Sanitary ceramic art glaze with leather texture and preparation method thereof

By using base glaze with potassium feldspar, aluminum oxide, zinc oxide and other components and surface glaze with high potassium sodium in sanitary ceramic art glaze, combined with tunnel kiln firing technology, the existing sanitary ceramic glaze surface is difficult to meet complex instruments. The problem of shape and high temperature fluidity requirements has achieved leather texture and a smooth and stain-resistant self-cleaning surface, enriching the decorative effect of sanitary ceramics.

CN118908572AActive Publication Date: 2024-11-08JOMOO KITCHEN & BATHROOM
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411261750.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-08
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

The existing sanitary ceramic decorative art glazes are mostly homogeneous and colorful matte, which is difficult to meet the high-temperature fluidity requirements of complex instruments. The crack glaze is easy to absorb dirty and difficult to clean, and the crystallized glaze is rigorous in firing conditions, which is not suitable for Sanitary ware.

Method used

Using sanitary ceramic art glaze with leather texture texture, the base glaze consists of potassium feldspar, alumina, zinc oxide, calcium phosphate and other components. Combined with a high-potassium-containing surface glaze, the glaze slurry performance is adjusted through ball milling and CMC, spraying and Fried in a tunnel kiln to form a flat, stain-resistant self-cleaning surface.

Benefits of technology

It realizes the decorative effect of leather texture texture, while ensuring the flatness, low roughness and easy cleaning of the glaze. It is suitable for the decorative art glaze of sanitary ceramic ware.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908572A_ABST
    Figure CN118908572A_ABST
Patent Text Reader

Abstract

The invention discloses a sanitary ceramic art glaze with leather texture and a preparation method of the sanitary ceramic art glaze, and the sanitary ceramic art glaze comprises a ground glaze and a cover glaze, comprising the following components: 25-35 parts of potassium feldspar, 4-6 parts of kaolin, 5-7 parts of aluminum oxide, 12-16 parts of calcite, 12-16 parts of zinc oxide, 18-24 parts of calcium phosphate, 8-10 parts of zirconium silicate, 2-4 parts of cobalt black pigment, 0.5-1 part of dark green pigment and 0.2-0.3 part of sodium carbonate. The artistic glaze disclosed by the invention has an artistic effect of leather texture on the whole, and the surface of the artistic glaze is a smooth and stain-resistant self-cleaning glaze surface, so that the artistic glaze is more suitable for decorative artistic glaze of sanitary ceramic sanitary ware.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of sanitary ceramics, in particular to a sanitary ceramic artistic glaze. Background Art

[0002] Existing sanitary ceramics are mainly white glazed, and the main reason is that many decorative art glazes of ceramics are not suitable for complex shapes of sanitary ceramics. For example, kiln-fired glazes require high-temperature fluidity, and large-sized toilets and basins are prone to local glaze thickness that is too high, resulting in cracks; crackle glazes will absorb dirt into the body, causing odor and difficulty in cleaning, and are not suitable for sanitary ware that is in contact with dirt for a long time; crystallized glazes are extremely strict with glaze thickness, firing temperature, and firing atmosphere, and are not suitable for tunnel kilns for sanitary ware.

[0003] Currently in the market, the decorative glazes of sanitary ceramics are mostly colorful matte artistic glazes, and the glazes are homogeneous. Summary of the invention

[0004] The main purpose of the present invention is to provide a sanitary ceramic art glaze. The sanitary ceramic art glaze provided by the present invention has a leather texture and is suitable for tunnel kiln firing of sanitary ware.

[0005] The technical solution adopted by the present invention to solve its technical problem is:

[0006] A sanitary ceramic art glaze with leather texture, comprising a base glaze of the following ingredients by mass: 25-35 parts of potassium feldspar, 4-6 parts of kaolin, 5-7 parts of aluminum oxide, 12-16 parts of calcite, 12-16 parts of zinc oxide, 18-24 parts of calcium phosphate, 8-10 parts of zirconium silicate, 2-4 parts of cobalt black material, 0.5-1 part of dark green material, and 0.2-0.3 part of sodium carbonate.

