0007] In order to solve the above technical problems, the purpose of the present invention is to provide a bismuth vanadate microbial photoanode and its preparation method, a microbial photoelectrolysis cell and a wastewater treatment method. By effectively combining the bismuth vanadate photoelectrode with specific electrochemical bacteria, the electron transfer efficiency can be improved, and the current density and wastewater degradation efficiency can be higher.
[0008] To achieve the above-mentioned purpose, the present invention provides a bismuth vanadate microbial photoanode, wherein the bismuth vanadate microbial photoanode comprises a bismuth vanadate photoelectrode and electrochemical bacteria; the bismuth vanadate photoelectrode comprises a substrate and a bismuth vanadate layer; the electrochemical bacteria are inoculated on the bismuth vanadate layer; and the electrochemical bacteria are Shewanella Oneidensis MR-1.
[0009] In the present invention, under natural light or artificial light, after bismuth vanadate is combined with electrochemical bacteria (MR-1), electron-hole pairs generated by the photocatalytic properties of bismuth vanadate can be transferred through the bacteria, thereby enhancing the electron transfer efficiency of MR-1 electrochemical bacteria.
[0010] According to a specific embodiment of the present invention, preferably, the electrochemical bacteria are inoculated on the surface of the bismuth vanadate layer by placing a bismuth vanadate photoelectrode in a culture medium for cultivation, and the number of colonies of the electrochemical bacteria in the culture medium is at least 1×10 6 CFU / mL, more preferably 1×10 6 CFU / mL to 1×10 8 CFU / mL.
[0011] According to a specific embodiment of the present invention, preferably, the bismuth vanadate layer meets the following requirements: at 100 mW·cm -2 Under the light power density of , the current density of the bismuth vanadate layer at +0.6V bias is 0.095A / m 2 Up to 0.105A / m 2 , more preferably 0.1A / m2 The bismuth vanadate layer can be prepared by conventional means as long as the above requirements are met. Among them, the photoactive bismuth vanadate has good photocatalytic performance and a suitable band gap, can effectively utilize sunlight, and can enhance the anode reaction, thereby increasing the photocurrent under illumination conditions and improving the efficiency of the photoelectrochemical reaction.
[0012] The present invention also provides a method for preparing the above-mentioned bismuth vanadate microbial photoanode, wherein the preparation method comprises: inoculating electrochemical bacteria on the surface of the bismuth vanadate layer of the bismuth vanadate photoelectrode to obtain the bismuth vanadate microbial photoanode.
[0013] According to a specific embodiment of the present invention, preferably, the inoculation process is: placing the bismuth vanadate photoelectrode in a culture medium and culturing it for 6-8 hours, and the number of electrochemical bacterial colonies in the culture medium is 1×10 6 CFU / mL to 1×10 8 CFU / mL.
[0014] According to a specific embodiment of the present invention, preferably, the bismuth vanadate photoelectrode is prepared by the following steps:
[0015] (1) forming a bismuth oxide iodide (BiOI) layer on a substrate;
[0016] (2) The bismuth iodide oxide layer is converted into a bismuth vanadate (BiVO4) layer by heat treatment to obtain a bismuth vanadate photoelectrode.
[0017] In some specific embodiments, preferably, the bismuth iodide oxylayer is prepared on the substrate by an electrodeposition method.
[0018] In some specific embodiments, preferably, the substrate is fluorine-doped tin oxide (FTO) glass and / or doped indium tin oxide (ITO), more preferably FTO glass.
[0019] In some specific embodiments, preferably, the method for preparing the bismuth vanadate photoelectrode specifically comprises the following steps:
[0020] (1) Cutting the FTO glass and cleaning and drying it;
[0021] (2) forming a BiOI layer on a FTO glass substrate by electrodeposition;
[0022] (3) coating vanadium acetylacetonate on the BiOI layer, followed by heat treatment to complete the conversion of BiOI to BiVO4, thereby obtaining a bismuth vanadate photoelectrode.
[0023] According to a specific embodiment of the present invention, preferably, the temperature of the heat treatment is 440-460° C., and the time of the heat treatment is 1.9-2.1 hours.
[0024] The present invention also provides a microbial photoelectrolysis cell, wherein the anode of the microbial photoelectrolysis cell is the above-mentioned bismuth vanadate microbial photoanode, or is the bismuth vanadate microbial photoanode prepared by the preparation method of the above-mentioned bismuth vanadate microbial photoanode. The microbial photoelectrolysis cell can be operated under natural light or artificial light source (such as xenon lamp, LED lamp), and the current generation is continuously monitored under the light condition to evaluate the treatment efficiency and the stability of the system.
