Method for rapidly synthesizing shape-preserving oxygen-vacancy-enriched hematite film photo-anode through thermal shock and application

By rapidly heating up the hematite precursor film by thermal shock method under vacuum negative pressure, the problems of long preparation period and high energy consumption of hematite film in the prior art are solved, and high efficiency and low energy are achieved The photoanode consumed hematite film is prepared, and its photoelectrocatalytic performance is comparable to that of traditional methods.

CN118908588APending Publication Date: 2024-11-08HEFEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411147352.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, the preparation process of hematite thin film photoanode has a long period, high energy consumption, low efficiency, and is difficult to effectively regulate the microstructure and oxygen vacancy, which affects its photoelectrocatalytic performance.

Method used

The hematite precursor film is rapidly heated by thermal shock method under vacuum environment, and the conductive resistance is used to carry out short-term power-on heating, so as to achieve rapid synthesis of hematite film photoelectrode, with a temperature increase rate of 103~104℃/ Min, the cooling rate is also relatively high, and can maintain the fine regulation of the microstructure of the material and the oxygen atom content.

Benefits of technology

It has achieved high-efficiency and low-energy consumption of hematite thin film photoanode preparation, rich in oxygen vacancy, and the photoelectro-catalytic decomposition of water is comparable to that of traditional methods, with improved efficiency and reduced energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908588A_ABST
    Figure CN118908588A_ABST
Patent Text Reader

Abstract

The invention discloses a method for rapidly synthesizing a shape-preserving oxygen-vacancy-enriched hematite film photo-anode through thermal shock and application, and belongs to the technical field of new energy materials. According to the method, in a vacuum negative-pressure environment, a hematite precursor film is subjected to temperature rising treatment through a thermal shock method, and the shape-preserving oxygen-vacancy-enriched hematite film photo-anode is obtained; and then cooling to obtain the hematite film photoelectrode converted from the hematite precursor film. According to the method, the hematite precursor film is subjected to thermal shock heat treatment in the negative pressure state, the shape-preserving hematite film photo-anode rich in oxygen vacancies can be obtained in one step, efficiency is higher, energy consumption is lower, and the photoelectrocatalytic water decomposition performance of the hematite film photo-anode is equivalent to that of a hematite film photo-anode obtained through a traditional heat treatment mode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of new energy materials, and specifically relates to a method for rapidly synthesizing a shape-preserving oxygen-vacancy-rich hematite thin film photoanode by thermal shock. Background Art

[0002] With the rapid development of social economy and industry, the global energy crisis and environmental pollution have increasingly attracted widespread attention from countries around the world. It is imperative to seek and develop renewable green energy technologies. Converting solar energy into storable chemical fuels through artificial means is a promising alternative for developing green energy technologies and solving the problem of intermittent solar energy. Among them, the photocatalytic technology of photodecomposing water to produce green energy carriers - hydrogen is a strategy with great application prospects for artificial utilization of solar energy resources. As the core component of the photoelectrochemical cell, the photoelectrode is responsible for capturing sunlight and is also the place where water decomposition occurs. Its properties play a decisive role in the catalytic water decomposition performance of the photoelectrochemical cell. Transition metal oxides such as hematite (Fe2O3), ZnO, TiO2, BiVO4) are currently the research hotspots of thin film photoelectrode materials due to their advantages such as abundant reserves of contained elements, low cost and non-toxicity.

[0003] At present, the preparation of transition metal oxide thin film photoelectrodes generally includes the following methods: (1) Preparing a precursor film on a conductive substrate such as conductive glass, and then subjecting the film to high temperature annealing treatment in a muffle furnace, tube furnace or other heat treatment equipment to obtain a transition metal oxide thin film photoelectrode; (2) Directly subjecting metal sheets such as iron sheets, tungsten sheets, titanium sheets, etc. to high temperature heat treatment oxidation in a muffle furnace, tube furnace or other equipment to obtain a transition metal oxide photoelectrode; (3) Directly preparing a transition metal oxide thin film photoelectrode on a conductive substrate such as conductive glass by medium and high temperature assisted chemical vapor deposition. Generally, the heat treatment cycle involved in the above process is several hours or even longer, resulting in low preparation efficiency and high energy consumption. In addition, the micromorphology and oxygen vacancies of the photoelectrode are generally considered to be important factors affecting its performance. How to achieve efficient heat treatment in the photoelectrode preparation process and simultaneously achieve the regulation of microstructure and oxygen vacancies is crucial. Summary of the invention