[0007] In a preferred embodiment, the base glaze includes the following ingredients, measured by mass: 25 parts of potassium feldspar, 4 parts of kaolin, 5 parts of aluminum oxide, 16 parts of calcite, 16 parts of zinc oxide, 24 parts of calcium phosphate, 10 parts of zirconium silicate, 4 parts of cobalt black material, 1 part of dark green material, and 0.2 parts of sodium carbonate.

[0008] In another preferred embodiment, the base glaze includes the following ingredients, measured by mass: 30 parts of potassium feldspar, 5 parts of kaolin, 6 parts of aluminum oxide, 14 parts of calcite, 14 parts of zinc oxide, 20 parts of calcium phosphate, 10 parts of zirconium silicate, 3 parts of cobalt black material, 1 part of dark green material, and 0.2 parts of sodium carbonate.

[0009] In another preferred embodiment, the base glaze includes the following ingredients, measured by mass: 35 parts of potassium feldspar, 6 parts of kaolin, 7 parts of aluminum oxide, 12 parts of calcite, 12 parts of zinc oxide, 18 parts of calcium phosphate, 8 parts of zirconium silicate, 2 parts of cobalt black material, 0.5 parts of dark green material, and 0.3 parts of sodium carbonate.

[0010] In the present invention, the sanitary ceramic art glaze with leather texture also includes a surface glaze. Further, the surface glaze is a self-cleaning surface glaze. In a preferred embodiment, the surface glaze includes the following components by mass: 25-30 parts of quartz, 30-35 parts of potassium feldspar, 12-16 parts of calcite, 1-3 parts of zinc oxide, 1-4 parts of aluminum oxide, 4-6 parts of kaolin, 2-6 parts of calcined talc, 6-8 parts of wollastonite, and 0.2-0.3 parts of sodium carbonate.

[0011] Another object of the present invention is to provide a method for preparing the sanitary ceramic artistic glaze having a leather texture, comprising the following steps:

[0012] Step 1: grind the base glaze according to the ratio of material: water = 100: (40-50), ball-mill until the particle size is less than 10 μm and the cumulative proportion is 70%-75%, remove the iron from the mill, adjust the glaze slurry performance to a flow rate of 50s / 100ml-60s / 100ml with CMC (hydroxymethyl cellulose), spray it on the body, and the thickness is 0.3mm-0.4mm;

[0013] Step 2: Put the top glaze into the mill according to the ratio of material: water = 100: (40-50), ball-mill until the particle size is less than 10μm and the cumulative proportion is 78%-82%. After exiting the mill, sieve to remove iron, adjust the glaze slurry performance to a flow rate of 40s / 100ml-50s / 100ml with CMC, and spray it on the base glaze with a thickness of 0.2mm-0.3mm.

[0014] Step three, firing in a shuttle kiln or tunnel kiln.

[0015] In a preferred embodiment, in step three, the sintering temperature is controlled at 1200° C. to 1250° C. and kept at this temperature for 0.5 h to 0.8 h.

[0016] In a preferred embodiment, in step three, sintering is performed in an oxidizing atmosphere.

[0017] In a preferred embodiment, the base glaze is put into the mill according to the ratio of material: water = 100:42, and is ball-milled to a particle size of less than 10μ, with a cumulative proportion of 72%. After being discharged from the mill, it is sieved to remove iron, and the glaze slurry performance is adjusted to a flow rate of 55s / 100ml with CMC, and sprayed on the body with a thickness of 0.4mm; then the top glaze is sprayed with 0.2mm, and fired in an oxidizing atmosphere in a shuttle kiln, the firing temperature is controlled at 1250°C, and the heat preservation is carried out for 0.8h.