[0025] According to a specific embodiment of the present invention, preferably, the microbial photoelectrolysis cell further comprises an anode electrolysis cell, a cathode electrolysis cell, and a cathode.
[0026] In some specific embodiments, preferably, the anode electrolysis cell contains wastewater.
[0027] In some specific embodiments, preferably, the cathode electrolytic cell contains a phosphate buffer, and the pH of the phosphate buffer is 7.
[0028] In some specific embodiments, the cathode can be a conventional electrode material, such as platinum wire.
[0029] In some specific embodiments, preferably, the microbial photoelectrolysis cell further comprises a device for applying voltage and measuring current to evaluate the efficiency and stability of the biological photoanode.
[0030] The present invention also provides a wastewater treatment method, wherein the treatment method comprises: adding wastewater as an anode electrolyte into the anode electrolysis cell of the above-mentioned microbial photoelectrolysis cell, and decomposing organic matter in the wastewater under a light source.
[0031] According to a specific embodiment of the present invention, preferably, the amount of wastewater used is 100-120 mL to ensure the effective operation of the photoelectrolysis cell.
[0032] According to a specific embodiment of the present invention, preferably, the optical power density of the light source is 90-110 mW·cm -2 .
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] (1) The bismuth vanadate microbial photoanode provided by the present invention significantly improves the photoelectric conversion efficiency through the synergistic effect of the bismuth vanadate photoelectrode and the MR-1 electrochemical bacteria. In the microbial photoelectrolysis cell (S-MEC) system, it has higher current density, stability and durability, and exhibits longer service life and higher photoelectrochemical performance. At the same time, the bismuth vanadate microbial photoanode can be applied to artificial wastewater treatment to achieve more efficient pollutant degradation efficiency.
[0035] (2) In the microbial photoelectrolysis cell provided by the present invention, the light source can provide the energy required for photocatalysis, and the photocatalytic properties of the BiVO4 photoelectrode are used to excite electron-hole pairs, and the electrons are directly transferred to the BiVO4 photoelectrode through the respiration of the bacteria. The microbial photoelectrolysis cell can decompose organic matter under the combined action of the photocatalytic properties of the BiVO4 photoanode and the electrochemical properties of Shewanella oneidensis MR-1, and significantly improve the wastewater treatment efficiency and energy conversion efficiency by improving the electron transfer efficiency. At the same time, the microbial photoelectrolysis cell also provides a new way for efficient wastewater treatment, bringing significant progress in environmental protection and energy sustainability.
[0036] (3) The present invention combines a microbial fuel cell (MFC) and a microbial photoelectrochemical cell (S-MEC) system. This combination is expected to significantly improve the efficiency and function of the microbial fuel cell, and achieve energy recovery and efficient energy conversion in the wastewater treatment process by utilizing the metabolic ability of microorganisms on organic matter and the photoelectric conversion ability of photoelectrodes. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 Schematic diagram of the microbial photoelectrolysis cell of the present invention.
[0038] Figure 2 XRD spectra of BiVO4, and the electrodes prepared in Example 1 and Comparative Example 1 after electrochemical reaction.
[0039] Figure 3 The UV-visible spectra of BiVO4 and the electrodes prepared in Example 1 and Comparative Example 1 are shown.
[0040] Figure 4 Photoluminescence spectroscopy characterization of BiVO4, and the electrodes prepared in Example 1 and Comparative Example 1.
[0041] Figure 5 These are the linear sweep voltammetry measurement results of the electrodes prepared in Example 1, Comparative Example 1, and Comparative Example 2.
[0042] Figure 6 The constant potential measurement performance of the electrodes prepared in Example 1, Comparative Example 1 and Comparative Example 2 is shown under a bias voltage of +0.6 V vs. a platinum counter electrode.
[0043] Figure 7 The graph is a graph showing the change in chemical oxygen demand (shown in mg / L) of the electrodes prepared in Example 1, Comparative Example 1, and Comparative Example 2 in a constant potential measurement when a bias of +0.6 V vs. a platinum counter electrode is applied.
[0044] Figure 8The graph is a graph showing the change in chemical oxygen demand (shown as a percentage) of the electrodes prepared in Example 1, Comparative Example 1, and Comparative Example 2 in a constant potential measurement when a bias voltage of +0.6 V vs. a platinum counter electrode is applied.