[0004] The purpose of the present invention is to provide a method for rapidly synthesizing a shape-preserving oxygen-vacancy-rich hematite thin film photoanode by thermal shock, so as to solve the problems of long cycle, high energy consumption and low efficiency in the prior art when preparing the hematite thin film photoanode.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] The method for rapidly synthesizing a shape-preserving oxygen-vacancy-rich hematite thin film photoanode by thermal shock comprises the following steps:

[0007] In a vacuum negative pressure environment, the hematite precursor film is heated by a thermal shock method and then cooled to obtain a hematite film photoelectrode converted from the hematite precursor film.

[0008] Furthermore, the negative pressure range of the vacuum negative pressure environment is -0.05 to -0.098 MPa.

[0009] Furthermore, the heating rate of the thermal shock method is 103-104°C / min.

[0010] Furthermore, the method is prepared by a shape-preserving oxygen-vacancy-rich hematite thin film photoanode preparation device, the device includes a sealed box, the sealed box is connected to a vacuum pump through an air guide pipe, the sealed box is evacuated by the vacuum pump, and a vacuum gauge is provided in the sealed box to detect the vacuum degree in the sealed box;

[0011] A support body is arranged in the sealing box, and a conductive resistor can be placed on the support body. The positive and negative electrodes of the conductive resistor are respectively electrically connected to the positive and negative electrodes of the DC power supply through wires.

[0012] Further, when preparing the conformal oxygen-rich vacancy hematite thin film photoanode by the conformal oxygen-rich vacancy hematite thin film photoanode preparation device, a replaceable conductive resistor is placed on the support body located in the sealed box;

[0013] Placing the conductive glass with the hematite precursor film on the conductive resistor so that the conductive resistor and the hematite precursor film are in contact with each other;

[0014] Use a vacuum pump to put the sealed box in a negative pressure state through the air pipe, and then close the valve and the vacuum pump;

[0015] After the sealed box reaches the target vacuum degree, turn on the DC power switch, adjust the current value, and heat the hematite precursor film through the conductive resistor. The power-on time is 1 to 15 seconds;

[0016] After the heating is completed, the DC current switch is turned off, and after the conductive glass is cooled, the sealing box is opened, and the hematite precursor film is converted into a hematite film photoelectrode.

[0017] Furthermore, the conductive resistor is a nickel sheet or a chromium-nickel alloy sheet.

[0018] Beneficial effects of the present invention:

[0019] 1. The present invention performs thermal shock heat treatment on the hematite precursor film under negative pressure, so as to obtain a shape-preserving hematite film photoanode rich in oxygen vacancies in one step, which has higher efficiency and lower energy consumption, and its photoelectrocatalytic water decomposition performance is equivalent to that of the hematite film photoanode obtained by traditional heat treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The present invention will be further described below in conjunction with the accompanying drawings.

[0021] Figure 1 It is a schematic diagram of the structure of a device for preparing a shape-preserving oxygen-vacancy-rich hematite thin film photoanode;

[0022] Figure 2 This is the microscopic morphology of the hematite thin film photoelectrode obtained by scanning electron microscopy;

[0023] (a) FeOOH precursor film, (b) hematite film photoanode obtained by traditional heat treatment, (c) hematite film photoelectrode rapidly synthesized by thermal shock.