[0018] Compared with the background technology, this technical solution has the following advantages:

[0019] 1. The difference of the base glaze of the present invention is mainly reflected in that conventional ceramic glazes are based on silicon-aluminum as glass network formers and maintain silicon saturation, while the base glaze formula of the present invention reduces the conventional silicon content of 70-75% to 35-40%, and replaces part of the silicon with phosphorus to form a network structure. During the high-temperature firing process, the surface glaze has a high potassium and sodium content and is melted first, while the base glaze is still in the stage of decomposition and exhaust. The surface glaze will form an uneven initial texture due to the decomposition and exhaust of the body and the base glaze; after the temperature continues to rise, the base glaze and the surface glaze are completely melted, but because the base glaze has a high zinc, calcium, and phosphorus content and a large surface tension, the base glaze will further agglomerate and form wrinkles along with the initial texture; the surface glaze has a high potassium, sodium, and silicon content and a lower surface tension, and will spread on the surface of the base glaze to form a smooth surface. Because the base glaze adds more phosphorus to replace silicon, the high-temperature viscosity is improved, and a large difference in composition is maintained, so that the base glaze remains at the bottom and does not affect the smooth and anti-fouling effect of the surface glaze layer.

[0020] 2. The top glaze is a conventional transparent, bright and self-cleaning glaze in the sanitary ceramics industry, which ensures the functionality of the sanitary ware glaze, such as low roughness, not easy to stain and easy to clean. However, by adjusting the base glaze formula and differentiating the composition with the top glaze, a leather texture touch and appearance effect is formed, enriching the decorative effect of sanitary ceramics.

[0021] 3. The present invention finally forms an artistic effect of overall leather texture, and the surface is a flat, stain-resistant, self-cleaning glaze surface, which is more suitable for decorative art glaze of sanitary ceramic sanitary ware. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.

[0023] Figure 1 The present invention provides a whole body leather art glaze product.

[0024] Figure 2 The invention discloses a leather art glaze product with partially decorated colors.

[0025] Figure 3 This is a physical picture of the leather art glaze of Example 1.

[0026] Figure 4 This is a real-object picture of the leather art glaze of Example 2.

[0027] Figure 5 This is a physical picture of the leather art glaze of Example 3.

[0028] Figure 6 This is a physical picture of the leather art glaze of Comparative Example 1.

[0029] Figure 7 This is a physical picture of the leather art glaze of Comparative Example 2. DETAILED DESCRIPTION

[0030] Example 1

[0031] Prepare a base glaze with the following ingredients in parts by mass: 25 parts of potassium feldspar, 4 parts of kaolin, 5 parts of aluminum oxide, 16 parts of calcite, 16 parts of zinc oxide, 24 parts of calcium phosphate, 10 parts of zirconium silicate, 4 parts of cobalt black material, 1 part of dark green material, and 0.2 parts of sodium carbonate.

[0032] Example 2

[0033] Prepare a base glaze with the following ingredients in parts by mass: 30 parts of potassium feldspar, 5 parts of kaolin, 6 parts of aluminum oxide, 14 parts of calcite, 14 parts of zinc oxide, 20 parts of calcium phosphate, 10 parts of zirconium silicate, 3 parts of cobalt black material, 1 part of dark green material, and 0.2 parts of sodium carbonate.

[0034] Example 3

[0035] Prepare a base glaze with the following ingredients in parts by mass: 35 parts potassium feldspar, 6 parts kaolin, 7 parts aluminum oxide, 12 parts calcite, 12 parts zinc oxide, 18 parts calcium phosphate, 8 parts zirconium silicate, 2 parts cobalt black material, 0.5 parts dark green material, and 0.3 parts sodium carbonate.

[0036] Comparative Example 1

[0037] Prepare a base glaze with the following ingredients in parts by mass: 24 parts quartz, 25 parts potassium feldspar, 4 parts kaolin, 5 parts aluminum oxide, 16 parts calcite, 16 parts zinc oxide, 0 parts calcium phosphate, 10 parts zirconium silicate, 4 parts cobalt black material, 1 part dark green material, and 0.2 parts sodium carbonate.

[0038] Comparative Example 2

[0039] Prepare a base glaze with the following ingredients in parts by mass: 10 quartz, 29 potassium feldspar, 4 kaolin, 5 aluminum oxide, 16 calcite, 3 zinc oxide, 24 calcium phosphate, 10 zirconium silicate, 4 cobalt black material, 1 dark green material, and 0.2 sodium carbonate.