[0045] Fig. 9 These are the linear sweep voltammetry measurement results of the electrodes prepared in Example 1, Comparative Example 3, and Comparative Example 4. DETAILED DESCRIPTION
[0046] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0047] Example 1
[0048] This embodiment provides a method for preparing a microbial photoelectrolysis cell, comprising the following steps:
[0049] (1) Fluorine-doped tin oxide (FTO) (produced by Yingkou Shangneng Photoelectric Materials Co., Ltd.) glass was cut into a size of 1 cm × 2.5 cm, ultrasonically cleaned in acetone, alcohol and ultrapure water for 15 minutes respectively, and then blown dry with dry air.
[0050] (2) dissolving bismuth (III) nitrate pentahydrate in a solution containing 0.4 M potassium iodide to prepare a 0.04 M bismuth nitrate solution; adding 1 M nitric acid to the above bismuth nitrate solution to adjust the solution pH to 1.7; then adding 20 mL of anhydrous ethanol and 0.23 M p-benzoquinone to the solution, stirring for 5 minutes, and using the solution as a reaction solution for electrodeposition; using a three-electrode system, with FTO as a working electrode, Ag / AgCl as a reference electrode, and platinum wire as a counter electrode, depositing at -0.1 V against the Ag / AgCl cathode for 5 minutes to form a bismuth oxyiodide (BiOI) layer.
[0051] (3) 0.2 mL of a dimethyl sulfoxide (DMSO) solution containing 0.2 M vanadium acetylacetonate was coated on an electrode (1 cm × 2.5 cm) on which a BiOI layer had been formed, and the electrode was heat treated at 450 °C in a muffle furnace for 2 h to achieve the conversion of BiOI to bismuth vanadate (BiVO4).
[0052] (4) Soak in 1 M NaOH solution for 30 minutes and gently stir to remove excess V2O5 in the electrode; rinse with ultrapure water and dry at room temperature to obtain a pure BiVO4 photoelectrode.
[0053] (5) The BiVO4 photoelectrode was placed in Luria-Bertani (LB) medium (LB in 1000 mL ultrapure water contains 10 g NaCl, 5 g yeast extract, and 10 g tryptone) containing microorganisms (MR-1) and cultured for 8 h. The number of MR-1 colonies in the culture medium was 1×10 6 CFU / mL, made into BiVO4 microbial photoanode.
[0054] (6) Assembling a microbial photoelectrolysis cell: Luria-Bertani (LB) medium was added as artificial wastewater (100 mL) into the anode electrolytic cell, phosphate buffer (pH 7, prepared from 50 mM KH2PO4 and K2HPO4) was placed into the cathode electrolytic cell as the cathode electrolyte, and the cathode electrode was a 3 mm platinum wire electrode.
[0055] Under a simulated natural light environment, the BiVO4 microbial photoanode was placed in the above-mentioned microbial photoelectrolysis cell for photoelectrochemical performance testing to evaluate its electrochemical reaction intensity and wastewater treatment efficiency.
[0056] Comparative Example 1
[0057] This comparative example provides a method for preparing a photoelectrolytic cell, comprising the following steps:
[0058] (1) A BiVO4 photoelectrode was prepared according to the steps of Example 1.
[0059] (2) Assemble a photoelectrolytic cell, add Luria-Bertani (LB) culture medium as artificial wastewater (100 mL) into the anode electrolytic cell, put phosphate buffer (pH 7, prepared from 50 mM KH2PO4 and K2HPO4) as the cathode electrolyte into the cathode electrolytic cell, and use a 3 mm platinum wire electrode as the cathode electrode.
[0060] Under a simulated natural lighting environment, the BiVO4 photoelectrode was used as the anode of the above-mentioned photoelectrolysis cell for photoelectrochemical performance testing to evaluate its electrochemical reaction intensity and wastewater treatment efficiency.
[0061] Comparative Example 2
[0062] This comparative example provides a method for preparing a microbial electrolytic cell, comprising the following steps:
[0063] (1) The carbon cloth was cut into a size of 1 cm × 2.5 cm, ultrasonically cleaned in acetone, alcohol, and ultrapure water for 15 min respectively, and then dried with dry air.
[0064] (2) The carbon cloth was placed in Luria-Bertani (LB) medium (LB in 1000 mL ultrapure water contains 10 g NaCl, 5 g yeast extract, and 10 g tryptone) containing microorganisms (MR-1) and cultured for 8 hours. The number of MR-1 colonies in the culture medium was 1×10 6 CFU / mL, made into carbon cloth microbial electrode.