[0024] Figure 3 It is the UV-visible absorption spectrum of the hematite film obtained by traditional heat treatment and the hematite film photoelectrode rapidly synthesized by thermal shock;

[0025] Figure 4 It is the X-ray photoelectron spectrum of the hematite film obtained by traditional heat treatment and the hematite film photoelectrode synthesized rapidly by thermal shock;

[0026] Figure 5 Linear sweep voltammogram of the hematite thin film photoelectrode in 1 mol potassium hydroxide aqueous solution under three-electrode test setup and intermittent illumination conditions for photoelectrocatalytic water splitting test. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] A method for rapidly synthesizing a shape-preserving oxygen-vacancy-rich hematite thin film photoanode by thermal shock is:

[0029] In a vacuum negative pressure environment, the hematite precursor film is rapidly heated by a thermal shock method, and then cooled to obtain a hematite film photoelectrode converted from the hematite precursor film;

[0030] The thermal shock method (Joule heat) has an extremely high heating rate (103-104℃ / min) and an extremely high cooling rate (up to 104℃ / min), which far exceeds the heating and cooling rates of most traditional furnaces. The extremely short sintering time can maintain the microstructure of the material to the maximum extent. Combined with rapid sintering in an oxygen-deficient environment, it can achieve fine control of the oxygen atom content in oxide materials.

[0031] In one embodiment of the present invention, the negative pressure range is -0.05 to -0.098 MPa, and a hematite precursor film is placed on a conductive resistor. By energizing the conductive resistor, rapid temperature rise is achieved in a short time, and after cooling, the required hematite film photoelectrode converted from the hematite precursor film is obtained.

[0032] like Figure 1 As shown, a device for preparing a conformal oxygen-vacancy-rich hematite thin film photoanode, the device comprises a sealed box 1, the sealed box 1 is connected to a vacuum pump 7 via an air guide pipe 8, the sealed box 1 is evacuated by the vacuum pump 7, and a vacuum gauge 9 is provided in the sealed box 1 for detecting the vacuum degree in the sealed box 1;

[0033] A support body 2 is provided in the sealed box 1 , and a conductive resistor 3 can be placed on the support body 2 . The positive and negative electrodes of the conductive resistor 3 are electrically connected to the positive and negative electrodes of a DC power source 6 through wires 5 , respectively.

[0034] When preparing a conformal oxygen-vacancy-rich hematite thin film photoanode by the above-mentioned apparatus, a replaceable conductive resistor 3 is placed on a support 2 located in a sealed box 1;

[0035] The conductive resistor can be a nickel sheet, a chromium-nickel alloy sheet, etc.

[0036] The conductive glass with the hematite precursor film 4 placed thereon is placed on the conductive resistor 3, so that the conductive resistor 3 and the hematite precursor film 4 are in contact with each other;

[0037] The hematite precursor film 4 is a FeOOH nanorod array grown on a conductive glass substrate. The microscopic morphology photograph obtained by scanning electron microscopy is as follows: Figure 2 As shown in a.

[0038] The conductive resistor 3 is electrically connected to the direct current 6 via the conductor 5;

[0039] Before the DC current 6 is energized, the sealed box 1 is placed in a negative pressure state through the air guide pipe 8 by means of the vacuum pump 7, the negative pressure range is -0.05 to -0.098Mpa, and then the valve and the vacuum pump are closed;

[0040] After the sealed box 1 reaches the target vacuum degree, the DC power supply 6 is turned on, the current value is adjusted, and the hematite precursor film 4 is heated through the conductive resistor 3, and the power-on time is 1 to 15 seconds;

[0041] After the heating is completed, the switch of the direct current 6 is turned off, and after waiting for a few minutes for the conductive glass to cool down, the sealing box 1 is opened, and the hematite precursor film 4 is converted into a hematite film photoelectrode.

[0042] exist Figure 2Through observation, we can find Figure 2 b relative to Figure 2 a, the nanorod array undergoes sintering and agglomeration due to the long-term heat treatment, that is, two or more nanorods are fused into one; while the hematite thin film photoelectrode synthesized rapidly by thermal shock Figure 2 c, the nanorod array is agglomerated, i.e., shape-preserving; different microscopic morphologies will lead to different optical properties;

[0043] UV-visible absorption spectroscopy Figure 3 Changes in the optical properties of the hematite film photoelectrodes obtained by conventional heat treatment and those synthesized rapidly by thermal shock can be observed;

[0044] X-ray photoelectron spectroscopy Figure 4 It can be observed that the hematite thin film photoelectrode rapidly synthesized by thermal shock described in the patent has more abundant oxygen vacancies.