[0040]

[0041] The above embodiments and comparative examples all use the same glaze, which includes, by mass:

[0042] Quartz 30, potassium feldspar 35, calcite 12, zinc oxide 2, aluminum oxide 3, kaolin 4, calcined talc 5, wollastonite 6, sodium carbonate 0.3.

[0043] In the above embodiments and comparative examples, the ingredients are prepared according to the above ratio, the base glaze is put into the mill according to the ratio of material: water = 100:42, ball-milled to a particle size of <10 μm with a cumulative proportion of 72%, and then sieved to remove iron after being discharged from the mill, and the glaze slurry performance is adjusted to a flow rate of 55s / 100ml with CMC, and sprayed on the body with a thickness of 0.4mm;

[0044] The surface glaze is put into the mill according to the ratio of material: water = 100:42, and ball-milled to a particle size of less than 10μm, with a cumulative proportion of 80%. After exiting the mill, it is sieved to remove iron, and the glaze slurry performance is adjusted to a flow rate of 45s / 100ml with CMC, and sprayed on the base glaze with a thickness of 0.2mm.

[0045] The shuttle kiln is used for firing in an oxidizing atmosphere, the firing temperature is controlled at 1250℃, and the temperature is kept for 0.8h. The heating stage is:

[0046] Room temperature -80℃, 50min; 80-700℃, 240min; 700-1050, 90min; 1050-1100, 90min; 1100-1250, 70min; the temperature is increased at a uniform rate in each heating stage. The results are as follows:

[0047]

[0048] In Examples 1 to 3, the ratio of feldspar to calcite, zinc oxide, and calcium phosphate was changed to adjust the composition difference with the glaze. The texture of Examples 1 to 3 can produce a leather texture effect, and the roughness is relatively low, with no significant difference from the conventional glaze roughness, all in the range of 0.07 to 0.1 μm, and the glaze cleanability is not significantly affected. Example 2 has the best comprehensive effect, with low glaze roughness, the best cleanability, and a strong leather texture.

[0049] Comparative Example 1 is different from Example 1 in that calcium phosphate is not added but quartz is used instead. The glaze can form a weak leather texture, but the surface roughness of the glaze is relatively large. Because the viscosity of the base glaze of Comparative Example 1 is lower than that of Example 1, the large difference in surface tension between the base glaze and the top glaze and the low viscosity will cause a more violent reaction of the glaze, making it difficult to form a smooth glaze effect on the surface, which seriously affects the easy-to-clean glaze and is not suitable for use as a sanitary ceramic glaze.

[0050] Comparative Example 2 is different from Example 1 in that the added zinc oxide ratio is less, and quartz is used instead, and the glaze surface does not form a leather texture. Because the amount of zinc oxide added is less, the exhaust stage of the base glaze is also earlier, and the base glaze begins to melt when the top glaze melts. The exhaust of the body is blocked by the base glaze, and it is difficult to form early wrinkles to trigger further reactions and changes between the base glaze and the top glaze.

[0051] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.

Claims

1. A sanitary ceramic art glaze with leather texture, characterized by: The base glaze includes the following ingredients by mass: 25-35 parts of potassium feldspar, 4-6 parts of kaolin, 5-7 parts of aluminum oxide, 12-16 parts of calcite, 12-16 parts of zinc oxide, 18-24 parts of calcium phosphate, 8-10 parts of zirconium silicate, 2-4 parts of cobalt black material, 0.5-1 part of dark green material, and 0.2-0.3 part of sodium carbonate.

2. A sanitary ceramic art glaze with leather texture, characterized by: The base glaze includes the following ingredients, by mass: 25 parts of potassium feldspar, 4 parts of kaolin, 5 parts of aluminum oxide, 16 parts of calcite, 16 parts of zinc oxide, 24 parts of calcium phosphate, 10 parts of zirconium silicate, 4 parts of cobalt black material, 1 part of dark green material, and 0.2 parts of sodium carbonate.