[0065] (3) Assemble a microbial electrolytic cell, add Luria-Bertani (LB) medium as artificial wastewater (100 mL) into the anode electrolytic cell, put phosphate buffer (pH 7, prepared from 50 mM KH2PO4 and K2HPO4) as the cathode electrolyte into the cathode electrolytic cell, and use a 3 mm platinum wire electrode as the cathode electrode.
[0066] The carbon cloth microbial electrode was used as the anode of the microbial electrolysis cell for electrochemical performance testing to evaluate its electrochemical reaction intensity and efficiency in wastewater treatment.
[0067] Comparative Example 3
[0068] This comparative example provides a method for preparing a microbial photoelectrolysis cell. The specific steps are basically the same as those in Example 1, except that: the heat treatment condition in step (3) is heat treatment at 400°C for 2 hours; the other steps and parameters are consistent with those in Example 1, and a BiVO4 microbial photoanode is prepared and a microbial photoelectrolysis cell is assembled.
[0069] Comparative Example 4
[0070] This comparative example provides a method for preparing a microbial photoelectrolysis cell. The specific steps are basically the same as those in Example 1, except that: the heat treatment condition in step (3) is heat treatment at 500°C for 2 hours; the other steps and parameters are consistent with those in Example 1, and a BiVO4 microbial photoanode is prepared and a microbial photoelectrolysis cell is assembled.
[0071] The anodes prepared in the above embodiments and comparative examples and their electrochemical and wastewater treatment performances are characterized and analyzed as follows:
[0072] Figure 1 A schematic diagram of the microbial photoelectrolysis cell provided by the present invention is shown; it includes an anode electrolytic cell 101, a BiVO4 microbial anode electrode 102, a 3 mm platinum wire counter electrode 103, a cathode electrolytic cell 104, a proton exchange membrane 105 and an electrochemical workstation 106.
[0073] Figure 2 The X-ray diffraction patterns of BiVO4, and the BiVO4 microbial photoanode and BiVO4 photoelectrode prepared in Example 1 and Comparative Example 1 after electrochemical reaction are shown. Figure 2As shown, after the electrochemical reaction, the crystal structure of the BiVO4 microbial photoanode and the BiVO4 photoelectrode remained original, indicating that the electrochemical reaction process did not lead to significant changes in the crystal structure.
[0074] Figure 3 The UV-visible spectra of BiVO4 (bismuth vanadate), and the BiVO4 microbial photoanode (bismuth vanadate microbial photoanode) and BiVO4 photoelectrode (bismuth vanadate photoanode) prepared in Example 1 and Comparative Example 1 are shown. Figure 3 As shown, the BiVO4 microbial photoanode and BiVO4 photoelectrode showed obvious absorption peaks in the wavelength range of 500 to 700 nm, indicating that the organic matter to be removed in the wastewater may accumulate on the electrode surface.
[0075] Figure 4 The photoluminescence spectra of BiVO4 (bismuth vanadate), and the BiVO4 microbial photoanode (bismuth vanadate microbial photoanode) and BiVO4 photoelectrode (bismuth vanadate photoanode) prepared in Example 1 and Comparative Example 1 are shown. Figure 4 As shown in the figure, the fluorescence peak of the BiVO4 microbial photoanode weakened, while the fluorescence signal of the BiVO4 photoelectrode increased. In the wavelength range of 500 to 700nm, both the BiVO4 microbial photoanode and the BiVO4 photoelectrode showed absorption. This indicates that after the electrochemical reaction, the organic matter to be removed in the wastewater may be adsorbed on the electrode surface.
[0076] Figure 5 The characterization results of the carbon cloth microbial electrode, BiVO4 microbial photoanode and BiVO4 photoelectrode prepared in Example 1 and Comparative Examples 1-2 using linear sweep voltammetry are shown. Wherein, a represents BiVO4 microbial photoanode-illumination (Example 1), b represents carbon cloth microbial electrode (Comparative Example 2), c represents BiVO4 photoelectrode-illumination (Comparative Example 1), d represents BiVO4 microbial photoanode-darkness (Example 1), and e represents BiVO4 photoelectrode-darkness (Comparative Example 1). Figure 5 As shown, at 100mW·cm -2 Under the illumination conditions, the current curve of BiVO4 microbial photoanode at +0.6V to Ag / AgCl bias is 3.5 times that of carbon cloth microbial electrode, which shows the synergistic effect of microorganisms and BiVO4 photoanode. The current of BiVO4 photoelectrode without microorganisms attached under the same illumination and voltage conditions is only 25% of that of carbon cloth microbial electrode.