[0045] The hematite film photoelectrode prepared by thermal shock rapid synthesis described in the patent was used to catalyze water decomposition in a photoelectrochemical cell. The hematite film photoelectrode prepared above was placed in a 1 mol / L potassium hydroxide aqueous solution and subjected to a photoelectrochemical water decomposition test under a three-electrode test setup and intermittent illumination conditions. The linear sweep voltammetric curve is shown in FIG. Figure 5 It can be seen that the hematite film photoelectrode rapidly synthesized by thermal shock under light irradiation has a strong light response, and its performance is comparable to that of the hematite film photoanode obtained by traditional heat treatment.

[0046] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for rapid synthesis of a shape-preserving oxygen-vacancy-rich hematite thin film photoanode by thermal shock, characterized in that: The steps include: In a vacuum negative pressure environment, the hematite precursor film is heated by a thermal shock method and then cooled to obtain a hematite film photoanode converted from the hematite precursor film.

2. The method for rapid synthesis of a shape-preserving oxygen-vacancy-rich hematite thin film photoanode by thermal shock according to claim 1, characterized in that: The negative pressure range of the vacuum negative pressure environment is -0.05~-0.098Mpa.

3. The method for rapid synthesis of a shape-preserving oxygen-vacancy-rich hematite thin film photoanode by thermal shock according to claim 1, characterized in that: The heating rate of the thermal shock method is 103-104°C / min.

4. The method for rapid synthesis of a shape-preserving oxygen-vacancy-rich hematite thin film photoanode by thermal shock according to claim 1, characterized in that: The method is prepared by a shape-preserving oxygen-vacancy-rich hematite thin film photoanode preparation device, the device comprising a sealed box (1), the sealed box (1) being connected to a vacuum pump (7) via an air guide pipe (8), the sealed box (1) being evacuated via the vacuum pump (7), and a vacuum gauge (9) being arranged in the sealed box (1) for detecting the vacuum degree in the sealed box (1); A support body (2) is provided in the sealed box (1), and a conductive resistor (3) can be placed on the support body (2). The positive and negative electrodes of the conductive resistor (3) are electrically connected to the positive and negative electrodes of a direct current power source (6) via wires (5), respectively.

5. The method for rapid synthesis of a shape-preserving oxygen-vacancy-rich hematite thin film photoanode by thermal shock according to claim 4, characterized in that: When preparing a conformal oxygen-vacancy-rich hematite thin film photoanode by using a conformal oxygen-vacancy-rich hematite thin film photoanode preparation device, a replaceable conductive resistor (3) is placed on a support (2) located in a sealed box (1); Placing the conductive glass with the hematite precursor film (4) placed on the conductive resistor (3) so that the conductive resistor (3) and the hematite precursor film (4) are in contact with each other; Using a vacuum pump (7) through an air guide pipe (8), the sealed box (1) is placed in a negative pressure state, and then the valve and the vacuum pump (7) are closed; After the sealed box (1) reaches the target vacuum degree, the DC power supply (6) is turned on, the current value is adjusted, and the hematite precursor film (4) is heated via the conductive resistor (3), and the power-on time is 1 to 15 seconds; After the heating is completed, the switch of the direct current (6) is turned off, and after the conductive glass is cooled, the sealing box (1) is opened, and the hematite precursor film (4) is converted into a hematite film photoelectrode.

6. The method for rapid synthesis of a shape-preserving oxygen-vacancy-rich hematite thin film photoanode by thermal shock according to claim 5, characterized in that: The conductive resistor (3) is a nickel sheet or a chromium-nickel alloy sheet.

7. Use of the hematite thin film photoanode prepared by the method according to any one of claims 1 to 6 in photoelectrocatalysis.