3. A sanitary ceramic art glaze with leather texture, characterized by: The base glaze includes the following ingredients, by mass: 30 parts of potassium feldspar, 5 parts of kaolin, 6 parts of aluminum oxide, 14 parts of calcite, 14 parts of zinc oxide, 20 parts of calcium phosphate, 10 parts of zirconium silicate, 3 parts of cobalt black material, 1 part of dark green material, and 0.2 parts of sodium carbonate.

4. A sanitary ceramic art glaze with leather texture, characterized by: The base glaze includes the following ingredients by mass: 35 parts of potassium feldspar, 6 parts of kaolin, 7 parts of aluminum oxide, 12 parts of calcite, 12 parts of zinc oxide, 18 parts of calcium phosphate, 8 parts of zirconium silicate, 2 parts of cobalt black material, 0.5 parts of dark green material, and 0.3 parts of sodium carbonate.

5. The sanitary ceramic art glaze with leather texture according to any one of claims 1 to 4, characterized in that: It also includes a glaze; the glaze includes the following ingredients by mass: 25-30 parts of quartz, 30-35 parts of potassium feldspar, 12-16 parts of calcite, 1-3 parts of zinc oxide, 1-4 parts of aluminum oxide, 4-6 parts of kaolin, 2-6 parts of calcined talc, 6-8 parts of wollastonite, and 0.2-0.3 parts of sodium carbonate.

6. The method for preparing a sanitary ceramic artistic glaze with leather texture according to claim 5, characterized in that: The steps include: Step 1: grind the base glaze according to the ratio of material: water = 100: (40-50), ball-mill until the particle size is less than 10 μm and the cumulative proportion is 70%-75%, remove the iron from the mill, adjust the glaze slurry performance to a flow rate of 50s / 100ml-60s / 100ml with CMC, and spray it on the body with a thickness of 0.3mm-0.4mm; Step 2: The top glaze is put into the mill according to the ratio of material: water = 100: (40-50), ball-milled to a particle size of less than 10 μm, with a cumulative proportion of 78%-82%, then sieved to remove iron, and the glaze slurry performance is adjusted to a flow rate of 40s / 100ml-50s / 100ml with CMC, and sprayed on the base glaze with a thickness of 0.2mm-0.3mm; Step three: firing using a shuttle kiln or tunnel kiln.

7. The method for preparing a sanitary ceramic artistic glaze with leather texture according to claim 6, characterized in that: In step three, the sintering temperature is controlled at 1200° C. to 1250° C. and kept at this temperature for 0.5 h to 0.8 h.

8. The method for preparing a sanitary ceramic artistic glaze with leather texture according to claim 7, characterized in that: In step three, sintering is performed in an oxidizing atmosphere.

9. The method for preparing a sanitary ceramic artistic glaze with leather texture according to claim 6, characterized in that: The base glaze is put into the mill according to the ratio of material: water = 100:42, and ball-milled to a particle size of <10μ, with a cumulative particle size of 72%. After being discharged from the mill, it is sieved to remove iron, and the glaze slurry performance is adjusted to a flow rate of 55s / 100ml with CMC, and sprayed on the body with a thickness of 0.4mm.

10. The method for preparing a sanitary ceramic artistic glaze with leather texture according to claim 9, characterized in that: After spraying the base glaze, spray the top glaze with a thickness of 0.2 mm. Use a shuttle kiln to fire in an oxidizing atmosphere. The firing temperature is controlled at 1250°C and the temperature is kept at this temperature for 0.8 hours.

Citation Information

Patent Citations

  • Production method for natural sandstone-imitating ceramic tile

    CN102786297A

  • Preparation method for architectural decoration flambe art ceramic tile

    CN105315015A

  • Ceramic product with self-cleaning glaze and making method thereof

    CN109437839A

  • High-plastic pug, making method of ceramic paper cutting / paper quilling and obtained product

    CN110590347A

  • Colored chrysanthemum-shaped crystal flower glaze, chrysanthemum-shaped crystal flower translucent ceramic tile, and production method of ceramic tile

    CN110835234A