[0077] Figure 6The constant potential measurement performance of the carbon cloth microbial electrode, BiVO4 microbial photoanode and BiVO4 photoelectrode prepared in Example 1 and Comparative Examples 1-2 is shown under the applied +0.6V vs. platinum counter electrode bias. Wherein, a represents BiVO4 microbial photoanode-illumination (Example 1), b represents carbon cloth microbial electrode (Comparative Example 2), c represents BiVO4 photoelectrode-illumination (Comparative Example 1), and the illumination condition is 100mW·cm -2 .like Figure 6 As shown, under a bias voltage of +0.6 V vs. Pt counter electrode, the current density of the BiVO4 microbial photoanode increases from 3 A / m to 10 A / m from 0 h to 60 h. 2 Down to 1A / m 2 , and the current density remained at 1A / m after 60 hours. 2 ; In the same period of time, the current density of the carbon cloth microbial electrode increased from 0.8A / m 2 Down to 0.3A / m 2 , and the current density remained at 0.3A / m after 60 hours. 2 Similarly, at +0.6 V vs. Pt counter electrode, the current density of the BiVO4 photoelectrode remained stable at 0.1 A / m 2 This indicates that the BiVO4 microbial photoanode can maintain a higher current density and has better photoelectric stability.
[0078] Figure 7 The changes in chemical oxygen demand (in mg / L) of the carbon cloth microbial electrode, BiVO4 microbial photoanode and BiVO4 photoelectrode prepared in Example 1 and Comparative Examples 1-2 in a constant potential measurement are shown under a bias voltage of +0.6V vs. a platinum counter electrode. Figure 7 As shown, the illumination condition is 100 mW·cm -2 , under a bias of +0.6V vs. platinum counter electrode, from 0 hours to 120 hours, the chemical oxygen demand of the BiVO4 microbial photoanode decreased from 8376.7mg / L to 5014.4mg / L; while in the same time period, the chemical oxygen demand of the carbon cloth microbial electrode only decreased from 8226.7mg / L to 7137.8mg / L; at the same time, the chemical oxygen demand of the BiVO4 photoelectrode decreased from 8537.8mg / L to 6893.3mg / L. Therefore, the chemical oxygen demand (COD) of the BiVO4 microbial photoanode decreased more significantly, showing a COD degradation rate of up to 40% within 120 hours, while the COD degradation rate of Comparative Examples 1-2 was only 13-19%, indicating that the BiVO4 microbial photoanode removed more organic matter and had a higher wastewater degradation efficiency.
[0079] Figure 8The change of chemical oxygen demand (shown as percentage) in constant potential measurement of the carbon cloth microbial electrode, BiVO4 microbial photoanode and BiVO4 photoelectrode prepared in Example 1 and Comparative Examples 1-2 is shown under the applied +0.6V vs. platinum counter electrode bias. Figure 8 As shown, the illumination condition is 100 mW·cm -2 , under a bias of +0.6V vs. platinum counter electrode, from 0 to 120 hours, the chemical oxygen demand of the BiVO4 microbial photoanode decreased to 59.9%; while the chemical oxygen demand of the carbon cloth microbial electrode only decreased to 86.8% during the same period; at the same time, the chemical oxygen demand of the BiVO4 photoelectrode only decreased to 80.7%. Therefore, the chemical oxygen demand of the BiVO4 microbial photoanode decreased more, indicating that the BiVO4 microbial photoanode removed more organic matter and had a higher wastewater degradation efficiency.
[0080] Fig. 9 The characterization results of BiVO4 microbial photoanodes prepared at different heat treatment temperatures in Example 1, Comparative Example 3, and Comparative Example 4 using linear sweep voltammetry are shown. - 2, the current curve results of BiVO4 microbial photoanode with different heat treatment temperatures under +0.6V bias against Ag / AgCl show that: Example 1 has the highest current density, showing the best electron transfer efficiency and photoelectric performance. The heat treatment temperature of Comparative Example 3 is lower (400°C), and the current density is the second highest. The heat treatment temperature of Comparative Example 4 is higher (500°C), and the current density is the lowest. These results show that the heat treatment conditions of Example 1 (450°C, 2 hours) provide the best performance in the present invention, showing the best synergy between microorganisms and BiVO4 photoanode. The current densities of Comparative Examples 3 and 4 are relatively low, respectively showing the effect of heat treatment temperature on the performance of the photoelectrode. When the heat treatment temperature is too low (400°C), the crystallinity of the bismuth vanadate layer is insufficient, resulting in reduced photoelectric conversion efficiency and electron transfer efficiency, so the current density is low; when the heat treatment temperature is too high (500°C), the excessively high temperature causes the lattice structure of the bismuth vanadate layer to be damaged, and even defects to appear, thereby reducing the performance of the photoelectrode. Therefore, although comparative examples 3 and 4 were inoculated with electrochemical bacteria, the performance of the bismuth vanadate layer was poor due to inappropriate heat treatment temperature, which further affected the overall photoelectric conversion efficiency.
Claims
1. A bismuth vanadate microbial photoanode, wherein: The bismuth vanadate microbial photoanode comprises a bismuth vanadate photoelectrode and electrochemical bacteria; The bismuth vanadate photoelectrode comprises a substrate and a bismuth vanadate layer; the electrochemical bacteria are inoculated on the bismuth vanadate layer; The electrochemical bacteria is Shewanella Oneidensis MR-1.
2. The bismuth vanadate microbial photoanode according to claim 1, wherein The electrochemical bacteria are inoculated on the surface of the bismuth vanadate layer by placing the bismuth vanadate photoelectrode in a culture medium for cultivation. In the culture medium, the number of colonies of the electrochemical bacteria is at least 1×10 6 CFU / mL, preferably 1×10 6 CFU / mL to 1×10 8 CFU / mL.
3. The bismuth vanadate microbial photoanode according to claim 1, wherein The bismuth vanadate layer meets the following requirements: At 100 mW cm -2 Under the light power density of , the current density of the bismuth vanadate layer at +0.6V bias is 0.095A / m 2 Up to 0.105A / m 2 .
4. The method for preparing the bismuth vanadate microbial photoanode according to any one of claims 1 to 3, wherein: The preparation method comprises: The surface of the bismuth vanadate layer of the bismuth vanadate photoelectrode is inoculated with electrochemical bacteria to obtain a bismuth vanadate microbial photoanode.
5. The preparation method according to claim 4, wherein The inoculation process is as follows: bismuth vanadate photoelectrode is placed in a culture medium and cultured for 6-8 hours. The number of electrochemical bacterial colonies in the culture medium is 1×10 6 CFU / mL to 1×10 8 CFU / mL.
6. The preparation method according to claim 4, wherein The bismuth vanadate photoelectrode is prepared by the following steps: (1) forming a bismuth iodide oxide layer on a substrate; (2) converting the bismuth iodide layer into a bismuth vanadate layer by heat treatment to obtain a bismuth vanadate photoelectrode; Preferably, the substrate is fluorine-doped tin oxide glass and / or doped indium tin oxide.
7. The preparation method according to claim 6, wherein: The temperature of the heat treatment is 440-460° C., and the time of the heat treatment is 1.9-2.1 hours.
8. A microbial photoelectrolysis cell, wherein: The anode of the microbial photoelectrolysis cell is the bismuth vanadate microbial photoanode described in any one of claims 1 to 3, or is the bismuth vanadate microbial photoanode prepared by the preparation method of the bismuth vanadate microbial photoanode described in any one of claims 4 to 7.
9. The microbial photoelectrolysis cell according to claim 8, wherein: The microbial photoelectrolysis cell also includes an anode electrolysis cell, a cathode electrolysis cell and a cathode.
10. A method for treating wastewater, wherein: The treatment method comprises: adding wastewater as an anolyte to the anode electrolysis cell of the microbial photoelectrolysis cell of claim 8 or 9, and decomposing organic matter in the wastewater under a light source; Preferably, the amount of wastewater is 100-120 mL; Preferably, the optical power density of the light source is 90-110 mW·cm -2 .
Citation Information
Patent Citations
Bioelectrochemical device for pollution reduction and hydrogen production by utilization of solar energy and method thereof
CN104817190A
Bismuth vanadate photo-anode, preparation method thereof and application of bismuth vanadate photo-anode in ammonia decomposition reaction
CN117328087A
Z-Scheme Microbial Photoelectrochemical System (MPS) for Wastewater-to-Chemical Fuel Conversion
US20180230028A1